A method for improving the rectangularity of the transverse section of wide and thick steel plates

By using a double stand production of rough rolling mill and finishing rolling mill in a wide-thick plate rolling mill, the slab temperature difference and rolling parameters are controlled, and the problem of the difference in the rectangularity of the transverse section of the wide-thick steel plate is solved, which significantly reduces the cutting amount and improves the material yield.

CN115463976BActive Publication Date: 2024-11-19BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202210963990.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-11
Publication Date
2024-11-19
Estimated Expiration
2042-08-11

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the rectangularity of the transverse section of wide and thick steel plates, resulting in a large difference in width of upper and lower surfaces, increasing the amount of cutting edges and loss yield.

Method used

The wide-thick plate rolling mill with double stands of rough rolling mill and finishing mill is produced. The temperature difference between the upper and lower surfaces when the slab is discharged is within 30℃. The working roller on the rough rolling mill is larger than the diameter of the lower working roller, and the bite speed and linear speed are set. and set appropriate torque and descaling methods during the widening phase.

Benefits of technology

The width difference between the upper and lower surfaces of the steel plate is effectively reduced, the cutting amount is reduced, and the material yield is improved, so that the lateral cross-sectional rectangularity of the wide and thick steel plate is reduced from more than 40mm to less than 5mm.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a method for improving the rectangularity of the transverse section of a wide and thick steel plate, comprising: (1) adopting a wide and thick plate rolling mill with a roughing mill and a finishing mill double frame, and completing the widening rolling of the steel plate on the roughing mill; (2) when the slab is discharged from the furnace, the temperature difference between the upper and lower surfaces does not exceed 30°C; (3) the diameter of the upper working roll of the roughing mill is 25-40mm larger than that of the lower working roll; (4) when the steel plate is rolled in the widening stage, the bite speed is set to 0.5m / s and the bite length is set to 0.5m; the linear speed of the lower working roll in the steel plate bite stage is 3%-8% faster than that of the upper working roll; (5) when the steel plate is rolled in the widening stage, the scale is removed 1-2 times, and the scale removal method is positive removal; (6) when the steel plate is rolled in the widening stage, the torque is set to 80% of the designed rated torque of the rolling mill. The purpose of the present invention is to provide a method that can effectively improve the rectangularity of the transverse section of a wide and thick steel plate, reduce the amount of steel plate trimming, and improve the yield rate of the steel plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of steel rolling, and in particular to a method for improving the rectangularity of the transverse section of a wide and thick steel plate. Background Art

[0002] At present, wide and thick steel plates are generally produced by wide and thick plate rolling mills. When casting thick slabs, the casting machine generally adopts light pressure to improve the quality of the cast slabs. The slabs cast in this way are generally wide on the upper surface and narrow on the lower surface. The difference in width between the upper and lower surfaces is generally 6 to 13 mm. When the steel plate is rolled, after widening and rolling, the width difference between the upper and lower surfaces of the steel plate is further increased due to the influence of the width ratio. During the heating process of the slab in the heating furnace, if the temperature of the lower surface is much lower than that of the upper surface, the deformation of the upper surface is greater than that of the lower surface during widening and rolling. The combined influence of the above-mentioned factors leads to the upper surface width of the rolled steel plate being wider than the lower surface. The thicker the steel plate, the wider the width, and the larger the width ratio, the more obvious this phenomenon is, presenting an "inverted trapezoidal" phenomenon. In severe cases, the width of the lower surface is more than 40 mm narrower than the width of the upper surface. Wide and thick plates are usually delivered in four-cut form, which requires shearing on both sides of the steel plate. Since the width of the lower surface is much narrower than that of the upper surface, in order to ensure the shearing quality of the lower surface of the steel plate, the width margin of the rolled large plate must be increased, which will result in a loss of part of the yield rate. Therefore, how to reduce the width difference between the upper and lower surfaces of the rolled large plate, reduce the width margin of the rolled large plate, and improve the rectangularity of the transverse section of the wide and thick steel plate is an urgent problem to be solved in the production of wide and thick steel plates.

[0003] The patent "High-strength steel plate shape control method" with publication number CN 101367091 A provides a high-strength steel plate shape control method, which can effectively control the flatness of the steel plate, but does not involve the control of the rectangularity of the transverse section of the steel plate.

[0004] The patent "Steel Plate Shape Control Method with Width Greater Than Equal to 3500mm" with publication number CN 108655184 A provides a wide steel plate shape control method, which can effectively control the straightness of the wide steel plate, but does not involve the control of the rectangularity of the transverse section of the steel plate.

[0005] The patent "A method for controlling the shape of the tail of a TMCP steel plate" with publication number CN 113617854 A provides a method for controlling the shape of a steel plate produced by the TMCP process. The method can effectively control the straightness of the tail of the steel plate produced by the TMCP process, but does not involve the control of the rectangularity of the transverse section of the steel plate. Summary of the invention

[0006] In order to solve the above technical problems, the purpose of the present invention is to provide a method that can effectively improve the rectangularity of the transverse section of wide and thick steel plates, reduce the amount of steel plate trimming, and improve the yield rate of steel plates.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for improving the rectangularity of the transverse section of a wide and thick steel plate, comprising:

[0009] (1) A wide and thick plate rolling mill with a roughing mill and a finishing mill is used for production, and the widening rolling of the steel plate is completed on the roughing mill;

[0010] (2) When the slab comes out of the furnace, the temperature difference between the upper and lower surfaces does not exceed 30°C;

[0011] (3) The upper working roll of the roughing mill is 25 to 40 mm larger in diameter than the lower working roll;

[0012] (4) When the steel plate is rolled in the widening stage, the bite speed is set to 0.5 m / s and the bite length is set to 0.5 m; the linear speed of the lower working roll in the steel plate bite stage is 3% to 8% faster than the linear speed of the upper working roll;

[0013] (5) When the steel plate is rolled in the widening stage, descaling is performed 1 to 2 times, and the descaling method is positive descaling;

[0014] (6) When the steel plate is rolled in the widening stage, the set torque is 80% of the designed rated torque of the rolling mill.

[0015] Furthermore, the thick steel plate is a steel plate with a thickness greater than or equal to 30 mm and a width greater than or equal to 2700 mm.

[0016] Furthermore, it specifically includes: adopting a wide and thick plate rolling mill with a double frame of a roughing mill and a finishing mill for production, completing the widening rolling of the steel plate on the roughing mill; the thickness of the produced steel plate is 30mm and the width is 2700mm; when the slab is out of the furnace, the temperature difference between the upper and lower surfaces is 30°C; the upper working roll of the roughing mill is 25mm larger in diameter than the lower working roll; when the steel plate is rolled in the widening stage, the bite speed is set to 0.5m / s and the bite length is 0.5m; the linear speed of the lower working roll in the steel plate bite stage is 8% faster than the linear speed of the upper working roll; when the steel plate is rolled in the widening stage, descaling is performed once, and the descaling method is positive descaling; when the steel plate is rolled in the widening stage, the torque is set to 80% of the designed rated torque of the rolling mill.

[0017] Furthermore, it specifically includes: adopting a wide and thick plate rolling mill with a double frame of a roughing mill and a finishing mill for production, completing the widening rolling of the steel plate on the roughing mill; the thickness of the produced steel plate is 48mm and the width is 2850mm; when the slab is out of the furnace, the temperature difference between the upper and lower surfaces is 26°C; the upper working roll of the roughing mill is 40mm larger in diameter than the lower working roll; when the steel plate is rolled in the widening stage, the bite speed is set to 0.5m / s and the bite length is 0.5m; the linear speed of the lower working roll in the steel plate bite stage is 3% faster than the linear speed of the upper working roll; when the steel plate is rolled in the widening stage, descaling is performed twice, and the descaling method is positive descaling; when the steel plate is rolled in the widening stage, the torque is set to 80% of the designed rated torque of the rolling mill.

[0018] Furthermore, it specifically includes: adopting a wide and thick plate rolling mill with a double frame of a roughing mill and a finishing mill for production, completing the widening rolling of the steel plate on the roughing mill; the thickness of the produced steel plate is 50mm and the width is 3120mm; when the slab is out of the furnace, the temperature difference between the upper and lower surfaces is 21°C; the upper working roll of the roughing mill is 32mm larger in diameter than the lower working roll; when the steel plate is rolled in the widening stage, the bite speed is set to 0.5m / s and the bite length is 0.5m; the linear speed of the lower working roll in the steel plate bite stage is 5% faster than the linear speed of the upper working roll; when the steel plate is rolled in the widening stage, descaling is performed once, and the descaling method is positive descaling; when the steel plate is rolled in the widening stage, the torque is set to 80% of the designed rated torque of the rolling mill.

[0019] Compared with the prior art, the beneficial technical effects of the present invention are:

[0020] By adjusting the heat supply of the upper and lower burners of the heating furnace when heating the slab, the temperature difference between the upper and lower surfaces can be controlled within a certain range, which is beneficial to control the width difference between the upper and lower surfaces of the steel plate during widening rolling. The upper working roll of the roughing mill is larger than the lower working roll so that during widening rolling, under the same rolling force, the lower surface has a larger reduction and larger extension deformation, which is beneficial to eliminate the width difference between the upper and lower surfaces. During the widening stage rolling, the speed of the lower working roll is faster than that of the upper working roll during the biting stage, and descaling during rolling is all to make the extension of the lower surface of the slab larger than that of the upper surface during widening rolling. Setting a smaller torque in the widening stage is to avoid the actual torque being large during rolling due to uneven slab temperature, or inaccurate slab length and thickness, which leads to deceleration of the upper and lower motors and inability to effectively control the extension of the upper and lower surfaces of the steel plate during rolling.

[0021] The present invention is simple to implement. It can effectively control the width difference between the upper and lower surfaces of the wide and thick steel plate and improve the rectangularity of the transverse section of the wide and thick steel plate by adjusting the production process parameter settings, improving the operation method and reasonably matching the rollers. After using this method, the width difference between the upper and lower surfaces of the wide and thick steel plate is reduced from more than 40 mm to less than 5 mm, reducing the amount of trimming and improving the yield rate, and the effect is very obvious. DETAILED DESCRIPTION

[0022] The present invention is further described below with reference to the embodiments.

[0023] Example 1

[0024] A method for improving the rectangularity of the transverse section of a wide and thick steel plate, comprising:

[0025] The wide and thick plate mill with a roughing mill and a finishing mill is used for production, and the widening rolling of the steel plate is completed on the roughing mill. The thickness of the steel plate produced is 30mm and the width is 2700mm. When the slab comes out of the furnace, the temperature difference between the upper and lower surfaces is 30℃. The upper working roll of the roughing mill is 25mm larger in diameter than the lower working roll. When the steel plate is rolled in the widening stage, the bite speed is set to 0.5m / s and the bite length is 0.5m; the linear speed of the lower working roll in the bite stage of the steel plate is 8% faster than the linear speed of the upper working roll. When the steel plate is rolled in the widening stage, the scale is removed once, and the descaling method is positive removal. When the steel plate is rolled in the widening stage, the torque is set to 80% of the rated torque of the mill design. The lower surface width of the steel plate finally rolled is 5mm narrower than the upper surface width, and the effect is good.

[0026] Example 2

[0027] A method for improving the rectangularity of the transverse section of a wide and thick steel plate, comprising:

[0028] The wide and thick plate mill with a roughing mill and a finishing mill is used for production, and the widening rolling of the steel plate is completed on the roughing mill. The thickness of the steel plate produced is 48mm and the width is 2850mm. When the slab is out of the furnace, the temperature difference between the upper and lower surfaces is 26℃. The upper working roll of the roughing mill is 40mm larger in diameter than the lower working roll. When the steel plate is rolled in the widening stage, the bite speed is set to 0.5m / s and the bite length is 0.5m; the linear speed of the lower working roll in the bite stage of the steel plate is 3% faster than the linear speed of the upper working roll. When the steel plate is rolled in the widening stage, the scale is removed twice, and the descaling method is positive removal. When the steel plate is rolled in the widening stage, the torque is set to 80% of the rated torque of the mill design. The lower surface width of the steel plate after final rolling is 3mm narrower than the upper surface width, with good results.

[0029] Example 3

[0030] A method for improving the rectangularity of the transverse section of a wide and thick steel plate, comprising:

[0031] The wide and thick plate mill with a roughing mill and a finishing mill is used for production, and the widening rolling of the steel plate is completed on the roughing mill. The thickness of the steel plate produced is 50mm and the width is 3120mm. When the slab is out of the furnace, the temperature difference between the upper and lower surfaces is 21℃. The diameter of the upper working roll of the roughing mill is 32mm larger than that of the lower working roll. When the steel plate is rolled in the widening stage, the bite speed is set to 0.5m / s and the bite length is 0.5m; the linear speed of the lower working roll in the bite stage of the steel plate is 5% faster than that of the upper working roll. When the steel plate is rolled in the widening stage, the scale is removed once, and the descaling method is positive removal. When the steel plate is rolled in the widening stage, the torque is set to 80% of the rated torque of the mill design. The lower surface width of the steel plate finally rolled is 2mm narrower than the upper surface width, and the effect is good.

[0032] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for improving the rectangularity of the transverse section of a wide and thick steel plate, characterized in that: include: (1) The wide and thick plate rolling mill with two stands of roughing mill and finishing mill is adopted, and the widening rolling of the steel plate is completed on the roughing mill; (2) When the slab comes out of the furnace, the temperature difference between the upper and lower surfaces does not exceed 30°C; (3) The diameter of the upper working roll of the roughing mill is 25 to 40 mm larger than that of the lower working roll; (4) When the steel plate is rolled in the widening stage, the bite speed is set to 0.5 m / s and the bite length is set to 0.5 m; the linear speed of the lower working roll in the steel plate bite stage is 3% to 8% faster than the linear speed of the upper working roll; (5) When rolling the steel plate in the widening stage, descaling is performed 1 to 2 times, and the descaling method is positive descaling; (6) When the steel plate is rolled in the widening stage, the set torque is 80% of the design rated torque of the rolling mill; The thick steel plate is a steel plate with a thickness greater than or equal to 30 mm and a width greater than or equal to 2700 mm.

2. The method for improving the rectangularity of the transverse section of a wide and thick steel plate according to claim 1, characterized in that: Specifically include: The steel plate produced is 30mm thick and 2700mm wide. When the slab comes out of the furnace, the temperature difference between the upper and lower surfaces is 30℃. The upper working roll of the roughing mill is 25mm larger in diameter than the lower working roll. The linear speed of the lower working roll during the steel plate biting stage is 8% faster than that of the upper working roll. During the widening stage of rolling, the steel plate is descaled once.

3. The method for improving the rectangularity of the transverse section of a wide and thick steel plate according to claim 1, characterized in that: Specifically include: The steel plate produced is 48mm thick and 2850mm wide. When the slab comes out of the furnace, the temperature difference between the upper and lower surfaces is 26°C. The upper working roll of the roughing mill is 40mm larger in diameter than the lower working roll. The linear speed of the lower working roll during the steel plate biting stage is 3% faster than that of the upper working roll. During the widening stage of rolling, the steel plate is descaled twice.

4. The method for improving the rectangularity of the transverse section of a wide and thick steel plate according to claim 1, characterized in that: Specifically include: The steel plate produced is 50mm thick and 3120mm wide. When the slab comes out of the furnace, the temperature difference between the upper and lower surfaces is 21°C. The upper working roll of the roughing mill is 32mm larger in diameter than the lower working roll. The linear speed of the lower working roll during the steel plate biting stage is 5% faster than that of the upper working roll. During the widening stage of rolling, the steel plate is descaled once.

Citation Information

Patent Citations

  • Control method for plate shape of high-strength steel plate

    CN101367091A

  • Controlling method of plate shape of steel plate having width of being more than or equal to 3500mm

    CN108655184A

  • TMCP steel plate tail plate shape control method

    CN113617854A

  • Production method of longitudinal thickness-variable steel plate

    CN102397875A

  • Method for controlling even deformation of edge portion in medium-thick board rolling

    CN102527735A