Pneumatic tires

By using a combination of multiple solution-polymerized styrene-butadiene rubbers and low-Tg hydrocarbon resins in tire rubber to replace rubber processing oil, the balance problem between wet skid resistance and rolling resistance of the tire rubber composition is solved and improved Overall tire performance and tread life.

CN115466443BActive Publication Date: 2024-10-11THE GOODYEAR TIRE & RUBBER CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210652653.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-10
Filing Date
2022-06-10
Publication Date
2024-10-11
Estimated Expiration
2042-06-10

AI Technical Summary

Technical Problem

It is difficult to find a balance between wet skid resistance and rolling resistance in existing tire rubber compositions, resulting in the improvement of one property at the expense of the other, affecting tread performance.

Method used

A rubber composition containing two solution-polymerized styrene-butadiene rubbers and a low-Tg hydrocarbon resin is used. By adjusting the component ratio and additive types, the traditional rubber processing oil is replaced, and the rubber mixing process is optimized to improve the tire's wet skid resistance. and rolling resistance balance.

Benefits of technology

It achieves improving the tire's wet skid resistance and rolling resistance performance, extending the tread life and improving the overall performance balance without compromising.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 45570DEST_PATH_IMAGE002
    Figure 45570DEST_PATH_IMAGE002
  • Figure 548413DEST_PATH_IMAGE004
    Figure 548413DEST_PATH_IMAGE004
  • Figure 732717DEST_PATH_IMAGE006
    Figure 732717DEST_PATH_IMAGE006
Patent Text Reader

Abstract

The present invention relates to a pneumatic tire formed from a tread rubber composition comprising a combination of at least two different solution-polymerized styrene-butadiene rubbers (s-SBR) each filled with oil and a low Tg traction resin. The low Tg traction resin replaces the high Tg traction resin in a conventional mixture and the rubber processing oil added during the rubber mixing process. The low Tg traction resin is a hydrocarbon resin having a Tg of about 100°C to about 30°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This exemplary embodiment relates to a rubber composition comprising a combination of at least two different solution polymerized styrene butadiene rubbers (s-SBRs), each of which is filled with oil, and a low Tg traction resin that replaces the rubber processing oil that is typically added during rubber mixing. It is particularly suitable for use in tire components and will be described with particular reference to tire components. However, it should be understood that this exemplary embodiment may also be used in other similar applications. Background Art

[0002] Tires are designed to have a combination of various properties, which, among other things, provide safe handling and fuel economy of the vehicle. It is desirable that the tire possess good wet-slip resistance (i.e., wet-weather grip), low rolling resistance, and good wear resistance (i.e., long tread life). However, these properties depend to a large extent on the dynamic viscoelastic properties of the rubber used when manufacturing the tire. For example, a rubber with high resilience is usually used in the tire to reduce rolling resistance and / or improve wear resistance, while a rubber with large energy loss is used to improve the wet-slip resistance of the tire. In order to balance the inconsistent properties of these two viscoelasticities, various types of mixtures of synthetic rubbers and natural rubbers are used in the tire tread. For example, there are various mixtures in which styrene-butadiene rubber and polybutadiene rubber are used.

[0003] However, improvement in one property often requires an acceptable compromise between that property and another. A rubber composition is desired that improves the balance between wet skid resistance and rolling resistance without compromising tread performance. Summary of the invention

[0004] One embodiment of the present invention relates to a pneumatic tire having a tread comprising a vulcanizable rubber composition. Based on 100 parts by weight of elastomer (phr), the rubber composition comprises:

[0005] (A) about 40 to about 80 phr of a first polymerized styrene butadiene rubber (s-SBR) having a bound styrene content of about 5 to about 50 weight percent, based on the weight of the rubber, a 1,2-vinyl content of about 10 to about 40 weight percent, and a Tg of about -85°C to about -20°C;

[0006] (B) about 30 to about 70 phr of a second solution polymerized styrene butadiene rubber having a bound styrene content of about 15 to about 45 wt %, a 1,2-vinyl content of about 20 to about 60 wt %, and a Tg of about -30°C to about -5°C;

[0007] (C) from about 5 to about 80 phr of a resin having a Tg of from about -100°C to about 30°C; and

[0008] (D) 0 to about 60 phr of rubber processing oil;

[0009] The total amount of resin and oil is less than 100 phr.

[0010] Another embodiment of the present invention is also directed to a pneumatic tire having a tread comprising a vulcanizable rubber composition comprising, based on 100 parts by weight of elastomer (phr):

[0011] (A) from about 40 to about 80 phr of a first polymerized styrene butadiene rubber (s-SBR) filled with less than 37.5 phr of oil;

[0012] (B) from about 30 to about 70 phr of a second solution polymerized styrene butadiene rubber filled with less than 37.5 phr of oil, the second s-SBR being different from the first s-SBR;

[0013] (C) from about 5 to about 80 phr of a low Tg hydrocarbon resin having a Tg of from about -100°C to about 300°C; and

[0014] (D) about 60 to 170 phr of silicon dioxide;

[0015] Wherein, the rubber composition does not contain additional rubber processing oil.

[0016] The present invention discloses the following technical solutions:

[0017] 1. A pneumatic tire having a tread comprising a vulcanizable rubber composition, based on 100 parts by weight of elastomer (phr), the vulcanizable rubber composition comprising:

[0018] (A) about 40 to about 80 phr of a first polymerized styrene butadiene rubber (s-SBR) having a bound styrene content of about 5 to about 50 wt %, based on the weight of the rubber, a 1,2-vinyl content of about 10 to about 40 wt %, and a Tg of about -85°C to about -20°C;

[0019] (B) about 30 to about 70 phr of a second solution polymerized styrene butadiene rubber having a bound styrene content of about 15 to about 45 wt %, a 1,2-vinyl content of about 20 to about 60 wt %, and a Tg of about -30°C to about -5°C;

[0020] (C) from about 5 to about 80 phr of a resin having a Tg of from about -100°C to about 30°C; and

[0021] (D) 0 to about 60 phr of rubber processing oil;

[0022] The total amount of resin and oil is less than 100 phr.

[0023] 2. The pneumatic tire according to technical solution 1, wherein the rubber composition further comprises about 5 to about 20 phr of polybutadiene.

[0024] 3. The pneumatic tire according to technical solution 1, wherein the resin is a hydrocarbon type resin or a modified product thereof.

[0025] 4. A pneumatic tire according to technical solution 1, wherein the resin is a renewable bio-based chemical type resin, a modified product or a mixture thereof.

[0026] 5. A pneumatic tire according to technical solution 1, wherein the oil is selected from: aromatic oil; paraffin oil, cyclopentane oil, MES, TDAE, heavy cyclopentane oil, triglyceride vegetable oil and combinations thereof.

[0027] 6. A pneumatic tire according to technical solution 5, wherein the oil is TDAE.

[0028] 7. A pneumatic tire according to technical solution 1, wherein the rubber composition does not contain a high Tg resin.

[0029] 8. The pneumatic tire according to technical solution 1, wherein the rubber composition does not contain rubber processing oil added during the mixing process.

[0030] 9. A pneumatic tire according to technical solution 1, wherein the first s-SBR is filled with less than about 37.5 phr of oil.

[0031] 10. A pneumatic tire according to technical solution 1, wherein the second s-SBR is filled with less than about 37.5 phr of oil.

[0032] 11. The pneumatic tire according to technical solution 1, wherein the rubber composition further comprises about 60 to about 170 phr of silica.

[0033] 12. A pneumatic tire according to technical solution 11, wherein the weight ratio of silica to the total amount of hydrocarbon resin and oil is greater than 2.

[0034] 13. A pneumatic tire having a tread comprising a vulcanizable rubber composition, based on 100 parts by weight of elastomer (phr), the vulcanizable rubber composition comprising:

[0035] (A) from about 40 to about 80 phr of a first polymerized styrene butadiene rubber (s-SBR) filled with less than about 37.5 phr of oil;

[0036] (B) from about 30 to about 70 phr of a second solution polymerized styrene butadiene rubber filled with less than about 37.5 phr of oil, the second s-SBR being different from the first s-SBR;

[0037] (C) from about 5 to about 80 phr of a low Tg hydrocarbon resin having a Tg of from about -100°C to about 30°C; and

[0038] (D) about 60 to 170 phr of silicon dioxide;

[0039] Wherein, the rubber composition does not contain additional rubber processing oil.

[0040] 14. A pneumatic tire according to technical solution 13, wherein the first s-SBR is characterized by having a combined styrene content of about 5 to about 50 weight percent based on the weight of the rubber, a 1,2-vinyl content of about 10 to about 40 weight percent, and a low Tg.

[0041] 15. The pneumatic tire according to technical solution 14, wherein the Tg of the first s-SBR is about -85°C to about -20°C.

[0042] 16. A pneumatic tire according to technical solution 13, wherein the second s-SBR is characterized by having a bound styrene content of about 15 to about 45 wt%, a 1,2-vinyl content of about 20 to about 60 wt%, and a Tg of about -30°C to about -5°C.

[0043] 17. A pneumatic tire according to technical solution 13, wherein the first s-SBR is filled with less than about 37.5 phr of oil.

[0044] 18. A pneumatic tire according to technical solution 13, wherein the second s-SBR is filled with less than about 37.5 phr of oil. DETAILED DESCRIPTION

[0045] The present invention relates to a pneumatic tire having a tread comprising a vulcanizable rubber composition. Based on 100 parts by weight of elastomer (phr), the rubber composition comprises:

[0046] (A) about 40 to about 80 phr of a first polymerized styrene butadiene rubber (s-SBR) having a bound styrene content of about 5 to about 50 weight percent, based on the weight of the rubber, a 1,2-vinyl content of about 10 to about 40 weight percent, and a Tg of about -85°C to about -20°C;

[0047] (B) about 30 to about 70 phr of a second solution polymerized styrene butadiene rubber having a bound styrene content of about 15 to about 45 wt %, a 1,2-vinyl content of about 20 to about 60 wt %, and a Tg of about -30°C to about -5°C;

[0048] (C) from about 5 to about 80 phr of a resin having a Tg of from about -100°C to about 30°C; and

[0049] (D) 0 to about 60 phr of rubber processing oil;

[0050] The total amount of resin and oil is less than 100 phr.

[0051] One component of the rubber composition is about 40 to about 80 phr of a first polymerized styrene butadiene rubber (s-SBR) having a bound styrene content of about 5 to about 50 wt %, based on the weight of the rubber, a 1,2-vinyl content of about 10 to about 40 wt %, and a Tg of about -85°C to about -20°C.

[0052] As the first styrene-butadiene rubber, the styrene-butadiene rubber of suitable solution polymerization can for example be made by organic lithium catalysis in the presence of an organic hydrocarbon solvent. The polyreaction adopted during the preparation of rubbery polymer is usually initiated by adding an organic lithium initiator into the organic polymerization medium containing monomer. Such polyreaction adopts continuous polymerization technology to carry out usually. In such continuous polymerization, monomer and initiator are continuously added to the organic polymerization medium, and the synthetic rubbery polymer is taken out continuously simultaneously. Such continuous polymerization is carried out usually in a multi-reactor system. Suitable polymerization methods are known in the art, for example, as described in U.S. Pat. Nos. 4,843,120; 5,137,998; 5,047,483; 5,272,220; 5,239,009; 5,061,765; 5,405,927; 5,654,384; 5,620,939; 5,627,237; 5,677,402; 6,103,842; and 6,559,240, the disclosures of which are incorporated herein by reference in their entireties.

[0053] Such solution polymerized styrene butadiene rubbers may be tin coupled or silicon coupled as known in the art.In one embodiment, suitable s-SBRs may be at least partially silicon coupled.

[0054] The second component of the rubber composition is about 30 to about 70 phr of a second solution-polymerized styrene-butadiene rubber that is different from the first s-SBR. Preferably, the second s-SBR has a bound styrene content of about 15 to about 45 wt%, a 1,2-vinyl content of about 20 to about 60 wt%, and a Tg of about -30°C to about -5°C.

[0055] As the second styrene butadiene rubber, a suitable solution polymerized styrene butadiene rubber can be made, for example, using the same method disclosed above for the first s-SBR.

[0056] As the second styrene butadiene rubber, suitable solution polymerized styrene butadiene rubber is commercially available, such as NS540 from Zeon, etc. Such solution polymerized styrene butadiene rubber can be tin coupled or silicon coupled as known in the art. In one embodiment, suitable s-SBR can be at least partially silicon coupled.

[0057] When referred to herein, reference to the glass transition temperature or Tg of an elastomer or elastomeric composition represents the glass transition temperature(s) of the corresponding elastomer or elastomeric composition in its uncured state or, in the case of an elastomeric composition, a potentially cured state. Tg may be suitably determined by differential scanning calorimetry (DSC) at a heating rate of 10°C / min as the peak midpoint, for example according to ASTM D7426 standard.

[0058] Another component of the rubber composition is about 5 to about 20 phr of cis-1,4-polybutadiene, also known as polybutadiene rubber or polybutadiene (BR). Suitable polybutadiene rubbers can be prepared, for example, by organic solution polymerization of 1,3-butadiene. Desirable features of BR can be, for example, having a cis-1,4-butadiene content of at least 90% and a glass transition temperature Tg of -95°C to -105°C. Suitable polybutadiene rubbers are commercially available, for example, from Goodyear's Budene ® 1207, etc.

[0059] The rubber composition may optionally include a rubber processing oil. The rubber composition may include 0 to about 60 phr of a rubber processing oil. Processing oil may be included in the rubber composition as an extending oil (extending oil) that is commonly used to fill elastomers. Processing oil may also be included in the rubber composition by directly adding the oil during rubber mixing. The processing oil used may include both the extending oil present in the elastomer and the processing oil added during mixing. In one embodiment, the rubber composition includes a low PCA oil. Suitable low PCA oils include, but are not limited to, mild extraction solvate (MES), treated distillation aromatic extract (TDAE), residual aromatic extract (RAE), SRAE and heavy naphthenic oils as known in the art; see, for example, U.S. Pat. Nos. 5,504,135; 6,103,808; 6,399,697; 6,410,816; 6,248,929; 6,146,520; U.S. Published Applications: 2001 / 00023307; 2002 / 0000280; 2002 / 0045697; 2001 / 0007049; EP0839891; JP2002097369; ES2122917, the disclosures of which are incorporated herein by reference.

[0060] Suitable low PCA oils include those having a polycyclic aromatic content of less than 3 wt % as determined by the IP346 method. The procedure for the IP346 method can be found in Standard Methods for Analysis & Testing of Petroleum and Related Products and British Standard 2000 Parts, 2003, 62nd edition, published by the British Petroleum Institute.

[0061] Suitable TDAE oils are available as Tudalen® SX500 from Klaus Dahleke KG, VivaTec® 400 and VivaTec® 500 from H&R Group, Enerthene® 1849 from BP, and Extensoil® 1996 from Repsol. These oils can be obtained as separate oils or together with elastomers in the form of extended elastomers.

[0062] Suitable vegetable oils include, for example, soybean oil, sunflower oil, rapeseed oil and canola oil, which are in the form of esters containing some degree of unsaturation.

[0063] Another component of the rubber composition is about 5 to about 80 phr of a resin. In one embodiment, the resin has a Tg of about -100°C to about 30°C, more preferably about -70°C to about 25°C, and most preferably about -40°C to about 20°C. In another embodiment, the resin is a hydrocarbon resin having a Tg below 30°C.

[0064] A suitable method for measuring the Tg of a resin is DSC according to ASTM D6604 or an equivalent protocol. The resin softening point is determined by ASTM E28, which is sometimes referred to as the ring and ball softening point. In one embodiment, the rubber composition may additionally comprise a hydrocarbon resin having a glass transition temperature above 20°C. Such optional hydrocarbon resins may have a softening point above 30°C.

[0065] The resin is selected from any hydrocarbon chemical type resin (AMS, coumarone-indene, C5, C9, C5 / C9, DCPD, DCPD / C9, etc.) and any modifications thereof (phenol, C9, hydrogenated, recycled monomers, etc.) and any renewable bio-based chemical type resin (e.g. any polyterpene, gum rosin, tall oil rosin, etc.) and modifications thereof (phenol, C9, hydrogenated, DCPD, esters, etc.) and mixtures thereof.

[0066] In one embodiment, the resin is a benzofuran-indene resin containing benzofuran and indene as monomer components constituting the resin backbone (main chain). In addition to benzofuran and indene, monomer components that can also be incorporated into the backbone are, for example, methylbenzofuran, styrene, α-methylstyrene, methylindene, vinyltoluene, dicyclopentadiene, cyclopentadiene and dienes (e.g., isoprene and piperlyene). Suitable benzofuran-indene resins are commercially available, such as Novares from Rutgers Novares GmbH. ® C30.

[0067] Suitable petroleum resins include aromatic and non-aromatic types. Several types of petroleum resins are available. Some resins have low unsaturation and high aromatic content, while some are highly unsaturated, and some are completely free of aromatic structure. The difference of the resins is largely due to the olefins in the raw materials derived from the resins. Conventional derivatives in such resins include any C5 species (containing olefins and dienes with an average of five carbon atoms), such as cyclopentadiene, dicyclopentadiene, dienes (such as isoprene and piperylene) and any C9 species (containing olefins and dienes with an average of 9 carbon atoms), such as vinyl toluene, alpha-methyl styrene and indene. Such resins are made by any mixture formed by the above-mentioned C5 species and C9 species.

[0068] In this article, styrene / alpha-methylstyrene resin is considered to be a relatively short-chain copolymer of styrene and alpha-methylstyrene. Styrene / alpha-methylstyrene resin can have, for example, a styrene content of about 10 to about 90%. On the one hand, such resins can be suitably prepared, for example, by cationic copolymerization of styrene and alpha-methylstyrene in a hydrocarbon solvent. Therefore, the styrene / alpha-methylstyrene resin under consideration can be characterized by, for example, its chemical structure (i.e., its styrene content and alpha-methylstyrene content) and its glass transition temperature, molecular weight and molecular weight distribution. Suitable styrene / alpha-methylstyrene resin is commercially available, such as PURE 20 AS from Rutgers Novares GmbH.

[0069] Terpene-phenol resins may be used. Terpene-phenol resins may be obtained by copolymerization of phenolic monomers with terpenes such as limonene, pinene and delta-3-carene.

[0070] In one embodiment, the resin is a resin derived from rosin and derivatives. Representatives thereof are, for example, gum rosin, wood rosin and tall oil rosin. Gum rosin, wood rosin and tall oil rosin have similar compositions, although the amounts of the components of the rosin may vary. Such resins may be dimerized, polymerized or disproportionated. Such resins may be in the form of esters of rosin acid and a polyol (e.g., pentaerythritol or ethylene glycol).

[0071] In one embodiment, the resin may be partially or fully hydrogenated.

[0072] The rubber composition comprises a combination of an optional processing oil, an optional hydrocarbon resin having a Tg above 20°C and a resin having a Tg of -100°C to 30°C in an amount of up to 80 phr.

[0073] The vulcanizable rubber composition may include from about 60 to about 170 phr of silica.

[0074] In one embodiment, the weight ratio of silica to the total amount of hydrocarbon resin and oil is greater than 2.

[0075] Commonly used siliceous pigments that can be used in rubber compounds include conventional pyrogenic siliceous pigments and precipitated siliceous pigments (silicon dioxide), but precipitated silica is preferred. Conventional siliceous pigments preferably used in the present invention are precipitated silicas, for example, those obtained by acidification of soluble silicates (e.g., sodium silicate).

[0076] Such conventional silicas may be characterized, for example, by having a BET surface area of ​​about 40 to about 600 square meters per gram, and more typically about 50 to about 300 square meters per gram, as measured using nitrogen. The BET method for measuring surface area is described in the Journal of the American Chemical Society, Vol. 60, p. 304 (1930).

[0077] Conventional silicas may also typically be characterized as having a dibutyl phthalate (DBP) absorption value of from about 100 to about 400, and more typically from about 150 to about 300.

[0078] Conventional silica may be expected to have an average final particle size of, for example, 0.01 to 0.05 microns as determined by electron microscopy, but the size of the silica particles may be even smaller or possibly larger.

[0079] Various commercially available silicas may be used, such as, by way of example only and not limitation, those commercially available from PPG Industries under the Hi-Sil trademark as types 210, 243, etc.; and under types Z1165MP, Z165GR, and Zeosil Premium ® 200 MP silica available from Rhodia; and silica available from Degussa AG as, for example, types VN2 and VN3, and the like.

[0080] The vulcanizable rubber composition may include from about 5 to about 50 phr of carbon black.

[0081] The carbon black commonly used can be used as conventional filler.Representative examples of such carbon black include N110, N121, N134, N220, N231, N234, N242, N293, N299, S315, N326, N330, M332, N339, N343, N347, N351, N358, N375, N539, N550, N582, N630, N642, N650, N683, N754, N762, N765, N774, N787, N907, N908, N990 and N991.These carbon blacks have iodine absorption of 9 to 145g / kg and 34 to 150cm 3 / 100g DPB value.

[0082] Other fillers may be used in the rubber composition, including but not limited to particulate fillers including ultra high molecular weight polyethylene (UHMWPE), particulate polymer gels, such as those disclosed in U.S. Pat. Nos. 6,242,534; 6,207,757; 6,133,364; 6,372,857; 5,395,891; or 6,127,488, and plasticized starch composite fillers, such as disclosed in U.S. Pat. No. 5,672,639, the disclosure of which is incorporated herein by reference.

[0083] It may be preferred that the rubber composition used for tire components additionally contains a conventional sulfur-containing organosilicon compound. Examples of suitable sulfur-containing organosilicon compounds have the following formula:

[0084]

[0085] Where Z is selected from:

[0086]

[0087] Among them, R 6 is an alkyl group having 1 to 4 carbon atoms, a cyclohexyl group or a phenyl group; R 7 is an alkoxy group having 1 to 8 carbon atoms, or a cycloalkoxy group having 5 to 8 carbon atoms; Alk is a divalent hydrocarbon group having 1 to 18 carbon atoms and n is an integer of 2 to 8.

[0088] Specific examples of sulfur-containing organosilicon compounds that can be used according to the present invention include: 3,3'-bis(trimethoxysilylpropyl) disulfide, 3,3'-bis(triethoxysilylpropyl) disulfide, 3,3'-bis(triethoxysilylpropyl) tetrasulfide, 3,3'-bis(triethoxysilylpropyl) octasulfide, 3,3'-bis(trimethoxysilylpropyl) tetrasulfide, 2,2'-bis(triethoxysilylethyl) tetrasulfide, 3,3'-bis(trimethoxysilylpropyl) trisulfide, 3,3'-bis(triethoxysilylpropyl) trisulfide, 3,3'-bis(tributoxysilylpropyl) disulfide, 3,3'-bis(tris(butyl)silylpropyl) 3,3'-bis(trimethoxysilylpropyl) hexasulfide, 3,3'-bis(trimethoxysilylpropyl) octasulfide, 3,3'-bis(trioctyloxysilylpropyl) tetrasulfide, 3,3'-bis(trihexyloxysilylpropyl) disulfide, 3,3'-bis(tri-2''-ethylhexyloxysilylpropyl) trisulfide, 3,3'-bis(triisooctyloxysilylpropyl) tetrasulfide, 3,3'-bis(tri-tert-butoxysilylpropyl) disulfide, 2,2'-bis(methoxydiethoxysilylethyl) tetrasulfide, 2,2'-bis(tripropoxysilylethyl) pentasulfide, 3,3'-bis(tricyclohexyloxysilylpropyl) 2,2'-bis(dimethylmethoxysilylethyl) disulfide, 2,2'-bis(dimethylmethoxysilylethyl) disulfide, 2,2'-bis(dimethylsec-butoxysilylethyl) trisulfide, 3,3'-bis(methylbutylethoxysilylpropyl) tetrasulfide, 3,3'-bis(di-tert-butylmethoxysilylpropyl) tetrasulfide, 2,2'-bis(phenylmethylmethoxysilane) 3,3'-bis(diphenylisopropoxysilylpropyl)tetrasulfide, 3,3'-bis(diphenylcyclohexyloxysilylpropyl)disulfide, 3,3'-bis(dimethylethylmercaptosilylpropyl)tetrasulfide, 2,2'-bis(methyldimethoxysilylethyl)trisulfide, 2,2'-bis(methylethoxypropoxysilylethyl)tetrasulfide, 3,3'-bis(diethylmethoxysilylpropyl)tetrasulfide, 3,3'-bis(ethyldi-sec-butoxysilylpropyl)disulfide, 3,3'-bis(propyldiethoxysilylpropyl)disulfide, 3,3'-bis(butyldimethoxysilylpropyl)trisulfide, 3,3'-Bis(phenyldimethoxysilylpropyl)tetrasulfide, 3-phenylethoxybutoxysilyl-3'-trimethoxysilylpropyl tetrasulfide, 4,4'-bis(trimethoxysilylbutyl)tetrasulfide, 6,6'-bis(triethoxysilylhexyl)tetrasulfide, 12,12'-bis(triisopropoxysilyldodecyl)disulfide, 18,18'-bis(trimethoxysilyloctadecyl)tetrasulfide, 18, 18'-Bis(tripropoxysilyloctadecenyl)tetrasulfide, 4,4'-bis(trimethoxysilyl-buten-2-yl)tetrasulfide, 4,4'-bis(trimethoxysilylcyclohexylene)tetrasulfide, 5,5'-bis(dimethoxymethylsilylpentyl)trisulfide, 3,3'-bis(trimethoxysilyl-2-methylpropyl)tetrasulfide, 3,3'-bis(dimethoxyphenylsilyl-2-methylpropyl)disulfide.

[0089] The preferred sulfur-containing organosilicon compound is 3,3'-bis(trimethoxy or triethoxysilylpropyl)sulfide. The most preferred compounds are 3,3'-bis(triethoxysilylpropyl)disulfide and 3,3'-bis(triethoxysilylpropyl)tetrasulfide. Therefore, for Formula VIII, Z is preferably:

[0090]

[0091] Where R 7 is an alkoxy group having 2 to 4 carbon atoms, wherein 2 carbon atoms are particularly preferred; alk is a divalent hydrocarbon group having 2 to 4 carbon atoms, wherein 3 carbon atoms are particularly preferred; and n is an integer of 2 to 5, wherein 2 to 4 are particularly preferred.

[0092] In another embodiment, suitable sulfur-containing organosilicon compounds include compounds disclosed in U.S. Pat. No. 6,608,125. In one embodiment, the sulfur-containing organosilicon compound includes 3-(octanoylthio)-1-propyltriethoxysilane, CH3(CH2)6C(=O)-S-CH2CH2CH2Si(OCH2CH3)3, which is commercially available, such as NXT from MomentivePerformance Materials. TM .

[0093] In another embodiment, suitable sulfur-containing organosilicon compounds include compounds disclosed in U.S. Publication No. 2006 / 0041063, the disclosure of which is incorporated herein by reference in its entirety. In one embodiment, the sulfur-containing organosilicon compound includes the reaction product of a hydrocarbon diol (e.g., 2-methyl-1,3-propanediol) and S-[3-(triethoxysilyl)propyl]thiooctanoate. In one embodiment, the sulfur-containing organosilicon compound is NXT-Z from Momentive Performance Materials. TM .

[0094] In another embodiment, suitable sulfur-containing organosilicon compounds include those disclosed in US Patent Publication No. 2003 / 0130535, which is incorporated herein by reference in its entirety. In one embodiment, the sulfur-containing organosilicon compound is Si-363 from Degussa.

[0095] The amount of sulfur-containing organosilicon compound of formula I in the rubber composition varies depending on the level of other additives used. The amount of compound of formula I is 0.5 to 20 phr. Preferably, the amount is 1 to 10 phr.

[0096] It is readily understood by those skilled in the art that the rubber composition is mixed by methods commonly known in the rubber mixing field, such as mixing various sulfur-vulcanizable component rubbers with various commonly used additive materials (e.g., sulfur donors, curing aids, such as activators and retarders and processing additives, fillers, pigments, fatty acids, zinc oxide, waxes, antioxidants and antiozonants and peptizers). As known to those skilled in the art, the above additives are selected and usually used in conventional amounts according to the intended use of the sulfur-vulcanizable material and the sulfur-vulcanized material (rubber). Representative examples of sulfur donors include elemental sulfur (free sulfur), disulfide amines, polymeric polysulfides and sulfur olefin adducts. Preferably, the sulfur-vulcanizing agent is elemental sulfur. The sulfur-vulcanizing agent can be used in an amount of 0.5 to 8 phr, preferably 1 to 6 phr. Typical amounts of antioxidants include about 1 to about 5 phr. Representative antioxidants can be, for example, diphenyl-p-phenylenediamine, for example, in The Vanderbilt Rubber Handbook (1978), those disclosed in pages 344 to 346. Typical amounts of antiozonants include about 1 to 5 phr. If used, typical amounts of fatty acids (which may include stearic acid) include about 0.5 to about 5 phr. Typical amounts of zinc oxide include about 2 to about 5 phr. Typical amounts of waxes include about 1 to about 5 phr. Microcrystalline wax is commonly used. Typical amounts of peptizers include about 0.1 to about 1 phr. Typical peptizers can be, for example, pentachlorothiophenol and dibenzamidodiphenyl disulfide.

[0097] Accelerator is used to control the time and / or temperature required for vulcanization and improve the properties of vulcanized rubber. In one embodiment, a single accelerator system, i.e., a primary accelerator, can be used. (One or more) primary accelerators can be used with a total amount of about 0.5 to about 6, preferably about 0.8 to about 3phr. In another embodiment, a combination of a primary accelerator and a secondary accelerator can be used, wherein the secondary accelerator is used with a lesser amount (such as about 0.05 to about 3phr) to activate and improve the properties of the vulcanized rubber. It can be expected that the combination of these accelerators produces a synergistic effect on the final properties, and to a certain extent, better than those effects produced by using any accelerator alone. In addition, a delayed action accelerator can be used, which is not affected by conventional processing temperatures, but produces satisfactory solidification at common vulcanization temperatures. Vulcanization retarders can also be used. Accelerators that can be used for the appropriate type of the present invention are amines, disulfides, guanidines, thioureas, thiazoles, thiurams, sulfenamides, dithiocarbamates and xanthates. Preferably, the primary accelerator is a sulfenamide. If a secondary accelerator is used, it is preferably a guanidine, dithiocarbamate or thiuram compound.

[0098] The mixing of the rubber composition can be achieved by methods known to those skilled in the art of rubber mixing. For example, the ingredients are usually mixed in at least two stages, i.e., at least one non-productive stage, followed by a productive mixing stage. The final curing machine (curative) including the sulfur-vulcanizing agent is usually mixed in the final stage conventionally referred to as the "productive" mixing stage, wherein the mixing is usually carried out at a temperature or final temperature lower than the mixing temperature of the previous (one or more) non-productive mixing stage (one or more). The terms "non-productive" and "productive" mixing stages are well known to those skilled in the art of rubber mixing. The rubber composition can be subjected to a thermomechanical mixing step. The thermomechanical mixing step generally includes machining a suitable time period in a mixer or extruder to produce a rubber temperature of 140°C to 190°C. The appropriate duration of thermomechanical processing varies with the operating conditions and the volume and properties of the components. For example, thermomechanical processing can be 1 to 20 minutes.

[0099] The rubber composition may be incorporated into the tread of a tire.

[0100] The pneumatic tire of the present invention can be a racing tire, a passenger tire, an aircraft tire, an agricultural tire, a bulldozer tire, an off-road vehicle tire, a truck tire, etc. Preferably, the tire is a passenger tire or a truck tire. The tire can also be a radial tire or a bias tire, wherein the radial tire is preferred.

[0101] The vulcanization of the pneumatic tire of the present invention is generally carried out at conventional temperatures of about 100° C. to 200° C. Preferably, the vulcanization is carried out at a temperature of about 110° C. to 180° C. Any conventional vulcanization process may be used, such as heating in a press or mold, heating with superheated steam or hot air. Such a tire may be constructed, shaped, molded and cured by various known methods and will be apparent to those skilled in the art.

[0102] The following examples are presented for the purpose of illustrating, but not limiting, the present invention. Unless specifically stated otherwise, all parts are by weight.

[0103] Example 1

[0104] In the present embodiment, the influence on the performance of the rubber mixture for the mixture in which the traction resin replaces some extender oils in the s-SBR material is illustrated. According to the formula in Table 1, the rubber component is mixed with a multi-step mixing procedure. The vulcanizing agent and curing technology of the standard amount are also used. Then the cured rubber mixture is also tested for various properties, including hysteresis (hysteresis), stress strain, tensile strength, elongation at break, wet skid resistance and rolling resistance.

[0105] A control rubber compound was prepared as Sample A using an s-SBR material with 37.5 phr of conventional extender oil.

[0106] A control rubber compound was prepared as Sample B using (i) an s-SBR material each formed using less phr of extender oil than the s-SBR in Sample A and (ii) additional rubber processing oil, with all other ingredients being the same.

[0107] For experimental rubber samples CF, the rubber compound was prepared using the same s-SBR material as control sample B, but with a resin having a different Tg replacing the rubber processing oil, with all other ingredients being the same.

[0108] The base formulations are shown in Table 2 below, expressed in parts per 100 parts by weight of elastomer (phr).

[0109] Table 1

[0110]

[0111] 1 Solution polymerized oil-extended SBR having a Tg of about -25°C, a styrene content of 34% and a vinyl content of 38%, had 37.5 phr of TDAE extender oil available as Tufdene E680 from Asahi Chemical.

[0112] 2Solution polymerized oil extended SBR having a Tg of about -25°C, a styrene content of 40% and a vinyl content of 14%, with 37.5 phr of TDAE extender oil available from Trinseo as SLR6430.

[0113] 3 High cis polybutadiene, available as Budene 1207 from The Goodyear Tire & Rubber Company.

[0114] 4 Solution polymerized oil extended SBR having a Tg of about -25°C, a styrene content of 34% and a vinyl content of 38%, with 25 phr of TDAE extender oil.

[0115] 5 Solution polymerized oil extended SBR having a Tg of about -25°C, a styrene content of 40% and a vinyl content of 14%, with 25 phr of TDAE extender oil available from Zeon as NS540.

[0116] 6 A copolymer of styrene and α-methylstyrene, Tg = +80°C, available from Cray Valley as Norsolene W120.

[0117] 7 A copolymer of styrene and alpha-methylstyrene, Tg = +39°C, available as Sylvatraxx 4401 from Arizona Chemicals.

[0118] 8 Copolymer of styrene and α-methylstyrene, Tg = -20°C, available from Rutgers as Pure AS20.

[0119] 9 Coumarone-indene resin, Tg = -10°C, was obtained from Rutgers as Novares C30.

[0120] 10 TESPD type silane coupling agent.

[0121] 11 Zeosil Z1165MP precipitated silica from Solvay has a CTAB surface area of ​​160 m 2 / g.

[0122] Various cured rubber properties of Control A and Control B and Experimental Samples CF are listed in Table 2 below.

[0123] Table 2

[0124] .

[0125] As can be seen from Table 2, the overall performance properties of Rubber Composition E and Rubber Composition F (which do not contain high Tg resin and rubber processing oil added during the rubber mixing stage) are advantageously superior to those of Control Sample A and Control Sample B.

[0126] It can further be seen that the rubber compound of Experimental Sample C (using a high Tg traction resin with a Tg of 80°C) did not improve the predicted wet traction and deteriorated the predicted rolling resistance properties.

[0127] It can further be seen that the rubber compound of Experimental Sample D (using a traction resin with a Tg of 39° C.) improves the predicted wet traction properties but compromises the predicted rolling resistance properties. Thus, the rubber compound of Experimental Sample D involves a compromise.

[0128] It can further be seen that the rubber compounds of Experimental Samples E and F (using low Tg traction resins having Tg values ​​of -20°C and -10°C, respectively) improve the properties of the tread compound related to predicted wet traction while maintaining predicted rolling resistance.

[0129] It is concluded that for tire treads formed from a rubber composition comprising a blend of at least two partially miscible s-SBRs, when a high loading of a low Tg resin is used to replace the rubber processing oil added during the rubber mixing stage, wet traction is improved and no compromise is made between wet traction and rolling resistance. An overall balance between properties is maintained.

[0130] Example 2

[0131] In the present embodiment, the influence on the rubber compound performance of the mixture in which the low Tg traction resin replaces the high Tg hydrocarbon resin and the low Tg oil is illustrated. According to the formula in Table 3, the rubber component is mixed with a multi-step mixing procedure. The vulcanizing agent and curing technology of the standard amount are also used. The cured rubber compound is then tested for various properties, including hysteresis, stress strain, tensile strength, elongation at break, wet skid resistance and rolling resistance.

[0132] A control rubber compound was prepared as Sample G using an s-SBR material (a combination of a resin comprising a high Tg resin; an oil; and silica) with 37.5 phr of a conventional extender oil.

[0133] For experimental rubber sample H, the rubber mixture was prepared using the same s-SBR material as control sample G, but with a low Tg resin having a higher total loading level instead of resin and rubber processing oil. All other ingredients were the same. The phr of the low Tg resin in experimental sample H matched the total amount of hydrocarbon resin and oil in control sample G.

[0134] The base formulations are shown in Table 3 below, expressed in parts per 100 parts by weight of elastomer (phr).

[0135] Table 3

[0136]

[0137] 1 Solution polymerized oil-extended SBR having a Tg of about -25°C, a styrene content of 34% and a vinyl content of 38%, had 37.5 phr of TDAE extender oil available as Tufdene E680 from Asahi Chemical.

[0138] 2 Solution polymerized oil extended SBR having a Tg of about -25°C, a styrene content of 40% and a vinyl content of 14%, with 37.5 phr of TDAE extender oil available from Trinseo as SLR6430.

[0139] 3 High cis polybutadiene, available as Budene 1207 from The Goodyear Tire & Rubber Company.

[0140] 4 Coumarone-indene resin, Tg = 55°C, was obtained from Rutgers as Novares C100.

[0141] 5 A copolymer of styrene and alpha-methylstyrene, Tg = +39°C, available as Sylvatraxx 4401 from Arizona Chemicals.

[0142] 6 Coumarone-indene resin, Tg = -10°C, was obtained from Rutgers as Novares C30.

[0143] 7 TESPD type silane coupling agent.

[0144] 8 Zeosil Premium precipitated silica from Solvay has a CTAB surface area of ​​200 m 2 / g.

[0145] Various cured rubber properties of Control G and Experimental Sample H are listed in Table 4 below.

[0146] Table 4

[0147] .

[0148] As can be seen from Table 4, the overall performance properties of Rubber Composition H (which contains no high Tg resin and no rubber processing oil added during the rubber mixing stage) are advantageously superior to those of Control Sample G.

[0149] Experimental Sample H is characterized by improved stiffness and hysteresis over Control Sample G. Thus, the addition of a low Tg resin to a rubber mixture in place of a high Tg resin and process oil (during rubber compounding) exhibits similar, but improved stiffness and hysteresis.

[0150] The 300% modulus value from stress-strain testing for experimental sample H is close to the 300% modulus value for control sample G. Therefore, adding low Tg resin to the rubber mix instead of high Tg resin and process oil (during rubber mixing) shows similar stress-strain.

[0151] Experimental Sample H is further characterized by a tensile strength at break of 20.5 (MPa), which is an improvement over the control Sample G (19.8 MPa). Thus, the addition of a low Tg resin to the rubber mixture in place of a high Tg resin and process oil (during rubber compounding) shows improved tensile strength.

[0152] Experimental Sample H is further characterized by an elongation at break of 558%. This is an improvement over Control Sample G (528%). Thus, the addition of a low Tg resin to the rubber mix in place of a high Tg resin and process oil (during rubber mixing) shows improved elongation.

[0153] Therefore, it can be observed that the tread wear resistance performance of the experimental sample H is similar to and / or improved over that of the control sample G.

[0154] Experimental Sample H was also characterized by a Wet Skid Index value of 7.1, which is an improvement over Control Sample G (7.3). Thus, the addition of a low Tg resin to the rubber mix in place of a high Tg resin and process oil (during rubber compounding) shows improved wet skid resistance or braking performance.

[0155] Experimental Sample H was also characterized by an improved Rolling Resistance Index value of 56.8, which was an improvement over Control Sample G (54). Thus, the addition of a low Tg resin to the rubber mixture in place of a high Tg resin and process oil (during rubber compounding) showed improved rolling resistance.

[0156] It is concluded that for tire treads formed from rubber compositions that do not contain high Tg resins and rubber processing oils added during the rubber mixing stage, the overall balance of rubber properties is improved when the rubber composition includes low Tg hydrocarbons. It is further concluded that for tire treads formed from such compositions, wet braking and rolling resistance are improved without compromising between these two properties.

[0157] One aspect of the present invention is that the disclosed tread rubber composition does not require compromises between properties.

[0158] The present invention may be varied according to the description provided herein. Although certain representative embodiments and details have been shown for the purpose of illustrating the present invention, it will be apparent to those skilled in the art that various changes and modifications may be made herein without departing from the scope of the present invention. Therefore, it should be understood that changes may be made in the specific embodiments described, but these changes will fall within the full intended scope of the present invention as defined in the appended claims.

Claims

1. A pneumatic tire having a tread comprising a vulcanizable rubber composition, the vulcanizable rubber composition comprising, based on 100 parts by weight of elastomer (phr): (A) 40 to 80 phr of a first solution polymerized styrene butadiene rubber (s-SBR) having a bound styrene content of 5 to 50 wt %, based on the weight of the rubber, a 1,2-vinyl content of 10 to 40 wt %, and a Tg of -85°C to -20°C, wherein the first s-SBR is an oil-extended s-SBR and is filled with less than 37.5 phr of oil; (B) 30 to 70 phr of a second solution polymerized styrene butadiene rubber having a bound styrene content of 15 to 45 wt %, a 1,2-vinyl content of 20 to 60 wt %, and a Tg of -30°C to -5°C, wherein the second s-SBR is an oil-extended s-SBR and is filled with less than 37.5 phr of oil; (C) 5 to 80 phr of a resin having a Tg of -100°C to 20°C; and (D) 0 to 60 phr of rubber processing oil; in, The total amount of resin and oil is less than 100 phr, The rubber composition does not contain rubber processing oil added during the mixing process. 2 . The pneumatic tire according to claim 1 , wherein the rubber composition further comprises 5 to 20 phr of polybutadiene.

3. The pneumatic tire according to claim 1, wherein the resin is a hydrocarbon type resin or a modified product thereof.

4. The pneumatic tire according to claim 1, wherein the resin is a renewable bio-based chemical type resin, a modification or a mixture thereof.

5. The pneumatic tire of claim 1, wherein the oil is selected from the group consisting of aromatic oil, paraffinic oil, naphthenic oil, MES, TDAE, triglyceride vegetable oil, and combinations thereof.

6. The pneumatic tire of claim 5, wherein the oil is TDAE. 7 . The pneumatic tire according to claim 1 , wherein the rubber composition further comprises 60 to 170 phr of silica.

8. The pneumatic tire according to claim 7, wherein the weight ratio of silica to the total amount of the resin and the oil is greater than 2.