A phosphorus-containing copolymer flame-retardant nylon and its preparation method and application
By controlling the molar ratio and reaction conditions, a phosphorus-containing copolymerized flame-retardant nylon with excellent characteristics was developed, which solved the problems of mechanical property degradation and flame retardant migration caused by the introduction of high flame-retardant monomers in the existing technology, and achieved high-efficiency flame retardant nylon. The coexistence of combustion and excellent mechanical properties.
Patent Information
- Application Number
- CN202211086418.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-06
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-09-06
AI Technical Summary
In the existing technology, phosphorus-containing copolymerized flame-retardant nylon requires a high amount of flame-retardant monomer to be introduced, which leads to a decrease in the mechanical properties and spinnability of the material, and there are problems with flame retardant migration and compatibility, which affects its application.
Using a specific structural unit composition and preparation method, and by controlling the molar ratio and reaction conditions, a phosphorus-containing copolymerized flame-retardant nylon was developed, with an intrinsic viscosity of 0.47-1.50dL/g and a limiting oxygen index of 24.3-36.4%. UL-94 The vertical combustion grade is V-2~V-0, the tensile strength is 50~120MPa, the flexural strength is 90MPa~170MPa, and the flexural modulus is 2600~4500MPa, which avoids damage to material properties caused by excessive use of flame retardants.
It achieves the maintenance of excellent flame retardant properties and mechanical properties at a lower dosage of flame retardant, solves the problem of flame retardant migration and compatibility, improves the thermal stability and spinnability of the material, and reduces production costs.
Smart Images

Figure BDA0003835327240000021 
Figure BDA0003835327240000022 
Figure BDA0003835327240000023
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of copolymer nylon and its preparation and application. Specifically, it relates to a phosphorus-containing copolymer flame-retardant nylon (including petroleum-based copolymer nylon and bio-based copolymer nylon) and its preparation method and application. This type of phosphorus-containing copolymer flame-retardant nylon can achieve excellent flame retardant properties at a relatively low monomer introduction amount while maintaining excellent mechanical properties. Background Art
[0002] Nylon, also known as polyamide (abbreviated as PA), is a type of thermoplastic resin containing repeating amide groups on the main chain of the molecule. As an important engineering plastic, it is widely used in various fields due to its high mechanical strength, excellent self-lubrication, heat resistance and good chemical corrosion resistance. Unfortunately, most nylons have poor flame retardancy, which will undoubtedly limit their application in transportation, electrical and electronic fields. Typical aliphatic nylons such as PA 66 have a limiting oxygen index (LOI) of 24.0% and a vertical burning UL 94 test of V-2 (J.Appl.Polym.Sci.,2020,137,47488.). Another aliphatic nylon PA6 has a limiting oxygen index of 22.0% and a vertical burning level of V-2 (Compos.Part A.,2021,146.). Typical bio-based nylon PA1010 has a limiting oxygen index of 25.8% and a vertical burning test level of V-2 (Polymers, 2020, 12, 1482.). In addition, when nylon burns, a large amount of molten droplets will fall, which seriously threatens people's lives and property safety. Therefore, it is of great significance to study flame-retardant nylon.
[0003] At present, in order to solve the problem of poor flame retardancy of nylon, the commonly used flame retardant methods are additive flame retardant and copolymer flame retardant. Among them, the additive flame retardant method has simple process and easy operation, and is currently the main method for producing flame retardant nylon. However, due to the generally poor compatibility between additive flame retardants and nylon substrates, there are problems such as flame retardant migration and precipitation during use, resulting in poor flame retardant durability; and in order to achieve the expected flame retardant effect, the amount of flame retardant added is usually large, which will damage the mechanical properties and spinning properties of the material (Polym. Adv. Technol., 2018, 29 (3), 1068-1077.), affecting the application of the material. The copolymer flame retardant method is to introduce flame retardant units into the polymer molecular chain through chemical copolymerization (melt polymerization, interfacial polymerization, etc.). This method does not have the problems of flame retardant migration and poor compatibility with the substrate, and thus exhibits good flame retardant durability and spinnability. However, some of the reported phosphorus-containing flame-retardant copolymer nylons usually require a high amount of flame-retardant monomers, which not only destroys the spinnability of the material, but also greatly affects the mechanical properties. For example, the tensile strength of a phosphorus-containing flame-retardant copolymer PA 6-5DPO will decrease from 76.3MPa of pure PA 6 to 58.5MPa, a decrease of 23.3% (Polym.Degrad.Stabili., 2019, 163, 151-160.); for another example, the tensile strength of a phosphorus-containing flame-retardant copolymer FRPA 6-5fibre will decrease from 4.3cN dtex of pure PA 6 to 58.5MPa, a decrease of 23.3% (Polym.Degrad.Stabili., 2019, 163, 151-160.). -1 Reduced to 3.0 cN dtex -1 , a reduction of 30.2% (RSC Adv., 2018, 8, 9261–9271.). Summary of the invention
[0004] The purpose of the present invention is to provide a phosphorus-containing copolymer flame-retardant nylon in view of the problems existing in the prior art. The flame-retardant nylon is not only highly flame-retardant and has high thermal stability, but also has excellent mechanical properties and spinnability.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned phosphorus-containing copolymer flame-retardant nylon.
[0006] Another object of the present invention is to provide an application of the above phosphorus-containing copolymer flame-retardant nylon.
[0007] The phosphorus-containing flame-retardant copolymer nylon provided by the present invention is characterized in that the flame-retardant nylon is composed of the following structural units represented by Ⅰ, Ⅳ or Ⅱ, Ⅲ, Ⅳ:
[0008]
[0009] In the formula, R 1 Represents C 3 ~C 12 of alkylene;
[0010]
[0011] Among them, R 2 Represents C 2 ~C 12 An alkylene or arylene group;
[0012]
[0013] Among them, R 3 Represents C 4 ~C 14 An alkylene or arylene group, R 2 and R 3 are not arylene groups at the same time;
[0014]
[0015]
[0016]
[0017] Where R 4 , R 5 is a carbonyl group, an imino group or m is an integer from 2 to 12, R 4 , R 5 are the same or different; Y is an oxygen atom or an imino group, Z 1 , Z 2 is any one of a hydrogen atom, a hydroxyl group, a methyl group or a methoxy group, Z 1 , Z 2 the same or different;
[0018] Z 3 , Z 4 is methylene, phenyl, biphenyl, sulfone, azo, piperazine, Any of: Z 5 It is any of methyl, methoxy, phenyl or phenoxy.
[0019] Among them, the number of structural units of IV is 1 to 99% of the number of structural units of II, the number of structural units of III: the number of structural units of [II+IV]=1, or the number of structural units of IV is 1 to 99% of the number of structural units of III, the number of structural units of II: the number of structural units of [III+IV]=1, or the number of structural units of IV is 1 to 99% of the number of structural units of I; each structural unit and the chain segment formed by them are arbitrarily connected and combined according to the carboxyl and amino functional groups, and the intrinsic viscosity [η] of the copolymer nylon is 0.47 to 1.50 dL / g; the limiting oxygen index is 24.3 to 36.4%; the UL-94 vertical burning grade is V-2 to V-0; the tensile strength is 50 to 120 MPa; the tensile modulus is 1700 to 2994 MPa, the flexural strength is 90 MPa to 170 MPa; and the flexural modulus is 2600 to 4500 MPa.
[0020] The number of structural units of IV in the flame retardant nylon is 1-20% of the number of structural units of II, the number of structural units of III: the number of structural units of [II+IV]=1, or the number of structural units of IV is 1-20% of the number of structural units of III, the number of structural units of II: the number of structural units of [III+IV]=1, or the number of structural units of IV is 1-20% of the number of structural units of I, its intrinsic viscosity [η] is 0.60-1.50 dL / g, the limiting oxygen index is 26.0-36.4%; UL 94 vertical burning grade is V-1 to V-0; tensile strength is 57-120 MPa; tensile modulus is 2000-2994 MPa; flexural strength is 110-170 MPa, flexural modulus is 2800-4500 MPa, and the structural unit represented by IV is preferably as follows:
[0021]
[0022]
[0023]
[0024] Where R 4 , R 5 is a carbonyl group, an imino group or m is an integer from 2 to 12, R 4 , R 5 are the same or different; Y is an oxygen atom or an imino group, Z 1 , Z 2 is any one of H atom, hydroxyl, methyl or methoxy, Z 1 , Z 2 the same or different;
[0025] Z 3 , Z 4 is methylene, phenyl, biphenyl, sulfone, azo, piperazine, Any of: Z 5 It is any of methyl, methoxy, phenyl or phenoxy.
[0026] The copolymer nylon is characterized in that the number of structural units of IV in the copolymer nylon is preferably 1-3% of the number of structural units of II, the number of structural units of III: the number of structural units of [II+IV]=1, or the number of structural units of IV is preferably 1-3% of the number of structural units of III, the number of structural units of II: the number of structural units of [III+IV]=1, or the number of structural units of IV is preferably 1-3% of the number of structural units of I, its intrinsic viscosity [η] is 0.64-1.50 dL / g, the limiting oxygen index is 28.3-36.4%; the vertical burning grade is V-1 to V-0; the tensile strength is 67-120 MPa, the tensile modulus is 2200-2885 MPa; the flexural strength is 130-170 MPa, and the flexural modulus is 3000-4500 MPa, wherein the structural unit represented by IV is preferably as follows:
[0027]
[0028]
[0029] Where R 4 , R 5 is a carbonyl group, an imino group or m is an integer from 2 to 12, R 4 , R 5 are the same or different; Y is an oxygen atom or an imino group, Z 1 , Z 2 is any one of H atom, hydroxyl, methyl or methoxy, Z 1 , Z 2 the same or different;
[0030] Z 3 , Z 4 is methylene, phenyl, biphenyl, sulfone, azo, piperazine, Any of: Z 5 It is any of methyl, methoxy, phenyl or phenoxy.
[0031] The preparation method of the above-mentioned phosphorus-containing flame-retardant nylon provided by the present invention is characterized in that the process steps and conditions of the preparation method are as follows:
[0032] (1) dissolving a nylon polymerization monomer diamine, an acid binding agent and a phase transfer catalyst in a molar ratio of 1:1-2.4:0.001-0.1 in water to prepare a 0.1-40 wt % aqueous phase solution;
[0033] (2) dissolving the dibasic acid chloride of nylon polymerization monomer in an organic solvent immiscible with water to prepare an organic phase solution with a concentration of 0.1 to 40 wt %;
[0034] (3) dissolving 1 to 99 mol% of a flame retardant monomer having an amino terminal group in the aqueous phase solution, or dissolving 1 to 99 mol% of a flame retardant monomer having an acyl chloride terminal group in the organic phase solution, based on the nylon polymerized monomer diamine;
[0035] (4) First, the organic phase solution is quickly poured into the aqueous phase solution, and the mixture is reacted at room temperature for 10 to 120 minutes under stirring conditions of 500 to 2000 rpm, and after suction filtration, washing, and drying, type II, III, and IV copolymer flame-retardant nylon products are obtained, wherein the molar number of the nylon polymerization monomer + the diamine of the flame-retardant monomer: the molar number of the nylon polymerization monomer + the dibasic acid chloride of the flame-retardant monomer in the reaction system is 0.8 to 1.2:1, or
[0036] (1) dissolving a nylon polymerized monomer dibasic acid and a nylon polymerized monomer diamine in ethanol, precipitating the salt after salt formation, filtering and drying to prepare a 10-90 wt % aqueous solution for standby use;
[0037] (2) dissolving a flame retardant monomer with a carboxyl terminal group and a nylon polymer monomer diamine in a molar ratio of 1:1-1:1.1 or a flame retardant monomer with an amino terminal group and a nylon polymer monomer diamine in a molar ratio of 1:1 in ethanol, reacting to form a salt, filtering and drying, and preparing a 10-90 wt % aqueous solution for standby use;
[0038] (3) Add the above two aqueous solutions to a reaction kettle, and then add nylon polymerized monomer dibasic acid or nylon polymerized monomer diamine, so that the molar number of the flame retardant monomer with a carboxyl terminal group is 1 to 99% of the molar number of the nylon polymerized monomer dibasic acid, or the molar number of the flame retardant monomer with an amino terminal group is 1 to 99% of the molar number of the nylon polymerized monomer diamine, and the molar number of the nylon polymerized monomer + the diamine of the flame retardant monomer: the molar number of the nylon polymerized monomer + the dibasic acid of the flame retardant monomer in the reaction system is 0.8 to 1.2:1, and then at a temperature of 210 to 240° C. and a pressure of 1.6 to 3.0 MPa, prepolymerize for 0.5 to 3 hours, gradually discharge the water vapor in the system, and start to evacuate to 1000 to 10000 Pa when the pressure drops to normal pressure, and then gradually increase the system temperature, and carry out a condensation reaction at 250 to 280° C. for 0.5 to 3 hours to obtain a copolymer flame retardant nylon product having structural units II, III, and IV, or
[0039] A flame retardant monomer, lactam, nylon polymerization monomer dibasic acid or diamine with a carboxyl terminal or an amino terminal is added into a polymerization container at a molar ratio of 0.01-0.99:1:0.001-0.1, and the temperature is raised to 220-260°C under nitrogen protection, and the reaction is carried out for 2-4 hours. Then, the water vapor in the system is gradually removed, and the reaction is continued for 2-4 hours. Finally, the system is evacuated to 1000-2000Pa and the reaction is carried out for 0.5-2 hours to obtain a copolymer flame retardant nylon product with structural units I and IV.
[0040] In the above method, the flame retardant monomer with carboxyl or amino terminal groups is preferably 1-20% by mole percentage of nylon polymerized monomer dibasic acid, nylon polymerized monomer diamine, nylon polymerized monomer dibasic acid chloride or lactam, and more preferably 1-3%.
[0041] When the end group of the flame retardant monomer in the above method is carboxyl or amino, the amount of the added amount is 1-99%, and any one of the following general structural formulas is selected:
[0042]
[0043]
[0044]
[0045] Where, X 1 , X 2 Carboxyl (-COOH), ester Chloroyl (-COOCl), amino (-NH2) or m is an integer from 2 to 12, n is an integer from 0 to 5, and X 1 , X 2 are the same or different; Y is an oxygen atom or an imino group, Z 1 , Z 2 is any one of H atom, hydroxyl, methyl or methoxy, Z 1 , Z 2 Same or different; Z 3 , Z 4 Methyl, phenyl, biphenyl, sulfone, azo, piperazine, Any of: Z 5 It is any of methyl, methoxy, phenyl or phenoxy.
[0046] When the end group of the flame retardant monomer in the above method is carboxyl or amino, the amount of the added amount is 1-20%, preferably any one of the following general structural formulas:
[0047]
[0048]
[0049]
[0050] Where, X 1 , X 2 Carboxyl (-COOH), ester Acyl chloride (-COOCl), amino (-NH 2 )or m is an integer from 2 to 12, n is an integer from 0 to 5, and X 1 , X 2 are the same or different; Y is an oxygen atom or an imino group, Z 1 , Z 2 is any one of H atom, hydroxyl, methyl or methoxy, Z 1 , Z 2 Same or different; Z 3 , Z 4 Methyl, phenyl, biphenyl, sulfone, azo, piperazine, Any of: Z 5 It is any of methyl, methoxy, phenyl or phenoxy.
[0051] When the amount of the carboxyl-terminated or amino-terminated flame-retardant monomer added in the above method is 1-3%, any one of the following general structural formulas is preferred:
[0052]
[0053]
[0054] Where, X 1 , X 2 For carboxyl, chloro, amino, m is an integer from 2 to 12, n is an integer from 0 to 5, and X 1 , X 2 are the same or different; Y is an oxygen atom or an imino group, Z 1 , Z 2 is any one of H atom, hydroxyl, methyl or methoxy, Z 1 , Z 2 Same or different; Z 3 , Z 4 Methyl, phenyl, biphenyl, sulfone, azo, piperazine, Any of: Z 5 It is any of methyl, methoxy, phenyl or phenoxy.
[0055] The general structural formula of the lactam described in the above method is: In the formula, R 1 Represents C 3 ~C 12The general structural formula of the nylon polymerization monomer diacyl chloride is: The general structural formula of the nylon polymerized monomer dibasic acid is: In the formula, R 2 Represents C 2 ~C 12 The general structural formula of the nylon polymer monomer diamine is: 2 NR 3 -NH 2 , where R 3 Represents C 4 ~C 14 An alkylene group or an arylene group.
[0056] In the above method, the acid binding agent is at least one of potassium carbonate, ammonium carbonate, sodium carbonate, sodium bicarbonate, sodium hydroxide, triethylamine, triethanolamine and pyridine; and the phase transfer catalyst is at least one of tetramethylammonium bromide, tetrapropylammonium bromide, tetrabutylammonium bromide, tetrabutylammonium chloride, benzyltriethylammonium bromide and benzyltriethylammonium chloride.
[0057] The application of the above-mentioned phosphorus-containing copolymer flame-retardant nylon provided by the present invention is characterized in that it is used directly to produce flame-retardant plastics and flame-retardant fiber materials alone, or is used as a macromolecular flame retardant for blending with other polymer materials to produce flame-retardant polymer materials.
[0058] Compared with the prior art, the present invention has the following advantages:
[0059] 1. Since the amount of flame retardant introduced into the phosphorus-containing copolymer flame-retardant nylon provided by the present invention is low, it not only avoids the destruction of the spinnability of the material, but also does not affect the excellent mechanical properties of the material, and at the same time can achieve efficient flame retardancy.
[0060] 2. Since the phosphorus-containing copolymer flame-retardant nylon provided by the present invention is an intrinsic flame-retardant nylon, there are no problems such as flame retardant migration and compatibility with the substrate, which not only solves the difficult problem of the contradiction between the flame retardant properties and mechanical properties of the material, but also makes the flame retardant efficiency more durable.
[0061] 3. Since the phosphorus-containing copolymer flame-retardant nylon provided by the present invention can not only achieve a flame retardant effect comparable to that of the prior art with a relatively small amount of flame retardant introduced (1 to 20 mol%), it does not need to be compounded with traditional flame retardants. In addition, in the case of a more preferred flame retardant, it can achieve flame retardant requirements at a lower introduction amount (1 to 3 mol%) while slightly improving mechanical properties, thereby greatly reducing the amount of flame retardant used and reducing costs.
[0062] 4. Since the polymerization and processing temperatures of the preparation method of the phosphorus-containing copolymer flame-retardant nylon provided by the present invention are within an appropriate range (melt polycondensation: 210-280°C, interfacial polymerization: 25°C), it will not cause premature decomposition of the substrate, so that the prepared copolymer nylon has good thermal stability, crystallization behavior, and certain chemical corrosion resistance and solvent resistance.
[0063] 5. Since the preparation process provided by the present invention is consistent with the traditional nylon production process, the process is mature, easy to operate, and easy to control and industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Figure 1 The phosphorus-containing copolymer flame-retardant nylon PA 66-co-DS prepared in Example 8 of the present invention 2 The tensile strength of pure PA 66 prepared in Example 2 is shown in the figure. 2 The tensile strength of the copolymer nylon is higher than that of pure PA 6, indicating that the introduction of flame retardant monomers will not destroy the mechanical properties of the copolymer nylon.
[0065] Figure 2 The phosphorus-containing copolymer flame-retardant nylon PA 6-co-MPA prepared in Example 5 of the present invention 1 The thermal gravimetric curve of pure PA 6 prepared in Example 1 is shown in Figure 1. 1 The thermal stability of the copolymer nylon is almost the same as that of pure PA 6, indicating that the introduction of flame retardant monomers does not affect the thermal stability of the copolymer nylon.
[0066] Figure 3 The phosphorus-containing copolymer flame-retardant nylon PA 6-co-BPA prepared in Example 17 of the present invention 3 The differential scanning calorimetry of pure PA 6 prepared in Example 4 is shown in Figure 4. 3 The melting point and crystallization temperature of copolymer nylon are not much different from those of pure PA 6, indicating that the introduction of flame retardant monomers will not destroy the processability of copolymer nylon.
[0067] Figure 4 The phosphorus-containing copolymer flame-retardant nylon PA 46-co-DS prepared in Example 3 of the present invention 2 The vertical combustion test combustion process diagram of pure PA 46 prepared in comparative example 3. As can be seen from the figure, pure PA 46 burns violently after ignition and produces a large number of molten droplets; while PA 46-co-DS 2 It will extinguish itself after ignition, showing excellent flame retardant properties.
[0068] Figure 5This is the H-NMR spectrum of the phosphorus-containing copolymer nylon PA 66-co-MP prepared in Example 24 of the present invention. 2.8ppm and 1.9ppm are the chemical shifts of hydrogen atoms on two methylene groups in adipoyl chloride (at positions a and b in the figure); 3.5ppm, 1.7ppm and 1.4ppm are the chemical shifts of hydrogen atoms on three methylene groups in hexamethylenediamine (at positions ce in the figure); 8-9ppm are the chemical shifts of hydrogen atoms on the benzene ring of the flame retardant monomer MP (at position f in the figure). All hydrogen atoms in the molecular structure of PA 66-co-MP have good peak assignments, indicating that it was successfully synthesized.
[0069] Figure 6 This is the infrared spectrum of the phosphorus-containing copolymer nylon PA 66-co-MP prepared in Example 24 of the present invention. As shown in the figure, the copolymer nylon 66 has a wavelength of 3300 cm -1 (NH), 2927cm -1 (-CH2), 2854cm -1 (-CH2-), 1600cm -1 (C=O) and 1527cm -1 (NH) shows typical polyamide peaks. In addition, copolymerized nylon 66 shows a peak at 1440 cm -1 PC absorption band appears at 1200cm -1 The P=O absorption peak appeared at , proving that PA 66-co-MP was successfully synthesized.
[0070] Figure 7 This is the H NMR spectrum of the phosphorus-containing copolymerized nylon PA 66-co-PDN prepared in Example 4 of the present invention, wherein 1.4ppm and 2.3ppm are the chemical shifts of hydrogen atoms on the methylene of adipic acid, i.e., the hydrogen atoms at positions a and b in the figure; 3.1ppm, 1.2ppm and 1.0ppm are the chemical shifts of hydrogen atoms on the methylene of the hexamethylenediamine group; and 6.7-8.3ppm are the chemical shifts of hydrogen atoms on the benzene ring of the flame retardant. All hydrogen atoms in the nylon 66 segment in PA 66-co-PDN and the flame retardant PDN segment can be well assigned, indicating the successful synthesis of the copolymerized nylon PA 66-co-PDN.
[0071] Figure 8 This is the infrared spectrum of the phosphorus-containing copolymer nylon PA 66-co-PDN prepared in Example 4 of the present invention. As shown in the figure, the copolymer nylon 66 has an infrared spectrum of 3303 cm -1 (NH), 2925cm -1 (-CH2), 2854cm -1 (-CH2-), 1639cm -1 (C=O) and 1538cm -1(NH) shows typical polyamide peaks. In addition, copolymerized nylon 66 shows a peak at 1443 cm -1 PC absorption band appears at 1174cm -1 The P=O absorption peak appeared at , proving that PA 66-co-PDN was successfully synthesized.
[0072] Fig. 9 This is the nuclear magnetic hydrogen spectrum of the phosphorus-containing copolymer nylon PA 6-co-CDP prepared in Example 21 of the present invention. As can be seen in the figure, the chemical shifts of hydrogen atoms in the alkyl segment after the ring opening of caprolactam are at 1.8-3.7ppm in the figure. The peak at 3.7ppm belongs to the chemical shift of hydrogen atoms in the methylene group close to the carbonyl group, that is, peak a; the peak at 2.8ppm belongs to the chemical shift of hydrogen atoms in the methylene group close to the amino group, that is, peak b; the peak at 1.9ppm belongs to the chemical shift of hydrogen atoms in the three methylene groups in the middle of the segment, that is, peak c. The integrated area ratio a:b:c=1:1:3 is proportional to the number of corresponding hydrogen atoms. In the figure, 7-9ppm is the chemical shift of hydrogen atoms on the benzene ring of the flame retardant monomer, that is, peak d. The peaks of hydrogen atoms on the polymer and the monomer can be well found, proving that the copolymer nylon was successfully synthesized.
[0073] Fig.10 This is the infrared spectrum of the phosphorus-containing copolymer nylon PA 6-co-CDP prepared in Example 21 of the present invention. As shown in the figure, the copolymer nylon 6 has an infrared spectrum of 3290 cm -1 (NH), 2922cm -1 (-CH2), 2854cm -1 (-CH2-), 1640cm -1 (C=O) and 1507cm -1 (NH) shows typical polyamide peaks. In addition, copolymerized nylon 6 shows a peak at 1436 cm -1 PC absorption band appears at 1200cm -1 The appearance of P=O absorption band at , proved that PA 6-co-CDP was successfully synthesized.
[0074] Fig.11The nuclear magnetic hydrogen spectrum of the phosphorus-containing copolymer nylon PA 6-co-PEC prepared in Example 25 of the present invention is shown in the figure. 1.0-4.0ppm is the chemical shift of the hydrogen atoms in the alkyl segment after the caprolactam ring is opened. The peak at 3.5ppm belongs to the chemical shift of the hydrogen atoms in the methylene group close to the carbonyl group, that is, peak a; the peak at 2.7ppm belongs to the chemical shift of the hydrogen atoms in the methylene group close to the amino group, that is, peak b; the peak at 1.7ppm belongs to the chemical shift of the hydrogen atoms in the three methylene groups in the middle of the segment, that is, peak c. The integrated area ratio a:b:c=1:1:3 is proportional to the number of corresponding hydrogen atoms. The peak at 7.1-10.0ppm belongs to the chemical shift of the hydrogen atoms on the benzene ring in PEC, that is, peak d. The peak attribution of hydrogen atoms on both the polymer and the monomer can be well found, proving that the copolymer nylon was successfully synthesized.
[0075] Fig.12 This is the infrared spectrum of the phosphorus-containing copolymerized nylon PA 6-co-PEC prepared in Example 25 of the present invention. As shown in the figure, the copolymerized nylon 6 has an infrared spectrum of 3292 cm -1 (NH), 2927cm -1 (-CH2), 2856cm -1 (-CH2-), 1634cm -1 (C=O) and 1539cm -1 (NH) shows typical polyamide peaks. In addition, copolymerized nylon 6 shows a peak at 1436 cm -1 PC absorption band appears at 1100cm -1 P=O absorption band appears at 725cm -1 The peak appearing at corresponds to the CH stretching vibration of benzene, proving that PA 6-co-PEC was successfully synthesized. DETAILED DESCRIPTION
[0076] The following examples are given to further illustrate the present invention. It is necessary to point out that the following examples cannot be understood as limiting the scope of protection of the present invention. If a person skilled in the art makes some non-essential improvements and adjustments to the present invention based on the above content of the present invention, it still belongs to the scope of protection of the present invention.
[0077] In addition, it is worth noting that: 1) The intrinsic viscosity [η] of the phosphorus-containing flame-retardant copolymer nylon obtained in the following examples and the pure PA 6 and PA 66 of the comparative examples are all prepared with formic acid as the solvent, and the solution is prepared with a concentration of 0.5 g / dL, and tested with an Ubbelohde viscometer at 25°C; 2) The limiting oxygen index of the phosphorus-containing flame-retardant copolymer nylon obtained in the following examples and the pure PA 6 and PA 66 of the comparative examples are all prepared by making them into 120×6.5×3.2 mm 3The vertical burning grade of the phosphorus-containing flame-retardant copolymer nylon obtained in the following examples and the pure PA 6 and PA 66 of the comparative examples is obtained by making it into 125×12.7×3.2mm 3 4) The tensile strength of the phosphorus-containing flame-retardant copolymer nylon obtained in the following examples and the pure PA 6 and PA 66 of the comparative examples were measured by making dumbbell-shaped specimens with a narrow neck width of 4.0±0.1mm and a thickness of 2.0±0.1mm according to ASTM D-638 using an INSTRON 3366 universal testing machine.
[0078] Example 1
[0079] 113g (0.1mol) of caprolactam, 0.7g (0.005mol) of adipic acid, 5g of secondary water, and 16.5g (0.03mol) of N,N'-di(2-aminophenyl)-P-cage-shaped phosphate-phenylphosphine diamide were added into a polymerization container according to the proportion, and the temperature was raised to 250°C under a nitrogen atmosphere to carry out a ring-opening polycondensation reaction for 3h, and the water molecules generated in the system were removed for 3h, and then vacuumed for 1h to finally obtain a copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0080] The flame retardant nylon has an intrinsic viscosity [η] of 1.38 dL / g, a limiting oxygen index of 29.3%, a vertical combustion grade of V-0, no melting drop, a tensile strength of 70 MPa, a tensile modulus of 2485 MPa, a flexural strength of 142 MPa, and a flexural modulus of 3106 MPa.
[0081] Example 2
[0082] 118g (1mol) of succinic acid and 102g (1mol) of butanediamine were dissolved in ethanol, reacted to form salts and precipitated, and filtered and dried to prepare a 50wt% aqueous solution; 170.0g (0.5mol) of 5-[(bis(2-oxazolidine-3-amino)phosphoryl]m-phenylenediamine and 83.0g (0.5mol) of adipic acid were dissolved in ethanol, reacted to form salts and precipitated, and filtered and dried to prepare a 50wt% aqueous solution; the two aqueous solutions were added to a reaction kettle, and a certain amount of hexanediamine was added to make the mole number of diamine in the reaction system: the mole number of dibasic acid = 0.8:1, the temperature was raised to 220°C, the pressure was increased to 1.6MPa, and a prepolymerization reaction was carried out under this condition for 0.5h; then, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 5000Pa and the system temperature was gradually increased, and a polycondensation reaction was carried out at 255°C for 0.5h to obtain a product.
[0083] The flame retardant nylon has an intrinsic viscosity [η] of 1.50 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-0, no melting drop, a tensile strength of 55 MPa, a tensile modulus of 1967 MPa, a flexural strength of 90 MPa, and a flexural modulus of 2850 MPa.
[0084] Example 3
[0085] 92.4 g (1.05 mol) of diaminobutane, 96 g (2.4 mol) of sodium hydroxide and 5 g of tetramethylammonium bromide were dissolved in 1 L of secondary water to prepare solution A; 183 g (1 mol) of adipoyl chloride and 7.8 g (0.02 mol) of 5-(diphenylphosphoramido)isophthalic acid were dissolved in 2 L of dichloromethane to prepare solution B; solution A and solution B were weighed so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1:1; solution B was quickly poured into solution A under rapid stirring at 2000 rpm, and stirring was continued for 30 min to complete polymerization and precipitate a large amount of fibrous solids, which were filtered, washed and dried to obtain the product.
[0086] The flame retardant nylon has an intrinsic viscosity [η] of 1.21 dL / g, a limiting oxygen index of 34.2%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 72 MPa, a tensile modulus of 2844 MPa, a flexural strength of 139 MPa, and a flexural modulus of 3455 MPa.
[0087] Example 4
[0088] 146g (1 mol) of adipic acid and 102g (1 mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 40wt% aqueous solution; 8.8g (0.02mol) of N, N'-di(2-aminophenyl)-P-cage phosphate-phenylphosphonic acid diamide and 8.8g (0.06mol) of adipic acid were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 40wt% aqueous solution. The two aqueous solutions were added to a reactor, and a certain amount of adipic acid was added to make the mole number of diamine in the reaction system: the mole number of dibasic acid = 1:1, the temperature was raised to 230°C, the pressure was increased to 2.4MPa, and the prepolymerization reaction was carried out under this condition for 2h. Subsequently, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 4000Pa and the system temperature was gradually increased, and the polycondensation reaction was carried out at 260°C for 1h to obtain the product.
[0089] The flame retardant nylon has an intrinsic viscosity [η] of 1.11 dL / g, a limiting oxygen index of 28.8%, a vertical combustion grade of V-0, no droplets, a tensile strength of 69 MPa, a tensile modulus of 2800 MPa, a flexural strength of 140 MPa, and a flexural modulus of 3500 MPa.
[0090] Example 5
[0091] 113g (1 mol) of caprolactam, 0.5g (0.004 mol) of benzoic acid, 10g of secondary water, and 6.1g (0.01 mol) of 5-((phenylmethylphosphoryl)amino)isophthalic acid were added into a polymerization container according to the ratio, and the temperature was raised to 260°C under a nitrogen atmosphere to carry out a ring-opening polycondensation reaction for 4 hours, and the water molecules generated in the system were removed for 2 hours, and then vacuumed for 1.5 hours to obtain flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0092] The flame retardant nylon has an intrinsic viscosity [η] of 1.44 dL / g, a limiting oxygen index of 28.8%, a vertical combustion grade of V-0, no melting drop, a tensile strength of 82 MPa, a tensile modulus of 2377 MPa, a flexural strength of 135 MPa, and a flexural modulus of 3050 MPa.
[0093] Example 6
[0094] 118g (1 mol) of succinic acid and 116g (1 mol) of hexamethylenediamine were dissolved in ethanol, precipitated after salt formation, filtered and dried to prepare a 30wt% aqueous solution; 11.9g (0.03mol) of bis (4- (((4-aminophenyl) imino) methyl) phenyl) phenylphosphonate and 16.38g (0.03mol) of hexamethylenediamine were dissolved in ethanol, precipitated after salt formation, filtered and dried to prepare a 30wt% aqueous solution. The two aqueous solutions were added to a reactor, a certain amount of adipic acid was added to make the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.2:1, the temperature was raised to 240°C, the pressure was increased to 2.5MPa, and a prepolymerization reaction was carried out under this condition for 1h; then, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 3000Pa and the system temperature was gradually increased, and a polycondensation reaction was carried out at 250°C for 1.5h to obtain a product.
[0095] The flame retardant nylon has an intrinsic viscosity [η] of 0.93 dL / g, a limiting oxygen index of 28.3%, a vertical combustion grade of V-1, a tensile strength of 97 MPa, a tensile modulus of 2885 MPa, a flexural strength of 130 MPa, and a flexural modulus of 3000 MPa.
[0096] Example 7
[0097] 102g (1mol) of pentamethylenediamine, 111.3g (1.05mol) of sodium carbonate, 3g of benzyltriethylammonium bromide and 1g of tetrapropylammonium bromide were dissolved in 1L of secondary water to prepare solution A; 262.9g (1mol) of sebacic acid chloride and 82.8g (0.20mol) of 2-((diphenoxyphosphoryl)amino)terephthalic acid were dissolved in 2L of a mixed solvent of benzene and toluene (volume ratio 1:1) to prepare solution B; solution A and solution B were weighed so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 0.8:1; solution B was quickly poured into solution A at a stirring speed of 1200rpm, and stirring was continued for 60min to complete polymerization and precipitate a large amount of fibrous solids, which were filtered, washed and dried to obtain a product.
[0098] The flame retardant nylon has an intrinsic viscosity [η] of 1.05 dL / g, a limiting oxygen index of 26.0%, a vertical combustion grade of V-0, no droplets, a tensile strength of 88 MPa, a tensile modulus of 2078 MPa, a flexural strength of 120 MPa, and a flexural modulus of 3200 MPa.
[0099] Example 8
[0100] 146g (1 mol) of adipic acid and 102g (1 mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 20wt% aqueous solution; 7.6g (0.02mol) of 5-(diphenylphosphoramido)phthalic acid and 2.3g (0.02mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 20wt% aqueous solution. The two aqueous solutions were added to a reactor, and a certain amount of adipic acid was added to make the mole number of diamine in the reaction system: the mole number of dibasic acid = 1.1:1, and the temperature was raised to 230°C and the pressure was increased to 2.1MPa for prepolymerization reaction for 1.5h. Subsequently, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 8000Pa and the system temperature was gradually increased, and the polycondensation reaction was carried out at 260°C for 2h to obtain the product.
[0101] The flame retardant nylon has an intrinsic viscosity [η] of 1.11 dL / g, a limiting oxygen index of 28.8%, a vertical combustion grade of V-1, a small amount of molten droplets, a tensile strength of 92 MPa, a tensile modulus of 2738 MPa, a flexural strength of 142 MPa, and a flexural modulus of 3277 MPa.
[0102] Example 9
[0103] 85.1g (1mol) butyrolactam, 0.5g (0.004mol) benzoic acid, 6g secondary water, 14.6g (0.04moL) N,N'-(piperazine-1,4-diyl) di-p-phenylene phosphinamide were added into a polymerization container according to the ratio, heated to 230°C in a nitrogen atmosphere, and the ring-opening polycondensation reaction was carried out for 3h, and the water molecules generated in the system were removed for 2h, and then vacuumed for 2h to finally obtain copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0104] The flame retardant nylon has an intrinsic viscosity [η] of 1.44 dL / g, a limiting oxygen index of 32.4%, a vertical combustion grade of V-0, no melting drop, a tensile strength of 78 MPa, a tensile modulus of 2795 MPa, a flexural strength of 115 MPa, and a flexural modulus of 3000 MPa.
[0105] Example 10
[0106] 118.8 g (1.1 mol) of p-phenylenediamine, 145 g (1.05 mol) of potassium carbonate and 6 g of benzyltriethylammonium chloride are prepared into solution A in 1 L of secondary water; 203 g (1 mol) of terephthaloyl chloride and 12.8 g (0.03 mol) of 3,9-bis(4-carboxypiperazinyl)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane-3,9-dioxide are dissolved in 2 L of carbon tetrachloride to prepare solution B; solution A and solution B are weighed so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.2:1; solution B is quickly poured into solution A at a stirring speed of 500 rpm, and stirring is continued for 120 min to complete polymerization and precipitate a large amount of fibrous solids, which are filtered, washed and dried to obtain a product.
[0107] The flame retardant nylon has an intrinsic viscosity [η] of 1.31 dL / g, a limiting oxygen index of 31.2%, a vertical combustion grade of V-0, no droplets, a tensile strength of 102 MPa, a tensile modulus of 2522 MPa, a flexural strength of 150 MPa, and a flexural modulus of 3650 MPa.
[0108] Embodiment 11
[0109] 139.2g (1.2mol) of hexamethylenediamine, 100.8g (1.2mol) of sodium bicarbonate, 48g (1.2mol) of sodium hydroxide, 2g of tetramethylammonium bromide and 3g of tetrapropylammonium bromide were dissolved in 1L of secondary water to prepare solution A; 183g (1mol) of adipic acid chloride and 54.5g (0.1mol) of (4,6-bis (4-carboxyphenoxy) -1,3,5-triazine-2-yl) phosphonic acid dimethyl ester were dissolved in 2L of a mixed solvent of cyclohexane and pentane (volume ratio 1:1) to prepare solution B; solution A and solution B were weighed so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.1:1; solution B was quickly poured into solution A at a stirring speed of 1500rpm, and after continuing to stir for 10min, polymerization was completed to precipitate a large amount of fibrous solids, and the product was obtained after suction filtration, washing and drying.
[0110] The flame retardant nylon has an intrinsic viscosity [η] of 0.98 dL / g, an oxygen index of 27.0%, a vertical combustion grade of V-0, no droplets, a tensile strength of 85 MPa, a tensile modulus of 2022 MPa, a flexural strength of 170 MPa, and a flexural modulus of 4500 MPa.
[0111] Example 12
[0112] 211.2g (1mol) tridecane lactam, 0.8g (0.005mol) terephthalic acid, 5g secondary water, 25.52g (0.08mol) 2-(methylphenylphosphorylamino) terephthalic acid were put into a polymerization container, heated to 240°C under a nitrogen atmosphere, and the ring-opening polycondensation reaction was carried out for 3h, and the water molecules generated in the system were removed for 4h, and then vacuumed for 2h to finally obtain copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0113] The flame retardant nylon has an intrinsic viscosity [η] of 0.79 dL / g, a limiting oxygen index of 31.4%, a vertical combustion grade of V-0, no melting drop, a tensile strength of 76 MPa, a tensile modulus of 2897 MPa, a flexural strength of 110 MPa, and a flexural modulus of 2900 MPa.
[0114] Example 13
[0115] 113g (1 mol) of caprolactam, 0.14g (0.001 mol) of adipic acid, 1g of secondary water, and 435.1g (0.99 mol) of 2-((diphenoxyphosphoryl)amino)isophthalic acid were placed in a polymerization container, heated to 250°C in a nitrogen atmosphere, and subjected to a ring-opening polycondensation reaction for 3 hours. The water molecules generated in the system were removed for a reaction of 3 hours, and then vacuumed for 1 hour to finally obtain a copolymer flame-retardant nylon. The product can be used directly after drying without post-treatment.
[0116] The flame retardant nylon has an intrinsic viscosity [η] of 0.47 dL / g, a limiting oxygen index of 36.4%, a vertical combustion grade of V-0, no droplets, a tensile strength of 57 MPa, a tensile modulus of 1700 MPa, a flexural strength of 92 MPa, and a flexural modulus of 2610 MPa.
[0117] Embodiment 14
[0118] 166g (1 mol) of terephthalic acid and 116g (1 mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 10wt% aqueous solution; 4.1g (0.01mol) of 4-((diphenylphosphino)amino)phthalic acid and 11.6g (0.1mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 10wt% aqueous solution. The two aqueous solutions were added to a reactor, a certain amount of hexamethylenediamine was added to make the mole number of diamine in the reaction system: the mole number of dibasic acid = 1.1:1, the temperature was raised to 240°C, the pressure was increased to 2.4MPa, and a prepolymerization reaction was carried out for 2h; then, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 2000Pa and the system temperature was gradually increased, and a polycondensation reaction was carried out at 270°C for 2h to obtain a product.
[0119] The flame retardant nylon has an intrinsic viscosity [η] of 0.99 dL / g; a limiting oxygen index of 28.4%, a vertical combustion grade of V-1 with a small amount of droplets, a tensile strength of 73 MPa, a tensile modulus of 2297 MPa, a flexural strength of 130 MPa, and a flexural modulus of 3200 MPa.
[0120] Embodiment 15
[0121] 202g (1 mol) of decanedioic acid and 172g (1 mol) of decanediamine were dissolved in ethanol, reacted to form salt and precipitated, and filtered and dried to prepare a 50wt% aqueous solution; 234.0g (0.25mol) of polybis (4-(((4-aminophenyl) imino) methyl) phenyl) phenyl phosphonate and 8.6g (0.1mol) of decanediamine were dissolved in ethanol, reacted to form salt and precipitated, and filtered and dried to prepare a 50wt% aqueous solution; the two aqueous solutions were added to a reaction kettle, a certain amount of hexamethylenediamine was added to make the molar number of diamine in the reaction system: the molar number of dibasic acid = 1:1, the temperature was raised to 210°C, the pressure was increased to 2.2MPa, and a prepolymerization reaction was carried out for 3h; then, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 5000Pa and the system temperature was gradually increased, and a condensation reaction was carried out at 280°C for 0.5h to obtain a product.
[0122] The flame retardant nylon has an intrinsic viscosity [η] of 0.93 dL / g, a limiting oxygen index of 29.3%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 69 MPa, a tensile modulus of 1979 MPa, a flexural strength of 98 MPa, and a flexural modulus of 2950 MPa.
[0123] Example 16
[0124] 230 g (1 mol) of dodecanedioic acid and 116 g (1 mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salt and precipitated, and then filtered and dried to prepare a 60 wt% aqueous solution; 3.92 g (0.08 mol) of bis (1-oxo-2,6,7-trioxo-1-phosphobicyclo [2.2.2] octane-4-yl) 2,5-diaminoterephthalate and 11.6 g (0.1 mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salt and precipitated, and then filtered and dried to prepare a 60 wt% aqueous solution. Add two aqueous solutions into a reactor, add a certain amount of hexamethylenediamine so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.01:1; add the two aqueous solutions into the reactor, heat to 230°C, pressurize to 3.0MPa and carry out prepolymerization reaction for 1 hour; then, gradually discharge the water vapor in the system, and when the pressure in the system drops to normal pressure, start to evacuate to 10000Pa and gradually increase the system temperature, and carry out polycondensation reaction at 270°C for 1 hour to obtain the product.
[0125] The flame retardant nylon has an intrinsic viscosity [η] of 0.72 dL / g, a limiting oxygen index of 29.5%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 96 MPa, a tensile modulus of 2115 MPa, a flexural strength of 120 MPa, and a flexural modulus of 3300 MPa.
[0126] Embodiment 17
[0127] 113g (1mol) caprolactam, 0.5g (0.004mol) benzoic acid, 10g secondary water, 17.6g (0.03mol) 5-(di([1,1'-biphenyl])phosphonyl)amino)isophthalic acid were put into a polymerization container, heated to 220°C in a nitrogen atmosphere for 4h of ring-opening polycondensation reaction, the water molecules generated in the system were removed for 2h, and then vacuumed for 2h to finally obtain copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0128] The flame retardant nylon has an intrinsic viscosity [η] of 0.76 dL / g, a limiting oxygen index of 31.6%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 67 MPa, a tensile modulus of 2200 MPa, a flexural strength of 145 MPa, and a flexural modulus of 3567 MPa.
[0129] Embodiment 18
[0130] 230g (1mol) of tetradecanedioic acid and 200g (1mol) of tetradecanedioic acid were dissolved in ethanol, precipitated after salt formation, filtered and dried to prepare a 90wt% aqueous solution; 21.2g (0.05mol) of 1-oxido-2,6,7-trioxa-1-phosphabicyclo [2.2.2] octane-4-yl) methylbis (4-methylpiperazine-1-yl) phosphine and 46g (0.2mol) of dodecanedioic acid were dissolved in ethanol, precipitated after salt formation, filtered and dried to prepare a 90wt% aqueous solution. The two aqueous solutions were added to a reactor, and a certain amount of dodecanedioic acid was added to make the mole number of diamine in the reaction system: the mole number of dibasic acid = 0.9:1, and the temperature was raised to 240°C and the pressure was increased to 2.8MPa for prepolymerization reaction for 2.5h. Subsequently, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 1000 Pa and the system temperature was gradually increased. The polycondensation reaction was carried out at 280°C for 3 hours to obtain the product.
[0131] The flame retardant nylon has an intrinsic viscosity [η] of 0.63 dL / g, a limiting oxygen index of 30.4%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 70 MPa, a tensile modulus of 2679 MPa, a flexural strength of 112 MPa, and a flexural modulus of 3100 MPa.
[0132] Embodiment 19
[0133] 197g (1mol) tridecanoic acid, 1.4g (0.01mol) adipic acid, 10g secondary water, 30.5g (0.01mol) 2-(4,6-bis(4-aminophenoxy)-1,3,5-triazine-2-yl)-5,5-dimethyl-1,3,2-dioxaphosphine 2-oxide were put into a polymerization container, heated to 240°C in a nitrogen atmosphere for ring-opening polycondensation reaction for 3h, the water molecules generated in the system were removed for reaction for 3h, and then vacuumed for 2h to finally obtain copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0134] The flame retardant nylon has an intrinsic viscosity [η] of 0.61 dL / g, a limiting oxygen index of 29.3%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 80 MPa, a tensile modulus of 2675 MPa, a flexural strength of 140 MPa, and a flexural modulus of 3800 MPa.
[0135] Embodiment 20
[0136] 166g (1 mol) of terephthalic acid and 158g (1 mol) of nonanediamine were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 70wt% aqueous solution; 7.9g (0.02mol) of 5-[(bis(2-oxazolidine-3-amino)phosphoryl]isophthalic acid and 15.9g (0.1mol) of nonanediamine were dissolved in ethanol, reacted to form salts and precipitated, filtered and dried to prepare a 70wt% aqueous solution. The two aqueous solutions were added to a reactor, and a certain amount of nonanediamine was added to make the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.2:1, and the temperature was raised to 230°C and the pressure was increased to 2.0MPa for prepolymerization reaction for 1.5h. Subsequently, the water vapor in the system was gradually discharged, and when the pressure in the system dropped to normal pressure, vacuum was evacuated to 1000Pa and the system temperature was gradually increased, and a polycondensation reaction was carried out at 270°C for 1.5h to obtain the product.
[0137] The flame retardant nylon has an intrinsic viscosity [η] of 0.87 dL / g, a limiting oxygen index of 35.7%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 76 MPa, a tensile modulus of 2374 MPa, a tensile strength of 132 MPa, and a bending modulus of 3987 MPa.
[0138] Embodiment 21
[0139] 113g (1 mol) of valerolactam, 1.4g (0.01 mol) of adipic acid, 6g of secondary water, and 5.5g (0.01 mol) of 5-(diphenylphosphorylamino)phthalic acid were added into a polymerization container according to the ratio, and the temperature was raised to 260°C under a nitrogen atmosphere to carry out a ring-opening polycondensation reaction for 3 hours, and the water molecules generated in the system were removed for 3 hours, and then vacuumed for 0.5 hours to finally obtain a copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0140] The flame retardant nylon has an intrinsic viscosity [η] of 1.35 dL / g, a limiting oxygen index of 24.3%, a vertical combustion grade of V-2, a small amount of droplets, a tensile strength of 84 MPa, a tensile modulus of 2700 MPa, a flexural strength of 138 MPa, and a flexural modulus of 3750 MPa.
[0141] Embodiment 22
[0142] 113g (1mol) caprolactam, 0.7g (0.005mol) adipic acid, 5g secondary water, 8.8g (0.02mol) N,N'-di(2-aminotriazine)-P-cage-shaped phosphate-phenylphosphonic acid diamide were put into a polymerization container, heated to 250℃ for ring-opening polycondensation reaction for 2h under nitrogen atmosphere, and the water molecules generated in the system were removed for reaction for 2h, and then vacuumed for 1h to finally obtain copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0143] The flame retardant nylon has an intrinsic viscosity [η] of 0.69 dL / g, a limiting oxygen index of 28.7%, a vertical combustion grade of V-1, no melting drop, a tensile strength of 69 MPa, a tensile modulus of 2579 MPa, a flexural strength of 145 MPa, and a flexural modulus of 3400 MPa.
[0144] Embodiment 23
[0145] 146g (1mol) of adipic acid and 116g (1mol) of hexamethylenediamine are dissolved in ethanol, react to form salt and precipitate, and then filter and dry to prepare a 40wt% aqueous solution; 30.1g (0.04mol) of bis(4-((()4-aminophenyl)imino)methyl)phenyl)piperazine-1,4-diylbisphenylphosphinate and 6.96g (0.06mol) of hexamethylenediamine are dissolved in ethanol, react to form salt and precipitate, and then filter and dry to prepare a 40wt% aqueous solution. Add the two aqueous solutions into the reaction kettle, add a certain amount of hexamethylenediamine so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.02:1, raise the temperature to 230°C, and pressurize to 1.8MPa for prepolymerization reaction for 2h; then, gradually discharge the water vapor in the system, and when the pressure in the system drops to normal pressure, start to evacuate to 4000Pa and gradually increase the system temperature, and carry out condensation reaction at 260°C for 2h to obtain the product.
[0146] The flame retardant nylon has an intrinsic viscosity [η] of 1.44 dL / g, a limiting oxygen index of 35.0%, a vertical combustion grade of V-0 without melting drops, a tensile strength of 120 MPa, a tensile modulus of 2994 MPa, a flexural strength of 170 MPa, and a flexural modulus of 4500 MPa.
[0147] Embodiment 24
[0148] 139.2g (1.2mol) hexamethylenediamine, 115.2g (1.2mol) triethylamine and pyridine, 2g benzyltriethylammonium bromide were prepared into solution A in 1L secondary water; 183g (1mol) adipic acid chloride and 120g (0.3mol) 5-((dimorpholinophosphoryl)amino)isophthalic acid were dissolved in 2L chloroform to prepare solution B. Solution A and solution B were weighed so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.1:1; solution B was quickly poured into solution A at a stirring speed of 1000rpm, and the stirring was continued for 100min to complete the polymerization and precipitate a large amount of fibrous solids, which were filtered, washed and dried to obtain the product.
[0149] The flame retardant nylon has an intrinsic viscosity [η] of 1.25 dL / g, a limiting oxygen index of 28.0%, a vertical combustion grade of V-1, no droplets, a tensile strength of 81 MPa, a tensile modulus of 1900 MPa, a flexural strength of 90 MPa, and a flexural modulus of 2800 MPa.
[0150] Embodiment 25
[0151] 113g (1mol) caprolactam, 0.7g (0.006mol) benzoic acid, 6g secondary water, 44.9g (0.04mol) bis (4-(((4-aminophenyl) amino)(6-oxydibenzo[1,2]oxaphosphin-6-yl)methyl)phenyl)phenylphosphonate were put into a polymerization container, heated to 255°C in a nitrogen atmosphere for ring-opening polycondensation reaction for 2h, the water molecules generated in the system were removed for reaction for 4h, and then vacuumed for 0.8h to finally obtain copolymer flame-retardant nylon. The product can be used directly without post-treatment after drying.
[0152] The flame retardant nylon has an intrinsic viscosity [η] of 0.89 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-0, no melting drop, a tensile strength of 50 MPa, a tensile modulus of 1700 MPa, a flexural strength of 90 MPa, and a flexural modulus of 2600 MPa.
[0153] Embodiment 26
[0154] 146g (1 mol) of adipic acid and 116g (1 mol) of hexamethylenediamine were dissolved in ethanol, precipitated after salt formation, filtered and dried, and then prepared into an 80wt% aqueous solution; 597g (0.5mol) of bis(4-(((4-aminophenyl)amino)(6-oxydibenzo[1,2]phosphin-6-yl)methyl)phenyl)piperazine-1,4-diylbis(phenyl phosphate) and 58.0g (0.5mol) of hexamethylenediamine were dissolved in ethanol, reacted to form salt, and precipitated. After filtering and drying, the mixture is prepared into an 80wt% aqueous solution; the two aqueous solutions are added into a reaction kettle, and a certain amount of hexamethylenediamine is added so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.02:1, and the temperature is raised to 235°C and the pressure is increased to 2.6MPa for prepolymerization reaction for 2.5h; then, the water vapor in the system is gradually discharged, and when the pressure in the system drops to normal pressure, vacuum is evacuated to 1500Pa and the system temperature is gradually increased, and a condensation reaction is carried out at 265°C for 1h to obtain a product.
[0155] The flame retardant nylon has an intrinsic viscosity [η] of 0.87 dL / g, a limiting oxygen index of 30.0%, a vertical combustion grade of V-1 without melting drops, a tensile strength of 53 MPa, a tensile modulus of 2488 MPa, a flexural strength of 91 MPa, and a flexural modulus of 2882 MPa.
[0156] Embodiment 27
[0157] 139.2 g (1.2 mol) of hexamethylenediamine, 115.2 g (1.2 mol) of ammonium carbonate, and 2 g of tetrabutylammonium chloride were prepared into solution A in 1 L of secondary water; 183 g (1 mol) of adipic acid chloride and 163.5 g (0.3 mol) of 3,9-bis((4-aminophenyl)amino)-2,4,8,10-tetraoxy-3,9-diphosphaspiro[5.5]undecane-3,9-dioxide were dissolved in 2 L of carbon tetrachloride to prepare solution B; solution A and solution B were weighed so that the molar number of diamine in the reaction system: the molar number of dibasic acid = 1.1:1; solution B was quickly poured into solution A at a stirring speed of 1200 rpm, and stirring was continued for 20 minutes to complete polymerization and precipitate a large amount of fibrous solids, which were filtered, washed, and dried to obtain the product.
[0158] The flame retardant nylon has an intrinsic viscosity [η] of 1.16 dL / g, a limiting oxygen index of 29.0%, a vertical combustion grade of V-1, no droplets, a tensile strength of 67 MPa, a tensile modulus of 2428 MPa, a flexural strength of 133 MPa, and a flexural modulus of 3060 MPa.
[0159] Comparative Example 1
[0160] 113g (1 mol) of caprolactam, 0.7g (0.005 mol) of adipic acid, and 5g of secondary water were added to a polymerization container, and the temperature was raised to 250°C for ring-opening polycondensation reaction for 3 hours under a nitrogen atmosphere, and the water molecules generated in the system were removed for 3 hours, and then vacuumed for 1 hour to obtain copolymerized nylon. The product can be used directly without post-treatment after drying.
[0161] The copolymer nylon has an intrinsic viscosity [η] of 0.50 dL / g; a limiting oxygen index of 20.5%, a vertical combustion grade of V-2, droplets, a tensile strength of 60 MPa, a tensile modulus of 1600 MPa; a flexural strength of 85 MPa, and a flexural modulus of 2700 MPa.
[0162] Comparative Example 2
[0163] 146 g (1 mol) of adipic acid and 116 g (1 mol) of hexamethylenediamine are dissolved in ethanol, reacted to form salt and precipitated, filtered and dried, and then prepared into a 50 wt% aqueous solution; the aqueous solution is added to a reactor, and a certain amount of hexamethylenediamine is added to make the mole number of all diamines: the mole number of all dibasic acids = 1.01:1, and the temperature is raised to 240° C. and the pressure is increased to 2.2 MPa to carry out a prepolymerization reaction for 1.5 hours; then, the water vapor in the system is gradually discharged, and when the pressure in the system drops to normal pressure, vacuum is evacuated to 5000 Pa and the system temperature is gradually increased, and a condensation reaction is carried out at 280° C. for 1 hour to obtain a product.
[0164] The copolymer nylon has an intrinsic viscosity [η] of 1.20 dL / g; a limiting oxygen index of 21.5%, a vertical combustion grade of V-2 with droplets, a tensile strength of 81 MPa, a tensile modulus of 2200 MPa, a flexural strength of 112 MPa, and a flexural modulus of 3300 MPa.
[0165] Comparative Example 3
[0166] 88g (1mol) of diaminodiamine, 80g (2mol) of sodium hydroxide and 5g of tetrabutylammonium chloride were dissolved in 1L of secondary water to prepare solution A; 183g (1mol) of adipic acid chloride was dissolved in 1L of dichloromethane to prepare solution B. Solution A and solution B were weighed so that the molar number of all diamines in the system: the molar number of all diacyl chlorides = 1:1; solution B was quickly poured into solution A at a stirring speed of 1500rpm, and the stirring was continued for 30min to complete the polymerization and precipitate a large amount of fibrous solids, which were filtered, washed and dried to obtain the product.
[0167] The intrinsic viscosity [η] of the copolymer nylon is 1.09 dL / g; the limiting oxygen index is 21.0%, the vertical combustion grade is stepless with droplets, the tensile strength is 65 MPa, the tensile modulus is 1999 MPa; the flexural strength is 85 MPa, and the flexural modulus is 2900 MPa.
[0168] Comparative Example 4
[0169] 113g (1 mol) of caprolactam, 0.7g (0.005 mol) of adipic acid, and 10g of secondary water were placed in a polymerization container, heated to 255°C for 4 hours under a nitrogen atmosphere, and the water molecules generated in the system were removed for 3 hours, and then vacuumed for 1 hour to obtain copolymerized nylon. The product can be used directly without post-treatment after drying.
[0170] The copolymer nylon has an intrinsic viscosity [η] of 0.43 dL / g; a limiting oxygen index of 21.0%, a vertical combustion grade of V-2, droplets, a tensile strength of 55 MPa, a tensile modulus of 1478 MPa; a flexural strength of 100 MPa, and a flexural modulus of 2500 MPa.
Claims
1. A phosphorus-containing flame-retardant copolymer nylon, characterized in that The flame retardant nylon is composed of the following structural units represented by Ⅰ, Ⅳ or Ⅱ, Ⅲ, Ⅳ: In the formula, R1 represents C3~C 12 of alkylene; Among them, R2 represents C2~C 12 An alkylene or arylene group; Among them, R3 represents C4~C 14 An alkylene group or an arylene group, R2 and R3 are not arylene groups at the same time; Wherein R4 and R5 are carbonyl, imino or m is an integer of 2 to 12, R4 and R5 are the same or different; Y is an oxygen atom or an imino group, Z1 and Z2 are any one of an H atom, a hydroxyl group, a methyl group or a methoxy group, Z1 and Z2 are the same or different; Z3 and Z4 are methylene, phenyl, biphenyl, sulfone, azo, piperazine, Z5 is any one of methyl, methoxy, phenyl or phenoxy, Among them, the number of structural units of IV is 1 to 3% of the number of structural units of II, the number of structural units of III: the number of structural units of [II+IV] = 1, or the preferred number of structural units of IV is 1 to 3% of the number of structural units of III, the number of structural units of II: the number of structural units of [III+IV] = 1, or the preferred number of structural units of IV is 1 to 3% of the number of structural units of I, its intrinsic viscosity [η] is 0.64 to 1.50 dL / g, and the limiting oxygen index is 28.3 to 36.4%; the vertical burning grade is V-1 to V-0; the tensile strength is 67 to 120 MPa, and the tensile modulus is 2200 to 2885 MPa; the flexural strength is 130-170 MPa, and the flexural modulus is 3000 to 4500 MPa.
2. A method for preparing the phosphorus-containing flame-retardant nylon according to claim 1, characterized in that The process steps and conditions of the preparation method are as follows: (1) dissolving a nylon polymerized monomer dibasic acid and a nylon polymerized monomer diamine in ethanol, precipitating the salt after salt formation, filtering and drying to prepare a 10-90 wt % aqueous solution for standby use; (1) dissolving a nylon polymerization monomer diamine, an acid binding agent and a phase transfer catalyst in a molar ratio of 1:1-2.4:0.001-0.1 in water to prepare a 0.1-40 wt % aqueous phase solution; (2) dissolving a flame retardant monomer with a carboxyl terminal group and a nylon polymer monomer diamine in a molar ratio of 1:1-1:1.1 or a flame retardant monomer with an amino terminal group and a nylon polymer monomer diamine in a molar ratio of 1:1 in ethanol, reacting to form a salt, filtering and drying, and preparing a 10-90 wt % aqueous solution for standby use; (3) Add the above two aqueous solutions to a reaction kettle, and then add nylon polymerized monomer dibasic acid or nylon polymerized monomer diamine, so that the molar number of the flame retardant monomer with a carboxyl terminal group is 1 to 99% of the molar number of the nylon polymerized monomer dibasic acid, or the molar number of the flame retardant monomer with an amino terminal group is 1 to 99% of the molar number of the nylon polymerized monomer diamine, and the molar number of the nylon polymerized monomer + the diamine of the flame retardant monomer: the molar number of the nylon polymerized monomer + the dibasic acid of the flame retardant monomer in the reaction system is 0.8 to 1.2:1, and then at a temperature of 210 to 240° C. and a pressure of 1.6 to 3.0 MPa, prepolymerize for 0.5 to 3 hours, gradually discharge the water vapor in the system, and start to evacuate to 1000 to 10000 Pa when the pressure drops to normal pressure, and then gradually increase the system temperature, and carry out a condensation reaction at 250 to 280° C. for 0.5 to 3 hours to obtain a copolymerized nylon product having structural units II, III, and IV, or Flame retardant monomers, lactams, nylon polymer monomer dibasic acids or diamines with carboxyl or amino terminal groups are added into a polymerization container at a molar ratio of 0.01-0.99:1:0.001-0.1, and the temperature is raised to 220-260°C under nitrogen protection for reaction for 2-4 hours, and then the water vapor in the system is gradually removed, and the reaction is continued for 2-4 hours, and finally the system is evacuated to 1000-2000Pa for reaction for 0.5-2 hours to obtain copolymer nylon products with structural units I and IV.
3. The method for preparing phosphorus-containing flame-retardant nylon according to claim 2, characterized in that In the preparation method, the flame retardant monomer having a carboxyl terminal or an amino terminal is any one of the following general structural formulas: In the formula, X1 and X2 are carboxyl, chloro, amino, m is an integer of 2 to 12, n is an integer of 0 to 5, X1 and X2 are the same or different; Y is an oxygen atom or an imino group, Z1 and Z2 are any one of an H atom, a hydroxyl group, a methyl group or a methoxy group, Z1 and Z2 are the same or different; Z3 and Z4 are methyl, phenyl, biphenyl, sulfone, azo, piperazine, Any one of; Z5 is any one of methyl, methoxy, phenyl or phenoxy.
4. The method for preparing phosphorus-containing flame-retardant nylon according to claim 2 or 3, characterized in that The general structural formula of the lactam in the preparation method is: In the formula, R1 represents C3~C 12 The general structural formula of the nylon polymerization monomer diacyl chloride is: The general structural formula of the nylon polymerized monomer dibasic acid is: In the formula, R2 represents C2~C 12 The general structural formula of the nylon polymer monomer diamine is: H2N-R3-NH2, where R3 represents C4~C 14 An alkylene group or an arylene group.
5. An application of the phosphorus-containing flame-retardant copolymer nylon according to claim 1, characterized in that Its application is to use it directly alone to produce flame-retardant plastics and flame-retardant fiber materials, or to use it as a macromolecular flame retardant to be blended with other polymer materials to produce flame-retardant polymer materials.
Citation Information
Cited By
DOPO-based halogen-free intrinsic flame-retardant nylon 66 and preparation method thereof
CN117209754A
A DOPO-based halogen-free intrinsic flame-retardant nylon 66 and a preparation method thereof
CN117209754B
Phosphorus-nitrogen-silicon multi-synergistic halogen-free intrinsic flame-retardant nylon 66 and preparation method thereof
CN121181902A
Halogen-free intrinsic flame-retardant nylon 66 with phosphorus-nitrogen-silicon multi-synergism and preparation method thereof
CN121181902B