A composite coated sodium ion positive electrode material precursor and preparation method thereof

By coating the sodium-ion battery cathode material with alkali solution and copper-cobalt solution co-current, the stability and performance problems of the layered transition metal oxide are solved, a dense and uniform coating layer is achieved, and the improvement Improve the cycle stability and rate performance of the battery.

CN115472807BActive Publication Date: 2024-10-29HENAN KELONG NEW ENERGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211326081.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-10-29
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

Layered structure transition metal oxides in sodium-ion batteries have problems such as unstable air storage, unstable crystal structure in the electrolyte, and insufficient cycle performance and rate performance, resulting in serious capacity fading, and the existing copper coating method is difficult to operate. , the effect is not good.

Method used

Co-flow of alkali solution and copper-cobalt solution is used to coat the precursor suspension, and the reaction conditions are controlled to form a dense and uniform coating layer, including adjusting the pH value, temperature and rotation speed in the reactor, and using surface activity agents and complexing agents to improve dispersion and deposition uniformity.

Benefits of technology

It achieves a dense distribution of the coating layer and is not easy to fall off, improves the air stability and cycle stability of the material, reduces the internal resistance of the battery, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115472807B_ABST
    Figure CN115472807B_ABST
Patent Text Reader

Abstract

The invention discloses a composite coated sodium ion positive electrode material precursor and a preparation method thereof. First, a nickel-manganese-iron-zinc mixed solution, a complexing agent, and a precipitant are added to a reactor in parallel, and a precursor matrix with uniform element distribution is obtained by a wet coprecipitation method; then pure water, a precursor matrix, a surfactant, and a complexing agent are added sequentially to the reactor to prepare a precursor matrix suspension; then an alkaline solution and a copper-cobalt solution are added to the precursor suspension in parallel, and finally the precursor is obtained through aging and drying and other processes, wherein copper exists in the form of copper oxide in the coating layer, cobalt exists in the form of trivalent cobalt, and sodium ions are controlled at 0-0.2%. The precursor coating layer prepared by the method has a dense structure, uniform distribution, is not easy to fall off, and has good product consistency, thereby effectively reducing the side reaction at the interface between the electrode material and the electrolyte at high voltage, thereby forming a more stable interface, reducing the internal resistance of the battery, and improving the battery cycle stability and rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion battery positive electrode material precursors, and in particular relates to a composite coated sodium ion positive electrode material precursor and a preparation method thereof. Background Art

[0002] Sodium-ion batteries have become a hot topic in battery technology research in recent years due to their abundant raw materials, low cost, and high safety. Potential applications include low-speed electric vehicles and energy storage devices. Positive electrode materials are one of the key materials for sodium-ion batteries. Among them, layered transition metal oxides have a high specific capacity and are compatible with lithium-ion battery positive electrode materials in terms of synthesis, battery manufacturing, and production equipment. They are one of the materials that are expected to be commercially produced in sodium-ion battery positive electrode materials.

[0003] Layered transition metal oxides have the disadvantages of poor storage stability in air and unstable crystal structure in charged electrolyte. The capacity decays seriously during long cycles and high current charge and discharge, that is, the cycle performance and rate performance cannot fully meet the application requirements. In view of the above problems, surface coating of layered transition metal oxides is one of the most effective modification methods: coating with an isolation layer to prevent direct contact between the electrolyte and the material, such as metal oxide and fluoride coating and carbon coating, effectively preventing the positive electrode material from reacting with the electrolyte without losing the material specific capacity, thereby improving the structural stability of the positive electrode material. The coated positive electrode material also increases the air storage stability, making the material more convenient in storage, transportation, processing and use, and the product quality is more consistent and stable.

[0004] When studying 3d transition metals suitable for developing low-cost systems with good overall performance, it was found that except for Ni, Co, Fe, and Mn, Ti's working potential is too low and is often used as anode materials. V is expensive and sintered in air to become a toxic pentavalent compound. Cr has a low cost but sintered in air to become a toxic hexavalent compound. Initially, Cu had no electrochemical activity in lithium- or sodium-containing layered oxides. Researchers often explored Cu in sodium-ion batteries superficially, so the electrochemical activity of Cu in sodium-containing layered oxides was discovered relatively late. As the research deepened, low-cost and basically non-toxic Cu gradually showed its advantages.

[0005] For lithium-ion batteries, the Cu element has no electrochemical properties in the lithium-ion oxide layer and cannot be used as a major element. In sodium-ion batteries, adding an appropriate amount of copper can provide charge compensation, improve the air stability, cycle stability, and rate performance of the material, and significantly improve the specific capacitance of the sodium-ion battery, thereby improving the overall performance of the material. The addition of copper in most sodium-ion batteries is achieved through co-deposition, and the co-deposition of copper elements often leads to low tap density of the precursor and low battery capacity. Therefore, copper coating has gradually entered the field of vision of researchers. Coating is mostly carried out in the sintering stage, which often requires multiple sinterings, and the coating is uneven and cannot completely cover the surface of the substrate. When coating on the surface of the precursor by co-precipitation, the amount added is often very limited, and the operation is difficult, resulting in poor coating effect. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention adopts a method of adding an alkaline solution and a copper-cobalt solution into a precursor suspension in parallel, so that the obtained precursor coating layer has a dense structure, is evenly distributed, is not easy to fall off, and has good product consistency.

[0007] The present invention provides a method for preparing a composite coated sodium ion positive electrode material precursor, comprising the following steps:

[0008] Step 1: prepare a reaction bottom solution in a reactor with one or more of pure water, ammonia solution, and a precipitant solution, the pH value of which is 7.0-13.4, maintain the reactor speed at 300-1000r / min, and the reaction temperature at 30-80°C, then flow the precipitant solution, ammonia solution, and a mixed salt solution containing nickel, manganese, iron, and zinc into the reactor in parallel, control the reaction pH to 8.0-13.5, and react for 20-300h, then centrifuge the obtained reaction mass to dry, and use 0.1-1mol / L of precipitant solution for elution, the precipitant solution temperature is 25 ℃-80 ℃, the weight ratio of the reaction material to the precipitant solution is 1:1.5-1:6, and then washed with pure water, the pure water temperature is 25 ℃-60 ℃, and the weight ratio of the reaction material to the pure water is 1:10-1:30; then the reaction material is transferred to a 100 ℃-200 ℃ oven for drying, and dried to a moisture content of <3500ppm, cooled to room temperature, and the dried and cooled reaction material is sieved with an ultrasonic vibration screen to obtain a precursor matrix;

[0009] Step 2: add pure water, precursor matrix, surfactant and complexing agent into the reaction kettle in sequence to prepare the precursor matrix suspension, and keep the speed of the reaction kettle at 300-1000r / min and the temperature at 30°C-70°C;

[0010] Step 3, a mixed salt solution containing copper and cobalt and an alkaline solution are simultaneously introduced into the above-mentioned reactor, the inflow rate of the mixed salt solution containing copper and cobalt is 10-300 mL / min, and the reaction pH is controlled to be 6.0-12.0;

[0011] Step 4: After the amount of the mixed salt solution containing copper and cobalt reaches the required coating amount, the addition of the alkaline solution is stopped, the pH is continued to be 12-14, the reaction vessel is aged for 3-24 hours, and the materials are dried;

[0012] Step 5: The dried material is transferred to a 150-200°C oven and dried for 5-10 hours, cooled, washed in 20-80°C pure water until the pH is 11-12, dried again at 100-200°C, and then sieved with an ultrasonic vibration screen to obtain the composite coated sodium ion positive electrode material precursor.

[0013] Further, in step one, the content of the precipitant solution is 0.8-8 mol / L, the content of the ammonia solution is 0.9-10 mol / L, the content of the mixed salt solution containing nickel, manganese, iron and zinc is 1.0-3.0 mol / L, the precipitant solution is one or more of sodium carbonate, sodium bicarbonate, ammonium bicarbonate, urea, sodium hydroxide and potassium hydroxide, the mixed salt solution containing nickel, manganese, iron and zinc is one or more of sulfate, chloride and nitrate, and the flow rate of the mixed salt solution containing nickel, manganese, iron and zinc is 50-300 mL / min.

[0014] Further, in step 2, the surfactant is one or more of hexadecyltrimethylammonium chloride, ethanol, hexadecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyvinyl pyrrolidone, polyethylene glycol, n-butanol, fatty acid polyoxyethylene ester, palmityl alcohol, and polyoxyethylene alkylamine, and the added amount of the surfactant is 0.5 g / L-3.5 g / L.

[0015] Further, in step 2, the complexing agent is one or more of sodium citrate, sodium fluoride, hydroxyethylethylenediaminetriacetic acid, sodium gluconate, ethylenediaminetetraacetic acid and its sodium salt, ammonia water, ethylenediaminetetrapropionic acid, and tetrahydroxypropylethylenediamine, and the added amount of the complexing agent is 5-100 g / L.

[0016] Furthermore, in step 2, the solid content of the precursor matrix suspension is 100-900 g / L.

[0017] Further, in step three, the copper source in the mixed salt solution containing copper and cobalt comes from one or more of copper sulfate, copper chloride, and copper nitrate, and the cobalt source comes from one or more of cobalt sulfate, cobalt chloride, and cobalt nitrate, and the concentration of the mixed salt solution containing copper and cobalt is 1.0-2.5 mol / L.

[0018] Furthermore, in step three, the alkaline solution is one or more of sodium hydroxide and potassium hydroxide, and the concentration of the alkaline solution is 0.8-8 mol / L.

[0019] Furthermore, in step three, the cobalt content in the mixed salt solution containing copper and cobalt is 1000-3000 ppm, and the molar ratio of copper in the mixed salt solution containing copper and cobalt to the total metal elements in the precursor matrix is ​​0.01-0.25:1.

[0020] The present invention also provides a composite coated sodium ion positive electrode material precursor prepared by the above method.

[0021] Beneficial effects: (1) The copper-cobalt composite coated sodium ion positive electrode material precursor prepared by the method provided by the present invention has a tap density increased by 0.1-0.4 g / cm compared with that before coating. 3 The specific surface area is increased by 0.3-0.6m 2 / g, the coating layer has a dense structure, uniform distribution, is not easy to fall off, has good product consistency, effectively reduces the side reaction at the interface between the electrode material and the electrolyte at high voltage, thereby forming a more stable interface, reducing the internal resistance of the battery, and improving the battery cycle stability and rate performance. This method has a wide range of applications and can achieve the coating of precursors of different types and compositions and the coating of precursor materials by different elements. The matrix is ​​not limited to nickel carbonate manganese iron zinc precursors, and the coating elements are not limited to copper cobalt coating.

[0022] (2) The present invention prepares a copper-cobalt composite coated sodium ion battery positive electrode material precursor by adding an alkaline solution and a copper-cobalt solution to a precursor suspension in parallel, which has a dense coating layer structure, is evenly distributed, is not easy to fall off, and has good product consistency. In the coating layer, copper exists in the form of copper oxide, cobalt exists in the form of trivalent cobalt, and sodium ions are controlled at 0-0.2%.

[0023] (3) Add surfactants to improve the dispersibility of the precursor suspension and the uniformity of copper-cobalt deposition coating, reduce the difficulty of copper deposition coating, and make the coating layer closely combined with the precursor and not easy to fall off. Add complexing agents to regulate the deposition rate of copper and cobalt elements and prevent element segregation. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the SEM image of the precursor matrix in Example 1.

[0025] Figure 2 This is the SEM image of the copper-cobalt coated precursor in Example 1.

[0026] Figure 3 This is a cross-sectional SEM image of the copper-cobalt coated precursor in Example 1.

[0027] Figure 4 This is the SEM-Mapping image of the copper-cobalt coated precursor in Example 1.

[0028] Figure 5 This is the SEM image of the copper-cobalt coated precursor in Comparative Example 1.

[0029] Figure 6 This is the SEM image of the copper-cobalt co-deposition doped precursor in Comparative Example 2. DETAILED DESCRIPTION

[0030] The present invention is described in detail below with reference to the embodiments.

[0031] Example 1

[0032] Step 1: In a reactor, pure water, 5 mol / L ammonia solution, and 8 mol / L sodium hydroxide solution are used to prepare a reaction base solution with a sodium hydroxide content of 5.0 g / L and an ammonia solution of 2.0 g / L, a pH value of 12.5-12.6, a reactor speed of 800 r / min, and a reaction temperature of 70 o C, 3 mol / L sodium carbonate solution, 5 mol / L ammonia solution, 2.0 mol / L nickel sulfate, manganese sulfate, ferrous sulfate, zinc sulfate mixed solution flow into the reactor, the liquid inlet rate is 100 mL / min, the reaction pH is controlled at 10.0-11.0, the reaction time is 80 h, the reaction materials enter the centrifuge to dry, and are eluted with 0.5 mol / L alkaline solution, the temperature of the alkaline solution is 80 o C, the weight ratio of the reaction material to the alkaline solution is 1:3, and then washed with pure water at a temperature of 25 o C, the weight ratio of the reaction mass to pure water was 1:20. The reaction mass after centrifugation was transferred to 150 o C oven to dry until the moisture is less than 3500ppm, and then cooled to room temperature. The dried and cooled reaction material is sieved with an ultrasonic vibration sieve to obtain a reaction product with the chemical formula Ni 0.2 Mn 0.4 Fe 0.35 Zn 0.05 CO3 precursor matrix.

[0033] Step 2: add 6L pure water, 5kg precursor matrix, 1.0g / L sodium dodecyl sulfate, and 20g / L ethylenediaminetetrapropionic acid into the reactor in sequence, the reaction temperature is 70°C, and the reactor speed is 700r / min.

[0034] Step 3, 2.0 mol / L copper sulfate, cobalt sulfate mixed solution and 8 mol / L sodium hydroxide flow into the above-mentioned reaction kettle in parallel, the copper sulfate, cobalt sulfate mixed solution inflow rate is 100 mL / min, and the reaction pH is 11.0-12.0.

[0035] Step 4: After the amount of copper sulfate and cobalt sulfate mixed solution reaches the required coating amount, the copper metering pump stops feeding, and the alkali metering pump continues to feed the solution to make the pH reach between 13 and 13.5, and the mixture is aged for 10 hours, and the materials in the reactor are dried.

[0036] Step 5: Transfer the dried material to 200 o C oven for 5 hours, cooled, washed in 25°C pure water to pH 11.0-11.5, dried again at 200°C, and then sieved with a 325-mesh ultrasonic vibration screen to obtain a copper-cobalt composite coated sodium ion battery positive electrode material precursor with a uniform coating layer, wherein copper exists in the form of copper oxide, cobalt exists in the form of trivalent cobalt, the molar ratio of copper to matrix metal elements nickel, manganese, iron and zinc is 0.1, the cobalt content is 1000ppm, and the sodium ion content is 0.1%.

[0037] Comparative Example 1

[0038] Step 1: In a reactor, pure water, 5 mol / L ammonia solution, and 8 mol / L sodium hydroxide solution are used to prepare a reaction base solution with a sodium hydroxide content of 5.0 g / L and an ammonia solution of 2.0 g / L, a pH value of 12.5-12.6, a reactor speed of 800 r / min, and a reaction temperature of 70 o C, 3 mol / L sodium carbonate solution, 5 mol / L ammonia solution, 2.0 mol / L nickel sulfate, manganese sulfate, ferrous sulfate, zinc sulfate mixed solution flow into the reactor, the liquid inlet rate is 100 mL / min, the reaction pH is controlled at 10.0-11.0, the reaction time is 80 h, the reaction materials enter the centrifuge to dry, and are eluted with 0.5 mol / L alkaline solution, the temperature of the alkaline solution is 80 o C, the weight ratio of the reaction material to the alkaline solution is 1:3, and then washed with pure water at a temperature of 25 o C, the weight ratio of the reaction mass to pure water was 1:20. The reaction mass after centrifugation was transferred to 150 o C oven to dry until the moisture is less than 3500ppm, and then cooled to room temperature. The dried and cooled reaction material is sieved with an ultrasonic vibration sieve to obtain a reaction product with the chemical formula Ni 0.2 Mn 0.4 Fe 0.35 Zn 0.05 CO3 precursor matrix.

[0039] Step 2: Add 6L of pure water and 5kg of precursor matrix into the reactor in sequence, with a reaction temperature of 70°C and a reactor speed of 700r / min.

[0040] Step 3, 2.0 mol / L copper sulfate, cobalt sulfate mixed solution and 8 mol / L sodium hydroxide flow into the reaction kettle in parallel, the copper sulfate, cobalt sulfate mixed solution inflow rate is 100 mL / min, and the reaction pH is 11.0-12.0.

[0041] Step 4: After the amount of copper-cobalt solution reaches the required coating amount, the copper metering pump stops feeding, and the alkali metering pump continues to feed the solution to make the pH reach between 13 and 13.5. After aging for 10 hours, the materials in the reactor are dried.

[0042] Step 5: Transfer the dried material to 200 o C oven for 5h, cooled, washed in 25°C pure water to pH 11.0-11.5, dried again at 200°C, and then sieved with a 325-mesh ultrasonic vibration screen, but failed to obtain a copper-cobalt-coated sodium ion battery positive electrode material precursor with a uniform coating layer.

[0043] Comparative Example 2

[0044] In a reactor, pure water, 5 mol / L ammonia solution, and 8 mol / L sodium hydroxide solution were used to prepare a reaction base solution with a sodium hydroxide content of 5.0 g / L and an ammonia solution of 2.0 g / L. The pH value was 12.5-12.6. The reactor speed was 800 r / min and the reaction temperature was 70 o C, 3 mol / L sodium carbonate solution, 5 mol / L ammonia solution, 2.0 mol / L nickel sulfate, manganese sulfate, cobalt sulfate, copper sulfate mixed solution flow into the reactor, the liquid inlet rate is 100 mL / min, the reaction pH is controlled at 10.0-11.0, the reaction time is 80 h, the reaction materials enter the centrifuge to dry, and are eluted with 0.5 mol / L alkaline solution, the temperature of the alkaline solution is 80 o C, the weight ratio of the reaction material to the alkaline solution is 1:3, and then washed with pure water at a temperature of 25 o C, the weight ratio of the reaction mass to pure water was 1:20. The reaction mass after centrifugation was transferred to 150 o C oven to dry until the moisture is less than 3500ppm, and then cooled to room temperature. The dried and cooled reaction material is sieved with an ultrasonic vibration sieve to obtain a reaction product with the chemical formula Ni 0.2 Mn 0.4 Cu 0.35 Co 0.05 Precursor of CO3, with low tap density of 0.76g / cm 3 , the structural stability is poor and the morphology is not easy to maintain.

Claims

1. A method for preparing a composite coated sodium ion positive electrode material precursor, characterized in that: The following steps are involved: Step 1: prepare a reaction bottom solution in a reactor with one or more of pure water, ammonia solution, and a precipitant solution, the pH value of which is 7.0-13.4, maintain the reactor speed at 300-1000r / min, and the reaction temperature at 30-80°C, then flow the precipitant solution, ammonia solution, and a mixed salt solution containing nickel, manganese, iron, and zinc into the reactor in parallel, control the reaction pH to 8.0-13.5, and react for 20-300h, then centrifuge the obtained reaction mass to dry, and use 0.1-1mol / L of precipitant solution for elution, the precipitant solution temperature is 25 ℃-80 ℃, the weight ratio of the reaction material to the precipitant solution is 1:1.5-1:6, and then washed with pure water, the pure water temperature is 25 ℃-60 ℃, and the weight ratio of the reaction material to the pure water is 1:10-1:30; then the reaction material is transferred to a 100 ℃-200 ℃ oven for drying, and dried to a moisture content of <3500ppm, cooled to room temperature, and the dried and cooled reaction material is sieved with an ultrasonic vibration screen to obtain a precursor matrix; Step 2: add pure water, precursor matrix, surfactant and complexing agent into the reaction kettle in sequence to prepare the precursor matrix suspension, and keep the speed of the reaction kettle at 300-1000r / min and the temperature at 30°C-70°C; Step 3, a mixed salt solution containing copper and cobalt and an alkaline solution are simultaneously introduced into the above-mentioned reactor, the inflow rate of the mixed salt solution containing copper and cobalt is 10-300 mL / min, and the reaction pH is controlled to be 6.0-12.0; Step 4: After the amount of the mixed salt solution containing copper and cobalt reaches the required coating amount, the addition of the alkaline solution is stopped, the pH is continued to be 12-14, the reaction vessel is aged for 3-24 hours, and the materials are dried; Step 5: The dried material is transferred to a 150-200°C oven and dried for 5-10 hours, cooled, washed in 20-80°C pure water until the pH is 11-12, dried again at 100-200°C, and then sieved with an ultrasonic vibration screen to obtain the composite coated sodium ion positive electrode material precursor.

2. The method for preparing a composite coated sodium ion positive electrode material precursor according to claim 1, characterized in that: In step one, the content of the precipitant solution is 0.8-8 mol / L, the content of the ammonia solution is 0.9-10 mol / L, the content of the mixed salt solution containing nickel, manganese, iron and zinc is 1.0-3.0 mol / L, the precipitant solution is one or more of sodium carbonate, sodium bicarbonate, ammonium bicarbonate, urea, sodium hydroxide and potassium hydroxide, the mixed salt solution containing nickel, manganese, iron and zinc is one or more of sulfate, chloride and nitrate, and the flow rate of the mixed salt solution containing nickel, manganese, iron and zinc is 50-300 mL / min.

3. The method for preparing a composite coated sodium ion positive electrode material precursor according to claim 1, characterized in that: In step 2, the surfactant is one or more of hexadecyltrimethylammonium chloride, ethanol, hexadecyltrimethylammonium bromide, dodecyltrimethylammonium chloride, sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, polyvinyl pyrrolidone, polyethylene glycol, n-butanol, fatty acid polyoxyethylene ester, palmityl alcohol, and polyoxyethylene alkylamine, and the added amount of the surfactant is 0.5g / L-3.5g / L.

4. The method for preparing a composite coated sodium ion positive electrode material precursor according to claim 1, characterized in that: In step 2, the complexing agent is one or more of sodium citrate, sodium fluoride, hydroxyethylethylenediaminetriacetic acid, sodium gluconate, ethylenediaminetetraacetic acid and its sodium salt, ammonia water, ethylenediaminetetrapropionic acid, and tetrahydroxypropylethylenediamine, and the added amount of the complexing agent is 5-100 g / L.

5. The method for preparing a composite coated sodium ion positive electrode material precursor according to claim 1, characterized in that: In step 2, the solid content of the precursor matrix suspension is 100-900 g / L.

6. The method for preparing a composite coated sodium ion positive electrode material precursor according to claim 1, characterized in that: In step three, the copper source in the mixed salt solution containing copper and cobalt comes from one or more of copper sulfate, copper chloride, and copper nitrate, and the cobalt source comes from one or more of cobalt sulfate, cobalt chloride, and cobalt nitrate. The concentration of the mixed salt solution containing copper and cobalt is 1.0-2.5 mol / L.

7. The method for preparing a composite coated sodium ion positive electrode material precursor according to claim 1, characterized in that: In step 3, the alkaline solution is one or more of sodium hydroxide and potassium hydroxide, and the concentration of the alkaline solution is 0.8-8 mol / L.

8. The method for preparing a composite coated sodium ion positive electrode material precursor according to claim 1, characterized in that: In step three, the cobalt content in the mixed salt solution containing copper and cobalt is 1000-3000 ppm, and the molar ratio of copper in the mixed salt solution containing copper and cobalt to the total metal elements in the precursor matrix is ​​0.01-0.25:

1.

9. A composite coated sodium ion positive electrode material precursor, characterized in that: The method is prepared by any one of the preparation methods described in claims 1 to 8.

Citation Information

Patent Citations

  • Modified NCM precursor material and preparation method therefor

    CN106328922A

  • Preparation method of composite Ni-Co-Mn precursor material obtained by doping and coating

    CN110589902A