Ethylene-vinyl alcohol copolymer resin particle composition, ethylene-vinyl alcohol copolymer film formed therefrom, and multilayer structure

By optimizing the solid volume and melting point of the surface peak part in the EVOH resin particles, combining ethylene content and shape, forming an EVOH resin particle composition, and designing a multi-layer structure, the problem of insufficient processing performance and mechanical properties of EVOH films in the prior art is solved. , achieving excellent processing performance and mechanical properties.

CN115477803BActive Publication Date: 2024-11-12CHANG CHUN PETROCHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210691641.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-16
Filing Date
2022-06-16
Publication Date
2024-11-12
Estimated Expiration
2042-06-16

AI Technical Summary

Technical Problem

The prior art is difficult to meet the multiple requirements for ethylene-vinyl alcohol copolymer (EVOH) films in both processing properties and mechanical properties, especially in terms of surface gel particles formation and elongation.

Method used

By using the first and second EVOH resin particles, respectively having a specific surface peak solid volume (Vmp) range and melting point, combined with a specific ethylene content and shape, the EVOH resin particle composition is formed and designed by a multi-layer structure, including Polymer layer and adhesive layer optimize the processing properties and mechanical properties of the film.

Benefits of technology

The good processing properties and mechanical properties of EVOH films are achieved, including reducing gel particle formation and improving elongation, meeting multiple requirements for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115477803B_ABST
    Figure CN115477803B_ABST
Patent Text Reader

Abstract

The present invention relates to an ethylene-vinyl alcohol copolymer (EVOH) resin particle composition, an ethylene-vinyl alcohol copolymer film formed therefrom, and a multilayer structure comprising the same. The EVOH resin particle composition comprises a first EVOH resin particle having a surface peak portion solid volume (Vmp) of 0.00001 to 6 μm. 3 / um 2 ; and a second EVOH resin particle having a surface peak volume (Vmp) of 0.00015 to 20 μm 3 / um 2 The present invention can improve the processing performance and mechanical properties of the EVOH composition when it is made into a film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an ethylene-vinyl alcohol (EVOH) copolymer composition; in particular, to an ethylene-vinyl alcohol copolymer resin particle composition, a film and a multilayer structure formed from the EVOH resin particle composition. Background Art

[0002] EVOH resin is widely used in multilayer bodies for preserving perishable items. For example, EVOH resin and multilayer bodies made therefrom are often used in the food packaging industry, medical equipment and consumables industry, pharmaceutical industry, electronics industry and agricultural chemical industry. Specifically, EVOH resin is often used in the form of a film; for example, it can be used to be added to a multilayer body as a unique layer to serve as an oxygen barrier layer.

[0003] In practice, the industry usually has requirements for the processing performance, mechanical properties, heat resistance, etc. of the above-mentioned films made of EVOH materials. For example, when the EVOH film is formed, if it does not form a large number of gel particles (also called fish eyes) on the surface, it can be said that it has excellent processing performance; and when the EVOH film has a good elongation when stretched under a specific tensile force, it can be said that it has ideal mechanical properties. Summary of the invention

[0004] However, the prior art has never proposed a concept or means that can effectively meet the above requirements. In response to this technical problem, the inventors have found through research that when the two EVOH resin particles contained in the EVOH resin particle composition each have a specific surface peak portion solid volume (Vmp) value range, the film formed by the EVOH resin particle composition can have good processing performance and mechanical properties.

[0005] Accordingly, the present invention provides an ethylene vinyl alcohol copolymer (EVOH) resin particle composition, which includes: a first EVOH resin particle having a surface peak volume (Vmp) of 0.00001 to 6 μm. 3 / um 2 , and a second EVOH resin particle having a surface peak volume (Vmp) of 0.00015 to 20 μm 3 / um 2 .

[0006] According to some embodiments of the present invention, the Vmp of the second EVOH resin particles is greater than the Vmp of the first EVOH resin particles.

[0007] According to some embodiments of the present invention, the melting point of the first EVOH resin particles is 135-179°C, and the melting point of the second EVOH resin particles is 180-198°C.

[0008] According to some embodiments of the present invention, the ethylene content of the first EVOH resin particles is 36 to 50 mol percent.

[0009] According to some embodiments of the present invention, the ethylene content of the second EVOH resin particles is 20 to 35 mol percent.

[0010] According to some embodiments of the present invention, the EVOH resin particles are shaped like cylinders, elliptical cylinders, angular cylinders, spheres, ellipsoids or go-shaped, and have a major diameter / height of 1-5 mm and a minor diameter of 1-5 mm.

[0011] According to some embodiments of the present invention, the weight percentage of the first EVOH resin particles to the second EVOH resin particles is 5:95 to 75:25.

[0012] According to some embodiments of the present invention, the EVOH resin particle composition has a boron content of 5 to 550 ppm.

[0013] According to some embodiments of the present invention, the EVOH resin particle composition has an alkali metal content of 10 to 550 ppm.

[0014] According to some embodiments of the present invention, the first EVOH resin particle has a kurtosis (Sku) surface parameter of 0.0020-25; and the second EVOH resin particle has a kurtosis (Sku) surface parameter of 0.0070-111.

[0015] According to some embodiments of the present invention, the first EVOH resin particle has a surface parameter of a maximum peak height (Sp) of 0.0005-29 um; and the second EVOH resin particle has a surface parameter of a maximum peak height (Sp) of 0.0020-63 um.

[0016] According to some embodiments of the present invention, the first EVOH resin particle has a protruding peak height (Spk) surface parameter of 0.001-2 um; and the second EVOH resin particle has a protruding peak height (Spk) surface parameter of 0.003-22 um.

[0017] According to some embodiments of the present invention, the first EVOH resin particle has a surface parameter of a peak height (Sxp) of 0.001-12 um; and the second EVOH resin particle has a surface parameter of a peak height (Sxp) of 0.002-48 um.

[0018] According to some embodiments of the present invention, the first EVOH resin particle has a surface parameter of a linear arithmetic mean height (Ra) of 0.001 to 0.990 um; and the second EVOH resin particle has a surface parameter of a linear arithmetic mean height (Ra) of 0.001 to 0.990 um.

[0019] According to some embodiments of the present invention, the first EVOH resin particle has a line maximum height (Rz) surface parameter of 0.001 to 9.900 um; and the second EVOH resin particle has a line maximum height (Rz) surface parameter of 0.001 to 9.900 um.

[0020] Another aspect of the present invention provides an ethylene-vinyl alcohol copolymer film, which is formed from the above-mentioned EVOH resin particle composition.

[0021] In another aspect, the present invention provides a multilayer structure comprising: (a) at least one ethylene-vinyl alcohol copolymer film formed from the EVOH resin particle composition; (b) at least one polymer layer; and (c) at least one adhesive layer.

[0022] According to some embodiments of the present invention, the polymer layer is selected from the group consisting of a low-density polyethylene layer, a polyethylene grafted maleic anhydride layer, a polypropylene layer, and a nylon layer, and the adhesive layer is a tie layer.

[0023] According to some embodiments of the present invention, the multi-layer structure is polymer layer / adhesive layer / ethylene-vinyl alcohol copolymer film / adhesive layer / polymer layer.

[0024] The present invention provides an ethylene vinyl alcohol copolymer (EVOH) resin particle composition, an ethylene vinyl alcohol copolymer film formed therefrom, and a multilayer structure comprising the film. Without being limited by a particular theory, the film formed from the EVOH resin particle composition can have good processing performance and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Embodiments of the present invention will now be described by way of example only with reference to the accompanying drawings, in which:

[0026] Figure 1 Schematic diagram illustrating the solid volume of the surface wave peak portion used according to the present invention.

[0027] It should be understood that aspects of the present invention are not limited to the configurations, instrumentalities, and characteristics shown in the drawings. DETAILED DESCRIPTION

[0028] One aspect of the present invention relates to an ethylene vinyl alcohol copolymer (EVOH) resin particle composition, which comprises: a first EVOH resin particle having a surface peak portion entity volume (Vmp) of 0.00001-6 μm 3 / um 2 , and a second EVOH resin particle having a surface peak volume (Vmp) of 0.00015 to 20 μm 3 / um 2 .

[0029] As used herein, the so-called surface peak volume (Vmp) refers to the volume of the load area ratio p%, and its specific definition can be referred to ISO 25178. In addition, the size of the core part, the protruding peak part, and the protruding trough part can also be quantified by volume parameters. Figure 1 As shown in the figure, Vmp represents the volume of the protruding peak part, Vmc represents the volume of the core part, Vvc represents the volume of the core space, and Vvv represents the load area ratio of the protruding trough part. Figure 1 The example preset specifies that 10% to 80% is the interval of the core part. The Vmp of the first EVOH resin particle is 0.00001 to 6 um 3 / um 2 , for example: 0.00001, 0.00005, 0.00100, 0.00200, 0.00500, 0.01000, 0.05000, 0.10000, 0.50000, 1, 2, 3, 4, 5, or 6um 3 / um 2 The Vmp of the second EVOH resin particles is 0.00015-20 um 3 / um 2 , for example: 0.00015, 0.00050, 0.01000, 0.05000, 0.10000, 0.50000, 1, 5, 10, 15 or 20um 3 / um 2 According to a preferred embodiment of the present invention, the Vmp of the second EVOH resin particles is greater than the Vmp of the first EVOH resin particles.

[0030] According to some embodiments of the present invention, the melting point of the first EVOH resin particles is 135-179° C., for example, 135, 140, 145, 150, 155, 160, 165, 170, 175 or 179° C. On the other hand, the melting point of the second EVOH resin particles is 180-198° C., for example, 180, 182, 184, 186, 188, 190, 192, 194, 196 or 198° C.

[0031] According to some embodiments of the present invention, the ethylene content of the first EVOH resin particles may be about 36-50 mole percent (mole%), for example, 36, 38, 40, 42, 44, 46, 48 or 50 mole%. On the other hand, the ethylene content of the second EVOH resin particles is 20-35 mole%, for example, 20, 21, 23, 25, 27, 29, 31, 33 or 35 mole%.

[0032] Additionally or alternatively, the EVOH may have a saponification degree of 90 mole% or higher, preferably 95 mole% or higher, preferably 97 mole% or higher, preferably 99.5 mole% or higher.

[0033] The EVOH particles described herein refer to the form and / or shape of one or more particles formed by granulation of EVOH resin. Although the present invention is described as forming one or more EVOH particles by granulation throughout the text, the EVOH particles can be processed into beads, cubes, fragments, shavings, etc.; according to some embodiments of the present invention, the shape of the EVOH resin particles is cylindrical, elliptical, angular, spherical, elliptical or go-shaped, and its major diameter or height is 1 to 5 mm, for example: 1, 2, 3, 4 or 5 mm; and its minor diameter is 1 to 5 mm, for example: 1, 2, 3, 4 or 5 mm. As used herein, the so-called "major diameter / height" refers to the longest outer diameter of an object whose surface is composed of a closed curved surface; and the so-called "minor diameter" refers to the smallest diameter in a cross section perpendicular to the major diameter or height and having the largest area. As used herein, the so-called “object whose surface is composed of a closed curved surface” can be understood as an object whose entire surface is composed of curved surfaces; an object formed by the intersection of multiple faces without edges and corners; or an object whose cross-section at any position is not rectangular.

[0034] Specifically, when the EVOH resin particles are cylindrical or elliptical, the height range is between 1 and 5 mm, for example, 1.5 to 5.0 mm, 1.7 to 5.0 mm, 2.2 to 5.0 mm, 2.4 to 5.0 mm, 2.6 to 5.0 mm, 2.8 to 5.0 mm, 3.0 to 5.0 mm, 3.2 to 5.0 mm, 3.4 to 5.0 mm, 3.6 to 5.0 mm, 3.8 to 5.0 mm, 4.0 to 5.0 mm, 1.7 to 4.5 mm, 1.7 to 4.4 mm, 1.7 to 4.2 mm, 1.7 to 4.0 mm, 1.7~3.8mm, 1.7~3.6mm, 1.7~3.4mm, 1.7~3.2mm, 1.7~3.0mm; its short diameter range is between 1~5mm, for example: 1.5~5.0mm, 1.7~5.0mm, 2.2~5.0mm, 2.4~5.0mm, 2.6~5.0mm, 2.8~5.0mm, 3.0~5.0mm, 3.2~5.0mm, 3.4~5.0mm, 3.6~5.0mm, 3.8~5.0mm, 4.0~5.0mm, 1.7~4.5mm, 1.7~4.4mm, 1.7~4.2mm, 1.7~4.0mm, 1.7~3.8mm, 1.7~3.6mm, 1.7~3.4mm, 1.7~3.2mm, 1.7~3.0mm.

[0035] When the EVOH particles are in the shape of spherical particles, such as spherical, elliptical or go-shaped particles, the range of their major diameter is between 1 and 5 mm, for example: 1.5-5.0 mm, 2.2-5.0 mm, 2.4-5.0 mm, 2.6-5.0 mm, 2.8-5.0 mm, 3.0-5.0 mm, 3.2-5.0 mm, 3.4-5.0 mm, 3.6-5.0 mm, 3.8-5.0 mm, 4.0-5.0 mm, 2.0-4.5 mm, 2.0-4.4 mm, 2.0-4.2 mm, 2.0-4.0 mm, 2.0-3.8 mm, 2.0~3.6mm, 2.0~3.4mm, 2.0~3.2mm, 2.0~3.0mm; the range of its short diameter is between 1~5mm, for example: 1.5~5.0mm, 1.8~4.6mm, 2.4~4.6mm, 2.6~4.6mm, 2.8~4.6 mm, 3.0~4.6mm, 3.2~4.6mm, 3.4~4.6mm, 3.6~4.6mm, 3.8~4.6mm, 4.0~4.6 mm, 1.6~4.5mm, 1.6~4.4mm, 1.6~4.2mm, 1.6~4.0mm, 1.6~3.8mm, 1.6~3.6 mm, 1.6~3.4mm, 1.6~3.2mm, 1.6~3.0mm. When the pellets are spherical, their long diameter and short diameter are equal.

[0036] According to some embodiments of the present invention, the weight percentage of the first EVOH resin particles to the second EVOH resin particles is 5:95 to 75:25, for example, 5:95, 15:85, 25:75, 35:65, 45:55, 55:45, 65:35 or 75:25.

[0037] According to some embodiments of the present invention, the EVOH resin particle composition may contain a boron compound and / or boric acid and / or cinnamic acid and / or an alkali metal and / or a conjugated polyene and / or a lubricant and / or an alkaline earth metal in some cases. The above substances can give the EVOH resin particle composition better properties.

[0038] According to some embodiments of the present invention, the EVOH resin particle composition may include a boron compound, wherein the boron content is 5 to 550 ppm. In some cases, the boron content of the EVOH resin particle composition may be 10 to 450 ppm, 10 to about 400 ppm, 10 to about 350 ppm, 10 to about 300 ppm, 10 to about 275 ppm, 10 to about 250 ppm, 10 to about 225 ppm, 10 to about 200 ppm, 10 to about 175 ppm, about 20 to 450 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 400 ppm, about 20 to about 45 ...10 to about 400 ppm, about 10 to about 275 ppm, about 10 to about 250 ppm, about 20 to about 350 ppm, about 20 to about 300 ppm, about 20 to about 275 ppm, about 20 to about 250 ppm, about 20 to about 225 ppm, about 20 to about 200 ppm, about 20 to about 175 ppm, about 60 to 450 ppm, about 60 to about 400 ppm, about 60 to about 350 ppm, about 60 to about 300 ppm, about 60 to about 275 ppm, about 60 to about 250 ppm, about 60 to about 225 ppm, about 60 to about 200 ppm, about 60 to about 175 ppm, about 100 to 450 ppm, about 100 to about 400 ppm, about 100 to about 350 ppm, about 100 to about 300 ppm, about 100 to about 275 ppm, about 100 to about 250 ppm, about 100 to about 225 ppm, about 100 to about 200 ppm, From about 100 to about 175 ppm, from about 140 to 450 ppm, from about 140 to about 400 ppm, from about 140 to about 350 ppm, from about 140 to about 300 ppm, from about 140 to about 275 ppm, from about 140 to about 250 ppm, from about 140 to about 225 ppm, from about 140 to about 200 ppm, from about 180 to about 450 ppm, from about 180 to about 400 ppm, from about 180 to about 350 ppm, from about 180 to about 300 ppm, from about 180 to about 275 ppm, from about 180 to about 250 ppm, from about 180 to about 225 ppm, from about 220 to 450 ppm, from about 220 to about 400 ppm, from about 220 to about 350 ppm, from about 220 to about 300 ppm, from about 220 to about 275 ppm. When the boron content of the EVOH resin particle composition is within a certain range, the viscosity of the EVOH resin particle composition can be increased and the chance of the EVOH resin particle composition adhering to the screw can be reduced, or the EVOH on the screw can be removed, so that the material has a self-cleaning function, which can further improve the uniformity of the film thickness. According to a preferred embodiment of the present invention, in addition to the boron compound, the EVOH resin particle composition may also include cinnamic acid, alkali metals, conjugated polyenes, alkaline earth metals, their salts and / or mixtures thereof; the above substances are common substances usually present in the EVOH resin particle composition, which makes it have better properties.When the content of the compound having a conjugated polyene structure is 1 to 30,000 ppm per unit weight of the EVOH resin pellet composition, coloration after heating can be further suppressed, and thermal stability is further improved. If the content of the alkali metal compound or alkaline earth metal compound per unit weight of the EVOH resin composition is 10 to 550 ppm in terms of metal, the long-term operation moldability can be better. The content can be, for example, between 10-550 ppm, between about 10-500 ppm, between about 10-450 ppm, between about 10-400 ppm, between about 10-350 ppm, between about 10-300 ppm, between about 10-250 ppm, between about 10-200 ppm, between about 10-150 ppm, between about 10-100 ppm, between about 10-50 ppm, between about 50-550 ppm, between about 50-500 ppm, between about 50-450 ppm, between about 50-400 ppm, between about 50-350 ppm, between about 50-300 ppm, between about 50-250 ppm, between about 50-200 ppm, between about 50-150 ppm, between about 50-100 ppm, between about 100-550 ppm, between about 100-500 ppm, between about 100-450 ppm, between about 100-400 ppm, between about 100-350 ppm, between about 100-300 ppm, between about 100-250 ppm, between about 100-200 ppm, between about 100-150 ppm, between about 200-550 ppm, between about 200-500 ppm, between about 200-450 ppm, between about 200-400 ppm, Between about 200-350 ppm, between about 200-300 ppm, between about 200-250 ppm, between about 300-550 ppm, between about 300-500 ppm, between about 300-450 ppm, between about 300-400 ppm, between about 300-350 ppm, between about 400-550 ppm, between about 400-500 ppm, between about 400-450 ppm or between about 500-550 ppm.

[0039] According to some embodiments of the present invention, the boron compound may include boric acid or a metal salt thereof. Examples of metal salts include, but are not limited to, calcium borate, cobalt borate, zinc borate (e.g., zinc tetraborate, zinc metaborate), potassium aluminum borate, ammonium borate (e.g., ammonium metaborate, ammonium tetraborate, ammonium pentaborate, ammonium octaborate), cadmium borate (e.g., cadmium orthoborate, cadmium tetraborate), potassium borate (e.g., potassium metaborate, potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate), silver borate (e.g., silver metaborate, silver tetraborate), copper borate (e.g., copper (II) borate, copper metaborate, copper tetraborate), sodium borate (e.g., sodium metaborate, sodium diborate, sodium tetraborate,

[0013] The present invention relates to a borate mineral comprising a borax mineral, a sintered borate mineral, a sintered borate mineral, a borax ... Among them, borax, boric acid and sodium borate (eg, sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate and sodium octaborate) are preferably used.

[0040] According to some embodiments of the present invention, the first EVOH resin particle has a kurtosis (Sku) surface parameter of 0.0020-25, for example, between about 0.0100-25, between about 0.1000-25, between about 1-25, between about 1-23.3000, between about 1-20, between about 1-15, between about 5-15, or between about 7-10. On the other hand, the second EVOH resin particle has a kurtosis (Sku) surface parameter of 0.0070-111, for example, between about 0.0100-111, 0.0200-100, between about 0.2000-65, between about 2-50, between about 2-40, between about 10-40, or between about 20-40.

[0041] As used herein, the so-called "kurtosis (Sku) surface parameter" is defined with reference to ISO 25178:2012; it can be understood as the height distribution of the contour surface within a sampling range, and is a parameter for determining the sharpness of the surface shape.

[0042] According to some embodiments of the present invention, the first EVOH resin particle has a surface parameter of a maximum peak height (Sp) of 0.0005 to 29 um, for example, between about 0.0005 to 28 um, between about 0.0010 to 25 um, between about 0.0100 to 25 um, between about 0.1000 to 25 um, between about 1 to 25 um, between about 1 to 20 um, between about 1 to 15 um, between about 5 to 15 um or between about 7 to 10 um. On the other hand, the second EVOH resin particles have a surface parameter of a maximum peak height (Sp) of 0.0020-63 um, for example, between about 0.0020-60 um, between about 0.0200-60 um, between about 0.2000-60 um, between about 2-60 um, between about 10-60 um, between about 20-50 um, between about 25-40 um, between about 30-40 um or between about 30-36 um.

[0043] As used herein, the so-called “maximum peak height (Sp) surface parameter” is defined with reference to ISO 25178:2012, which can be understood as the maximum height value relative to a reference surface within a sampling range.

[0044] According to some embodiments of the present invention, the first EVOH resin particle has a surface parameter of a protruding peak height (Spk) of 0.001-2 um, for example, between about 0.001-2 um, between about 0.005-2 um, between about 0.010-2 um, between about 0.050-2 um, between about 0.100-2 um, between about 0.100-1 um, or between about 0.500-1 um. On the other hand, the second EVOH resin particle has a surface parameter of a protruding peak height (Spk) of 0.003-22 um, for example, between about 0.003-20 um, between about 0.030-20 um, between about 0.300-20 um, between about 1-20 um, between about 5-20 um, between about 5-15 um, or between about 5-10 um.

[0045] As used herein, the so-called "protruding peak height (Spk) surface parameter" is defined with reference to ISO 25178:2012; specifically, it refers to the average height of the protruding peaks.

[0046] According to some embodiments of the present invention, the first EVOH resin particle has a peak height (Sxp) surface parameter of 0.001-12 um, for example, between about 0.001-11 um, between about 0.005-10 um, between about 0.010-2 um, between about 0.050-2 um, between about 0.100-2 um, between about 0.100-1 um, or between about 0.500-1 um. On the other hand, the second EVOH resin particle has a peak height (Sxp surface parameter of 0.002-48 um, for example, between about 0.003-48 um, between about 0.030-30 um, between about 0.300-20 um, between about 1-20 um, between about 5-20 um, between about 5-15 um, or between about 5-10 um.

[0047] As used herein, the so-called "pole height (Sxp) surface parameter" is defined with reference to ISO 25178:2012; specifically, it refers to the height difference between the surface average surface and the surface peak portion after removing particularly high peaks in the surface, and by default represents the height difference between a load area ratio of 2.5% and 50%.

[0048] According to some embodiments of the present invention, the first EVOH resin particle has a linear arithmetic average height (Ra) surface parameter of 0.001 to 0.990 um, for example: between about 0.001 to 0.990 um, between about 0.001 to 0.700 um, between about 0.001 to 0.500 um, between about 0.001 to 0.300 um, between about 0.001 to 0.100 um, between about 0.050 to 0.990 um, between about 0.050 to 0.700 um, between about 0.050 to 0.500 um, between about 0.050 to 0.300 um or between about 0.050 to 0.100 um. On the other hand, the second EVOH resin particles have a linear arithmetic average height (Ra) surface parameter of 0.001 to 0.990 um, for example: between about 0.001 to 0.990 um, between about 0.001 to 0.700 um, between about 0.001 to 0.500 um, between about 0.010 to 0.300 um, between about 0.010 to 0.100 um, between about 0.050 to 0.990 um, between about 0.050 to 0.700 um, between about 0.050 to 0.500 um, between about 0.050 to 0.300 um or between about 0.050 to 0.100 um.

[0049] As used herein, the so-called "line arithmetic mean height (Ra) surface parameter" is a parameter for defining surface roughness, and its definition can refer to JIS B 0601. Specifically, it can be understood as the average absolute value of a profile curve over a reference length.

[0050] According to some embodiments of the present invention, the first EVOH resin particle has a line maximum height (Rz) surface parameter of 0.0010 to 9.9000 um, for example: between about 0.0010 to 9 um, between about 0.0010 to 7 um, between about 0.0010 to 5 um, between about 0.0100 to 3 um, between about 0.0500 to 5 um, between about 0.0500 to 3 um, between about 0.0500 to 1 um or between about 0.0500 to 0.0800 um. On the other hand, the second EVOH resin particle has a line maximum height (Rz) surface parameter of 0.0010-9.9000 um, for example: between about 0.0800-9 um, between about 0.1000-9 um, between about 0.1500-9 um, between about 0.1500-7 um, between about 0.5000-5 um, between about 0.5000-2.5000 um or between about 1-2.5000 um. As used herein, the so-called "line maximum height (Rz) surface parameter" is a parameter defining surface roughness, and its definition can refer to JIS B 0601. Specifically, it can be understood as the distance between the highest peak and the lowest valley on a profile curve relative to a reference length.

[0051] In another aspect, the present invention provides an ethylene-vinyl alcohol copolymer film, which is formed from the above EVOH resin particle composition. Specifically, the ethylene-vinyl alcohol copolymer film is a single-layer film.

[0052] In yet another aspect, the present invention provides a multilayer structure comprising: (a) at least one ethylene-vinyl alcohol copolymer film formed from the EVOH resin particle composition; (b) at least one polymer layer; and (c) at least one adhesive layer.

[0053] According to some embodiments of the present invention, the polymer layer is selected from the group consisting of a low-density polyethylene layer, a polyethylene grafted maleic anhydride layer, a polypropylene layer and a nylon layer, and the adhesive layer is a tie layer, such as ARKEMA OREVAC 18729 of ARKEMA. Specifically, the stacked structure of the multilayer structure is a polymer layer, an adhesive layer, an ethylene-vinyl alcohol copolymer film, an adhesive layer and a polymer layer in sequence. According to some embodiments of the present invention, the thickness of the polymer layer is 100-500um, preferably 200-400um, and more preferably 300um; the thickness of the adhesive layer is 10-40um, preferably 20-30um, and more preferably 25um; the thickness of the ethylene-vinyl alcohol copolymer film is 20-80um, preferably 40-60um, and more preferably 50um.

[0054] Without being limited by any theory, it is believed that since the surface peak volume (Vmp) is the main factor affecting the thermal conductivity of the tip, it is related to the melting state during material processing, which will further affect the uniformity of thermal conductivity of the first EVOH resin particle and the second EVOH resin particle during processing. Therefore, when the Vmp values ​​of the first EVOH resin particle and the second EVOH resin particle in the EVOH resin particle composition are within a specific range, when the surface roughness of the EVOH peak with a high melting point is large, the peak portion will be melted first during processing, which can make the plastic particles more uniform in thermal conductivity and make the temperature of the melting zone forward; when the surface roughness of the EVOH peak with a low melting point is small, it can reduce local overheating of the peak portion during processing; therefore, it is possible to control the surface peak volume (Vmp) of the two EVOH resin particles to regulate the thermal conductivity state after melt mixing, so that they can be melted uniformly, and then obtain an EVOH film with good processing performance and mechanical properties in the subsequent process.

[0055] Example

[0056] The following non-limiting examples of various aspects of the present invention are provided primarily to illustrate various aspects of the present invention and the benefits achieved thereby. The EVOH formulation of each embodiment and comparative example is prepared from at least two components. More specifically, the two components of the EVOH resin particle composition of the embodiment and comparative example are two kinds of EVOH resin particles.

[0057] Preparation of EVOH resin particle composition

[0058] The following provides a non-limiting method for preparing EVOH resin particle compositions. Five non-limiting example EVOH resin particle compositions (Examples EVOH 1-5) and six comparative example EVOH resin particle compositions (Comparative Examples EVOH 1-6) were prepared according to methods similar to those disclosed below. However, the specific methods for preparing Example EVOH 1-5 and Comparative Examples EVOH 1-6 will generally differ from the methods disclosed below in one or more aspects.

[0059] First EVOH resin pellets of Example 1

[0060] In a polymerization reactor equipped with a cooling coil, 500 kg of vinyl acetate, 100 kg of methanol, 0.0585 kg of acetyl peroxide, and 0.015 kg of citric acid were added. The polymerization reactor was temporarily purged with nitrogen and then purged with ethylene and pressurized until the ethylene pressure reached 45 kg / cm 2 . Under ethylene pressure environment, the temperature was raised to 67°C while stirring to start polymerization. 6 hours after the start of polymerization, when the polymerization rate reached 60%, 0.0525 kg of sorbic acid conjugated polyene was added as an inhibitor. Thus, an ethylene-vinyl acetate copolymer with an ethylene structural unit content of 44 mole% was obtained. Then, the reaction solution containing the ethylene-vinyl acetate copolymer was supplied to a distillation tower, and methanol vapor was introduced from the lower part of the tower to remove unreacted vinyl acetate, thereby obtaining a methanol solution of ethylene-vinyl acetate copolymer.

[0061] In this embodiment, EVOH is formed by saponifying a component formed by polymerizing ethylene monomer and vinyl acetate monomer (ethylene-vinyl acetate copolymer, hereinafter referred to as "EVAC" polymer) with a saponification degree of 99.5%. Subsequently, EVOH is dissolved in an alcohol aqueous solution with a ratio of methanol to water of 70:30. The EVOH / methanol / water solution is placed at 60°C for 1 hour to promote the dissolution of EVOH in the EVOH / methanol / water solution. The solid content of the EVOH / methanol / water solution is 41wt%.

[0062] Next, the solution of methanol, water and EVOH is granulated by strip cutting. Specifically, the solution of methanol, water and EVOH is pumped into a feed pipe at a flow rate of 120 L / min using a pump, and then fed into a circular opening die with a diameter of 0.5 mm, and the EVOH solution is extruded into a 5°C water / methanol mixed solution (water / methanol mass ratio = 9 / 1) to precipitate into strands, which are then cut with a rotating knife at a rotation speed of 500 rpm to obtain EVOH particles. Subsequently, the EVOH particles are centrifuged to separate the EVOH particles, and the separated EVOH particles are washed with water; the above-mentioned centrifugal dehydration step is performed for the second time, and then the EVOH particles are immersed in a boric acid / sodium acetate solution, and then a drying step is performed and calcium stearate is added to obtain the final product of EVOH resin particles. The drying is carried out in three stages. The first stage uses a belt dryer and is dried at 80°C for 2 hours; the second stage uses a belt dryer and is dried at 100°C for 20 hours; the third stage uses a flow dryer and is dried at 120°C for 20 hours. Finally, the particles are transported. The so-called transportation is carried out under the following conditions: the transportation form is air transportation, the pipeline diameter is 6 inches, the number of elbows is 4, the pipeline length is 30 meters, and the transportation speed is 40m / min. The first EVOH resin particle of this embodiment is cylindrical, with a height of 5mm and a short diameter of 1mm.

[0063] In the aforementioned centrifugation and washing steps, the first dehydrator speed is 5000rpm; the water / wet particle ratio during transportation is 10; the type of centrifugal pump used for transportation is open; the delivery pump speed is 3000rpm; the water / wet particle weight ratio during water washing is 5; the water flow rate during water washing is 2m / min; the second dehydrator speed is 2000rpm.

[0064] Second EVOH resin pellets of Example 1

[0065] The second EVOH resin particles of Example 1 were prepared by a method similar to the above. The difference was that ethylene-vinylacetate copolymer (hereinafter referred to as "EVAC") with an ethylene content of 32 mole% was saponified at a saponification degree of 99.5% to prepare the EVOH polymer. The diameter of the opening die for strip cutting was 2 mm, and the rotating speed of the rotary knife was 2000 rpm.

[0066] In the centrifugal and washing steps of the second EVOH resin particles of this embodiment, the first dehydrator speed is 3000 rpm; the water / wet particle ratio during transportation is 3; the type of the centrifugal pump for transportation is open; the delivery pump speed is 2000 rpm; the water / wet particle weight ratio during water washing is 3; the water flow rate during water washing is 2.5 m / min; the second dehydrator speed is 3000 rpm. In addition, the final product of the second EVOH resin particles of this embodiment is cylindrical, with a height of 2 mm and a short diameter of 3 mm.

[0067] For subsequent further processes, the first EVOH resin particles and the second EVOH resin particles are further mixed in a ratio of 25 and 75 wt % respectively to form the EVOH resin particle composition of Example 1, and mixed using a conical screw mixer (model: CM-2, purchased from Xiehui Machinery Industry Co., Ltd.) at 10 rpm for 5 minutes.

[0068] The first and second EVOH resin particles of Example 2

[0069] The first and second EVOH methanol aqueous solutions used in Example 2 were prepared using a similar process (preparation process) to the EVOH resin particles of Example 1. However, when preparing the first EVOH methanol aqueous solution of Example 2, its ethylene content was 48 mole%; and the granulation step was performed by underwater pelletization to granulate the aforementioned methanol, water and EVOH solution. Specifically, a pump was used to pump the aforementioned methanol, water and EVOH solution into a feed pipe at a flow rate of 120 L / min, and then sent into an input pipe with a diameter of 1 mm, and a rotary knife was used to cut at 1500 rpm to obtain EVOH particles. At the same time, 5°C circulating condensed water was used to cool the EVOH particles. Subsequently, the EVOH particles were centrifuged to separate the EVOH particles, and the separated EVOH particles were washed with water; the above-mentioned centrifugal dehydration step was performed for the second time, and then the EVOH particles were immersed in a boric acid / sodium acetate solution, and then a drying step was performed and calcium stearate was added to obtain the final product of EVOH resin particles. The first EVOH resin particle of this embodiment was elliptical, with a long diameter of 3 mm and a short diameter of 2 mm.

[0070] In the centrifugation and washing steps, the speed of the first dehydrator is 3000rpm; the water / wet particle ratio during transportation is 10; the type of the centrifugal pump for transportation is semi-open; the speed of the delivery pump is 4000rpm; the water / wet particle weight ratio during water washing is 10; the water flow rate during water washing is 2m / min; the speed of the second dehydrator is 1000rpm; finally, the product of the first EVOH resin particle is ellipsoidal, with a major diameter of 3mm and a minor diameter of 2mm.

[0071] On the other hand, when preparing the second EVOH methanol aqueous solution of Example 2, its ethylene content is 27 mole%; and a similar process as the first EVOH resin particles of Example 2 is used; and the diameter of the input pipe is 2 mm; and in the centrifugal and washing steps, the first dehydrator speed is 2000 rpm; the water / wet particle ratio during transportation is 5; the type of the centrifugal pump for transportation is a closed type; the delivery pump speed is 1000 rpm; the water / wet particle weight ratio during water washing is 10; the water flow rate during water washing is 5 m / min; the second dehydrator speed is 3000 rpm; finally, the product of the second EVOH resin particles is spherical, and its short diameter is 3 mm. Further, the first EVOH resin particles and the second EVOH resin particles are further mixed in a weight percentage ratio of 10 and 90 wt% respectively to form the EVOH resin particle composition of Example 2.

[0072] The first and second EVOH resin particles of Example 3

[0073] The first EVOH methanol aqueous solution used in Example 3 was prepared using a process similar to that of the EVOH resin particles in Example 2. However, when preparing the first EVOH methanol aqueous solution in Example 3, its ethylene content was 38 mole%; and using a process similar to that of the first EVOH resin particles in Example 2, the diameter of the input pipe was 0.5 mm, and the rotating blade speed was 3000 rpm; and in the centrifugal and washing steps, the first dehydrator speed was 2500 rpm; the water / wet particle ratio during transportation was 8; the type of the centrifugal pump for transportation was open; the delivery pump speed was 5000 rpm; the water / wet particle weight ratio during water washing was 8; the water flow rate during water washing was 2.5 m / min; the second dehydrator speed was 3000 rpm; and finally, the product of the first EVOH resin particles was spherical, and its short diameter was 1 mm.

[0074] On the other hand, when the second EVOH methanol aqueous solution of Example 3 is prepared by a similar process to the EVOH resin particles of Example 1, its ethylene content is 29 mole%; the diameter of the opening die for strip cutting is 4 mm, and the rotating knife speed is 3000 rpm; and in the centrifugal and washing steps, the first dehydrator speed is 1000 rpm; the water / wet particle ratio during transportation is 5; the type of the centrifugal pump for transportation is semi-open; the speed of the delivery pump is 5000 rpm; the water / wet particle weight ratio during water washing is 5; the water flow rate during water washing is 5 m / min; the second dehydrator speed is 4000 rpm; finally, the product of the second EVOH resin particle is cylindrical, with a height of 1 mm and a short diameter of 5 mm. Further, the first EVOH resin particle and the second EVOH resin particle are further mixed in a weight percentage ratio of 50 and 50 wt% respectively to form the EVOH resin particle composition of Example 3.

[0075] The first and second EVOH resin particles of Example 4

[0076] The first EVOH resin pellets used in Example 4 were prepared using a process similar to that of the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Example 4, its ethylene content was 48 mol %; the diameter of the input pipe was 0.5 mm, and the rotating blade speed was 500 rpm; in the centrifugal and washing steps, the first dehydrator speed was 2500 rpm; the water / wet pellet ratio during transportation was 6; the type of the centrifugal pump for transportation was semi-open; the delivery pump speed was 5000 rpm; the water / wet pellet weight ratio during water washing was 7; the water flow rate during water washing was 2 m / min; the second dehydrator speed was 4000 rpm; Finally, the product of the first EVOH resin pellet was an ellipsoidal sphere with a major diameter of 5 mm and a minor diameter of 1 mm.

[0077] On the other hand, when the second EVOH methanol aqueous solution of Example 4 is prepared by a similar process to the EVOH resin particles of Example 1, its ethylene content is 32 mol%; and the diameter of the opening die for strip cutting is 2 mm, and the rotating knife speed is 1500 rpm; and in the centrifugal and washing steps, the first dehydrator speed is 3000 rpm; the water / wet particle ratio during transportation is 9; the type of the centrifugal pump for transportation is open; the speed of the delivery pump is 4000 rpm; the water / wet particle weight ratio during water washing is 10; the water flow rate during water washing is 5 m / min; the second dehydrator speed is 4000 rpm; finally, the product of the second EVOH resin particle is cylindrical, with a height of 3 mm and a short diameter of 3 mm. Further, the first EVOH resin particle and the second EVOH resin particle are further mixed in a weight percentage ratio of 15 and 85 wt% respectively to form the EVOH resin particle composition of Example 4.

[0078] The first and second EVOH resin particles of Example 5

[0079] The first and second EVOH resin pellets used in Example 5 were prepared using a similar process to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Example 5, its ethylene content was 38 mol%, and the diameter of the input pipe was 1 mm, and the rotating blade speed was 1000 rpm. In the centrifugal and washing steps, the first dehydrator speed was 4000 rpm, the water / wet pellet ratio during transportation was 7, the type of the centrifugal pump for transportation was open, the delivery pump speed was 3000 rpm, the water / wet pellet weight ratio during water washing was 8, the water flow rate during water washing was 7 m / min, and the second dehydrator speed was 2000 rpm. Finally, the product of the first EVOH resin pellet was an ellipsoidal sphere with a major diameter of 4 mm and a minor diameter of 2 mm.

[0080] On the other hand, when preparing the second EVOH methanol aqueous solution of Example 5, its ethylene content is 24 mol%; and the diameter of the input pipe is 0.5mm, and the rotating speed of the rotary knife is 1000rpm; and in the centrifugal and washing steps, the speed of the first dehydrator is 5000rpm; the water / wet particle ratio during transportation is 9; the type of the centrifugal pump for transportation is semi-open; the speed of the delivery pump is 3000rpm; the water / wet particle weight ratio during water washing is 10; the water flow rate during water washing is 6m / min; the speed of the second dehydrator is 1000rpm; Finally, the product of the second EVOH resin particle is an ellipsoidal sphere with a long diameter of 4mm and a short diameter of 1mm. Further, the first EVOH resin particle and the second EVOH resin particle are further mixed in a weight percentage of 35 and 65wt% respectively to form the EVOH resin particle composition of Example 5.

[0081] The first and second EVOH resin pellets of Comparative Example 1

[0082] The first EVOH resin pellets used in Comparative Example 1 were prepared using a process similar to that of the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 1, its ethylene content was 44 mol %; the diameter of the input pipe was 2.5 mm, and the rotating blade speed was 1200 rpm; in the centrifugal and washing steps, the first dehydrator speed was 2000 rpm; the water / wet pellet ratio during transportation was 10; the type of the centrifugal pump for transportation was open; the delivery pump speed was 1000 rpm; the water / wet pellet weight ratio during water washing was 15; the water flow rate during water washing was 2 m / min; the second dehydrator speed was 1000 rpm; and finally, the product of the first EVOH resin pellets was spherical, and its short diameter was 3.5 mm.

[0083] On the other hand, when the second EVOH methanol aqueous solution of Comparative Example 1 was prepared by a similar process to the EVOH resin particles of Example 1, its ethylene content was 29 mol%; and the diameter of the opening die for strip cutting was 3.5 mm, and the rotating knife speed was 500 rpm; and in the centrifugal and washing steps, the first dehydrator speed was 1000 rpm; the water / wet particle ratio during transportation was 15; the type of centrifugal pump for transportation was open; the speed of the delivery pump was 2000 rpm; the water / wet particle weight ratio during water washing was 20; the water flow rate during water washing was 1 m / min; the second dehydrator speed was 1000 rpm; finally, the product of the second EVOH resin particles was cylindrical, with a height of 5 mm and a short diameter of 4.5 mm. Further, the first EVOH resin particles and the second EVOH resin particles were further mixed in a weight percentage ratio of 5 and 95 wt% respectively to form the EVOH resin particle composition of Comparative Example 1.

[0084] The first and second EVOH resin pellets of Comparative Example 2

[0085] The first EVOH resin pellets for Comparative Example 2 were prepared using a process similar to that of the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 2, its ethylene content was 35 mol %; the diameter of the input pipe was 1 mm, and the rotating blade speed was 1500 rpm; in the centrifugal and washing steps, the first dehydrator speed was 3000 rpm; the water / wet pellet ratio during transportation was 20; the type of the centrifugal pump for transportation was open; the delivery pump speed was 1000 rpm; the water / wet pellet weight ratio during water washing was 15; the water flow rate during water washing was 1.5 m / min; the second dehydrator speed was 2000 rpm; and finally, the product of the first EVOH resin pellets was an ellipsoidal sphere with a major diameter of 3 mm and a minor diameter of 2 mm.

[0086] On the other hand, the second EVOH resin pellets of Comparative Example 2 were prepared by a similar process to the EVOH resin pellets of Example 1, however, when preparing the second EVOH methanol aqueous solution of Comparative Example 2, its ethylene content was 24 mol%; and the diameter of the opening die for strip cutting was 1 mm, and the rotating knife speed was 1000 rpm; and in the centrifugal and washing steps, the first dehydrator speed was 8000 rpm; the water / wet pellet ratio during transportation was 1; the type of the centrifugal pump for transportation was a closed type; the delivery pump speed was 8000 rpm; the water / wet pellet weight ratio during water washing was 1; the water flow rate during water washing was 8 m / min; the second dehydrator speed was 5000 rpm; finally, the product of the second EVOH resin pellets was cylindrical, with a height of 4 mm and a short diameter of 2 mm. Further, the first EVOH resin pellets and the second EVOH resin pellets were further mixed in a weight percentage ratio of 75 and 25 wt% respectively to form the EVOH resin pellet composition of Comparative Example 2.

[0087] The first and second EVOH resin pellets of Comparative Example 3

[0088] The first and second EVOH resin pellets for Comparative Example 3 were prepared using a process similar to that of the EVOH resin pellets of Example 1. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 3, its ethylene content was 48 mol %; the diameter of the opening die for strip cutting was 3 mm, and the rotating knife speed was 1700 rpm; and in the centrifugal and washing steps, the first dehydrator speed was 7000 rpm; the water / wet pellet ratio during transportation was 3; the type of the centrifugal pump for transportation was a closed type; the delivery pump speed was 7000 rpm; the water / wet pellet weight ratio during water washing was 1; the water flow rate during water washing was 7 m / min; the second dehydrator speed was 6000 rpm; and finally, the product of the first EVOH resin pellet was cylindrical, with a height of 2.5 mm and a short diameter of 4 mm. On the other hand, when preparing the second methanol aqueous solution of Comparative Example 3, its ethylene content is 32 mol%; and the diameter of the opening die for strip cutting is 2 mm, and the rotating knife speed is 1200 rpm; and in the centrifugal and washing steps, the first dehydrator speed is 6000 rpm; the water / wet particle ratio during transportation is 1; the type of the centrifugal pump for transportation is a closed type; the delivery pump speed is 6000 rpm; the water / wet particle weight ratio during water washing is 3; the water flow rate during water washing is 6 m / min; the second dehydrator speed is 5000 rpm; finally, the product of the second EVOH resin particle is cylindrical, with a height of 3.5 mm and a short diameter of 3 mm. Further, the above-mentioned first EVOH resin particle and the second EVOH resin particle are further mixed in a weight percentage ratio of 15 and 85 wt% respectively to form the EVOH resin particle composition of Comparative Example 3.

[0089] The first and second EVOH resin pellets of Comparative Example 4

[0090] The first and second EVOH resin pellets for Comparative Example 4 were prepared using a process similar to that of the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 4, its ethylene content was 38 mol %; the diameter of the input pipe was 0.5 mm, and the rotating blade speed was 3000 rpm; in the centrifugal and washing steps, the first dehydrator speed was 3000 rpm; the water / wet pellet ratio during transportation was 8; the type of the centrifugal pump for transportation was open; the delivery pump speed was 4000 rpm; the water / wet pellet weight ratio during water washing was 8; the water flow rate during water washing was 2.5 m / min; the second dehydrator speed was 3000 rpm; and finally, the product of the first EVOH resin pellet was spherical, and its short diameter was 1 mm. On the other hand, when preparing the second EVOH methanol aqueous solution of Comparative Example 4, its ethylene content is 27 mol%; and the diameter of the input pipe is 3mm, and the rotating blade speed is 1000rpm; and in the centrifugal and washing steps, the first dehydrator speed is 8000rpm; the water / wet particle ratio during transportation is 1; the type of the centrifugal pump for transportation is a closed type; the delivery pump speed is 8000rpm; the water / wet particle weight ratio during water washing is 3; the water flow rate during water washing is 6m / min; the second dehydrator speed is 6000rpm; finally, the product of the second EVOH resin particle is spherical, and its short diameter is 4mm. Further, the first EVOH resin particle and the second EVOH resin particle are further mixed in a weight percentage ratio of 10 and 90wt% respectively to form the EVOH resin particle composition of Comparative Example 4.

[0091] The first and second EVOH resin pellets of Comparative Example 5

[0092] The first and second EVOH resin pellets for Comparative Example 5 were prepared using a similar process to the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 5, its ethylene content was 44 mol%, and the diameter of the input pipe was 2.5 mm, and the rotating blade speed was 1000 rpm; and in the centrifugal and washing steps, the first dehydrator speed was 1000 rpm; the water / wet pellet ratio during transportation was 10; the type of the centrifugal pump for transportation was open; the delivery pump speed was 3000 rpm; the water / wet pellet weight ratio during water washing was 10; the water flow rate during water washing was 1 m / min; the second dehydrator speed was 1000 rpm; and finally, the product of the first EVOH resin pellet was an ellipsoidal sphere with a major diameter of 4 mm and a minor diameter of 3.5 mm. On the other hand, when preparing the second EVOH methanol aqueous solution of Comparative Example 5, its ethylene content is 29 mol%; and the diameter of the input pipe is 0.5 mm, and the rotating knife speed is 1700 rpm; and in the centrifugal and washing steps, the first dehydrator speed is 3000 rpm; the water / wet particle ratio during transportation is 5; the type of the centrifugal pump for transportation is a closed type; the delivery pump speed is 2000 rpm; the water / wet particle weight ratio during water washing is 10; the water flow rate during water washing is 5 m / min; the second dehydrator speed is 3000 rpm; Finally, the product of the second EVOH resin particle is an ellipsoidal sphere with a long diameter of 2.5 mm and a short diameter of 1 mm. Further, the first EVOH resin particle and the second EVOH resin particle are further mixed in a weight percentage ratio of 20 and 80 wt% respectively to form the EVOH resin particle composition of Comparative Example 5.

[0093] The first and second EVOH resin pellets of Comparative Example 6

[0094] The first and second EVOH resin pellets for Comparative Example 6 were prepared using a process similar to that of the EVOH resin pellets of Example 2. However, when preparing the first EVOH methanol aqueous solution of Comparative Example 6, its ethylene content was 38 mol %; the diameter of the input pipe was 1.5 mm, and the rotating blade speed was 1700 rpm; and in the centrifugal and washing steps, the first dehydrator speed was 7000 rpm; the water / wet pellet ratio during transportation was 2; the type of the centrifugal pump for transportation was a closed type; the delivery pump speed was 8000 rpm; the water / wet pellet weight ratio during water washing was 3; the water flow rate during water washing was 10 m / min; the second dehydrator speed was 6000 rpm; and finally, the product of the first EVOH resin pellet was spherical, and its short diameter was 2.5 mm. On the other hand, when preparing the second EVOH methanol aqueous solution of Comparative Example 6, its ethylene content is 32 mol%; and the diameter of the input pipe is 0.5 mm, and the rotating blade speed is 1000 rpm; and in the centrifugal and washing steps, the first dehydrator speed is 1000 rpm; the water / wet particle ratio during transportation is 3; the type of the centrifugal pump for transportation is semi-open; the speed of the delivery pump is 3000 rpm; the water / wet particle weight ratio during water washing is 5; the water flow rate during water washing is 3 m / min; the second dehydrator speed is 4000 rpm; finally, the product of the second EVOH resin particle is an ellipsoidal sphere with a long diameter of 4 mm and a short diameter of 1 mm. Further, the first EVOH resin particle and the second EVOH resin particle are further mixed in a weight percentage ratio of 35 and 65 wt% respectively to form the EVOH resin particle composition of Comparative Example 6.

[0095] Parameters of EVOH resin pellets

[0096] The parameters of the EVOH resin pellets of the present invention and their evaluation / analysis methods are provided below.

[0097] Particle surface roughness

[0098] In order to evaluate / analyze the surface roughness of the EVOH resin particles in the embodiment, the EVOH resin particles are placed flat on a plate to measure the surface roughness of the particles; when measuring, the part of the data when the inclination is greater than 0.5 should be excluded to ensure that the scanning plane is in a relatively horizontal state (inclination = maximum surface height Sz / side length of the analysis range 129μm). The laser microscope is LEXT OLS5000-SAF manufactured by Olympus, and the image is made at an air temperature of 24±3°C and a relative humidity of 63±3%. The filter is set to no filtering. The light source is a 405nm-wavelength light source. The objective lens is 100x magnification (MPLAPON-100xLEXT). The optical zoom is set to 1.0x. The image area is set to 129μm x 129μm (when measuring Rz, the center line of the image area is taken). The resolution is set to 1024 pixels x 1024 pixels. The values ​​of 100 particles are measured and the average value is taken. Among them, Vmp, Sku, Sp, Spk and Sxp are measured using the ISO 25178:2012 method; Ra and Rz are measured using the JIS B 0601 (2001) method.

[0099] Ethylene content analysis

[0100] In order to evaluate / analyze the ethylene content of the EVOH resin particles of the embodiment, the present invention uses a Raman spectrometer manufactured by UniDRON, and uses a laser light source with a wavelength of 473nm to randomly measure the ethylene content of 5 points on each EVOH resin particle, and takes the average value as the ethylene content value of the EVOH resin particle sample.

[0101] Melting point analysis

[0102] Here, the melting point temperature of the EVOH resin pellets is measured according to ISO 11357-3-2011 method using a DSC Q200 device (TZERO TECHNOLOGIES, INC.; Tzero lid is TA Instruments T170607, and Tzero pan is TA Instruments T170620).

[0103] In practice, without being limited by a specific theory, when there are a large number of EVOH resin particles, 100 EVOH resin particles can be taken and their individual ethylene contents can be obtained by the above-mentioned ethylene content analysis method. Subsequently, for those with an ethylene content between 35 and 48 mol%, they are pre-classified as low-melting-point EVOH resin particles with a melting point of about 135 to 179°C; and for those with an ethylene content between 24 and 34 mol%, they are pre-classified as high-melting-point EVOH resin particles with a melting point of about 180 to 198°C. Further, 10 EVOH resin particles are randomly taken out from the groups of low-melting-point EVOH resin particles and high-melting-point EVOH resin particles, and their surface roughness is obtained by the above-mentioned surface parameter determination method, and then the melting points of these EVOH resin particles are determined by the above-mentioned melting point determination method.

[0104] Preparation and analysis of EVOH single-layer film

[0105] The EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6 were formed into films according to the following method. The EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6 were fed into a single screw extruder (model ME25 / 5800V4, brand OCS) to extrude and prepare a single-layer film. The thickness of the films formed by the EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6 was 20 μm. The temperature of the extruder was set to 220° C.; and the rotation frequency of the screw was set to 7 rpm (rotations / minutes).

[0106] Analysis of processing performance of EVOH film: determination and evaluation of gel particles (Gel)

[0107] Here, a charge coupled device (CCD) sensor and FSA-100 designed with FSA-100V.8 software were used to measure and analyze the gel particles of the above EVOH film. The evaluation method is: if the size of the gel particles is <100μm, the number of which is <450 is represented by "O" for the best; the number of which is 450-1000 is represented by "Δ" for acceptable; and the number of which is >1000 is represented by "X" for poor. If the size of the gel particles is 100-200μm, the number of which is <50 is represented by "O" for the best; the number of which is 50-100 is represented by "Δ" for acceptable; and the number of which is >100 is represented by "X" for poor. If the gel particle size is >200 μm, the number of which is less than 10 is indicated by “O” as the best; the number of which is 10-20 is indicated by “Δ” as fair; and the number of which is >20 is indicated by “X” as poor.

[0108] Analysis of mechanical properties of EVOH film: Determination and evaluation of film elongation

[0109] Here, a single-layer film with a thickness of 180um was formed by the above-mentioned single screw extruder, and was cut into a size of MD30mm*TD90mm (Transverse Direction, TD, or width direction; MD refers to Machine Direction, i.e., machine direction or longitudinal direction, length direction); then, after being placed in an environment with a temperature of 130°C for 30 minutes, the film was measured in the MD and TD directions respectively at a tensile speed of 1000mm / min using ASTM D882. As used herein, "stretching rate (%)" is defined as [(length after stretching - length before stretching) / length before stretching]*100%; the evaluation method is: if the film stretching rate value of the film sample is greater than 1000%, "O" indicates the best; if the film stretching rate value of the film sample is between 800 and 1000%, "Δ" indicates acceptable; and if the film stretching rate value of the film sample is less than 800%, "X" indicates poor.

[0110] Preparation of multilayer structures

[0111] Here, the EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6, polypropylene and a bonding layer (eg 18729, Arkema Co., Ltd.) were co-extruded to form the respective multilayer films of Examples 1 to 5 and Comparative Examples 1 to 6. The multilayer film has 5 layers. Specifically, EVOH particles (Ⅰ), polypropylene (Ⅱ) and adhesive resin (Ⅲ) were fed to a five-layer co-extrusion film forming machine to prepare a multilayer sheet having the following structure: (Ⅱ) / (Ⅲ) / (Ⅰ) / (Ⅲ) / (Ⅱ), with thicknesses of 300 / 25 / 50 / 25 / 300 (um), respectively.

[0112] Results Analysis of Examples and Comparative Examples

[0113] In this section, the EVOH resin particle compositions of Examples 1 to 5 and Comparative Examples 1 to 6, as well as the gel particles and elongation analysis results of the films prepared therefrom are compared. The specific data are shown in Tables 1 and 2, respectively.

[0114] Table 1

[0115]

[0116] Table 2

[0117]

[0118] As can be seen from Table 1 and Table 2, the surface peak volume (Vmp) of the first EVOH resin particles contained in the EVOH resin particle composition of Examples 1 to 5 is 0.00001 to 6 μm. 3 / um 2 , and at the same time the surface peak volume (Vmp) of the second EVOH resin particle is 0.00015-20um 3 / um 2 ; and thus the film made thereof has good performance in gel particles and elongation; in other words, the film substantially has excellent processing performance and mechanical properties. In contrast, the EVOH resin particle composition of Comparative Examples 1 to 6 does not meet the numerical range of the surface peak portion solid volume (Vmp) of the above-mentioned first and second EVOH resin particles; resulting in unsatisfactory processing performance and mechanical properties of the film made thereof. Preferably, the Vmp of the second EVOH resin particle of the present invention is greater than the Vmp of the first EVOH resin particle. Preferably, the melting point of the first EVOH resin particle is 135 to 179°C, and the melting point of the second EVOH resin particle is 180 to 198°C. Preferably, the ethylene content of the first EVOH resin particle is 36 to 50 mole percent, and the ethylene content of the second EVOH resin particle is 20 to 35 mole percent.

[0119] Further comparison of Table 1 and Table 2 shows that although the first EVOH resin particles contained in the EVOH resin particle composition of Comparative Example 4, the second EVOH resin particles contained in the EVOH resin particle composition of Comparative Example 5, and the second EVOH resin particles contained in the EVOH resin particle composition of Comparative Example 6 respectively fall within the Vmp numerical range of the first / second EVOH resin particles defined in the present invention, the other EVOH resin particles contained in these EVOH resin particle compositions are not within the corresponding Vmp numerical range. It can be understood that only when the two EVOH resin particles contained in the EVOH resin particle composition meet the Vmp numerical range defined in this case, the two EVOH resins can have more ideal processing performance and mechanical properties after being mixed and made into a film.

[0120] In addition, the inventors have found that by adjusting the manufacturing process variables of the centrifugation and washing procedures during the processing of EVOH resin particles, the desired surface peak volume (Vmp) of the present invention can be further controlled and obtained; specifically, without being limited by any theory, too high a dehydrator speed, too low a water / wet particle ratio during transportation and water washing, too high a conveying pump speed when a closed centrifugal pump is used during transportation, and too fast a water flow rate will all increase the surface peak volume of EVOH resin particles to a certain extent; On the contrary, if the speed of the dehydrator is too low, the water / wet particle ratio during transportation and water washing is too high, the speed of the conveying pump is too low when the centrifugal pump is used in an open type during transportation, and the water flow rate is too slow, etc., they will all cause a decrease in the surface peak portion of the EVOH resin particles to a certain extent; in a specific embodiment, the speed of the dehydrator is preferably controlled at 1000-5000rpm, the water / wet particle ratio during transportation and water washing is preferably controlled at 3 to 10, the speed of the conveying pump is preferably not more than 5000rpm when the centrifugal pump is used in a closed type during transportation, the speed of the conveying pump is preferably not less than 1000rpm when the centrifugal pump is used in an open type during transportation, the water flow rate during water washing is between 2 and 7m / min, and the speed of the second dehydrator is preferably controlled at 1000-4000rpm, so as to obtain the desired surface peak portion of the EVOH resin particles.

[0121] Herein, all ranges provided are intended to include each specific range within a given range and combinations of sub-ranges between the given ranges. In addition, unless otherwise stated, all ranges provided herein include the endpoints of the ranges. Thus, ranges 1-5 specifically include 1, 2, 3, 4, and 5, and sub-ranges such as 2-5, 3-5, 2-3, 2-4, 1-4, etc.

[0122] All publications and patent applications cited in this specification are incorporated herein by reference, and each individual publication or patent application is specifically and individually indicated to be incorporated herein by reference for any and all purposes. In the event of any inconsistency between this document and any publication or patent application incorporated herein by reference, this document controls.

[0123] As used herein, the terms "include", "have" and "comprises" have an open, non-restrictive meaning. The terms "a", "an" and "the" are to be understood to cover the plural as well as the singular. The term "one or more" means "at least one", and thus may include a single feature or a mixture / combination of features. The term "between" includes both endpoints.

[0124] Except in the operating examples or where otherwise indicated, all numbers indicating amounts of ingredients and / or reaction conditions may in all cases be modified by the term "about", meaning within ±5% of the indicated number. As used herein, the terms "substantially free" or "substantially free" refer to less than about 2% of a particular feature. All elements or features that are positively described herein may be negatively excluded from the claims.

[0125]

Symbol explanation

[0126]

Biological material deposit

Claims

1. An ethylene vinyl alcohol copolymer (EVOH) resin particle composition comprising: The first EVOH resin particle has a surface peak volume (Vmp) of 0.00001-6 μm 3 / um 2 ,and The second EVOH resin particle has a surface peak volume (Vmp) of 0.00015-20 μm 3 / um 2 , wherein the ethylene content of the first EVOH resin particles is 36 to 50 mol percent, and the ethylene content of the second EVOH resin particles is 20 to 35 mol percent; The Vmp of the second EVOH resin particles is greater than the Vmp of the first EVOH resin particles.

2. The EVOH resin particle composition according to claim 1, wherein the melting point of the first EVOH resin particles is 135 to 179°C, and wherein the melting point of the second EVOH resin particles is 180 to 198°C.

3. The EVOH resin particle composition according to claim 1 or 2, wherein the EVOH resin particles are in the shape of a cylinder, an elliptical cylinder, an angular cylinder, a sphere, an elliptical sphere or a go shape, and have a major diameter / height of 1 to 5 mm and a minor diameter of 1 to 5 mm. 4 . The EVOH resin particle composition according to claim 1 , wherein the weight percentage of the first EVOH resin particles to the second EVOH resin particles is 5:95 to 75:

25.

5. The EVOH resin pellet composition according to claim 1 or 2, which has a boron content of 5 to 550 ppm.

6. The EVOH resin pellet composition according to claim 1 or 2, which has an alkali metal content of 10 to 550 ppm.

7. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a kurtosis (Sku) surface parameter of 0.0020 to 25; and The second EVOH resin particles have a kurtosis (Sku) surface parameter of 0.0070 to 111.

8. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a surface parameter of a maximum peak height (Sp) of 0.0005 to 29 μm; and The second EVOH resin particles have a surface parameter of a maximum peak height (Sp) of 0.0020 to 63 μm.

9. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a surface parameter of a protruding peak height (Spk) of 0.001 to 2 um; and The second EVOH resin particles have a surface parameter of a protruding peak height (Spk) of 0.003 to 22 μm.

10. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a surface parameter of a peak height (Sxp) of 0.001 to 12 um; and The second EVOH resin particles have a pole height (Sxp) surface parameter of 0.002-48 um.

11. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a surface parameter of a linear arithmetic average height (Ra) of 0.001 to 0.990 um; and The second EVOH resin particles have a surface parameter of a linear arithmetic average height (Ra) of 0.001 to 0.990 um.

12. The EVOH resin particle composition according to claim 1 or 2, wherein: The first EVOH resin particles have a line maximum height (Rz) surface parameter of 0.0010 to 9.9000 um; and The second EVOH resin particles have a line maximum height (Rz) surface parameter of 0.0010 to 9.9000 um.

13. An ethylene-vinyl alcohol copolymer film, which is formed from the EVOH resin particle composition according to any one of claims 1 to 12.

14. A multi-layer structure comprising: (a) at least one layer of an ethylene-vinyl alcohol copolymer film formed from the EVOH resin particle composition according to any one of claims 1 to 12; (b) at least one polymer layer; and (c) at least one adhesive layer.

15. The multilayer structure of claim 14, wherein the polymer layer is selected from the group consisting of a low density polyethylene layer, a polyethylene grafted maleic anhydride layer, a polypropylene layer, and a nylon layer, and the adhesive layer is a tie layer.

16. The multilayer structure according to claim 14 or 15, wherein the multilayer structure is polymer layer / adhesive layer / ethylene-vinyl alcohol copolymer film / adhesive layer / polymer layer.