A method for efficiently extracting vanadium, molybdenum and nickel from polymetallic vanadium shale
Vanadium and nickel leaching through sulfuric acid and fluorite additives, hydrogen peroxide and citric acid leaching molybdenum in step by step, and through the pH adjustment of the acid leachate, the problem of vanadium, molybdenum and nickel in vanadium shale is solved, achieving high efficiency The effect of separation and low acid consumption.
Patent Information
- Application Number
- CN202211048575.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-08-30
AI Technical Summary
The prior art is difficult to extract vanadium, molybdenum and nickel at the same time from vanadium shale, and there is a lack of an effective separation method.
Use sulfuric acid and fluorite additives to efficiently leach vanadium and nickel, and hydrogen peroxide and citric acid to leach molybdenum in step by step. The molybdenum-containing complex is stabilized by adjusting the pH value of the acid leach solution, making full use of residual acid and reducing acid consumption.
It realizes efficient leaching of vanadium, molybdenum and nickel and has low acid consumption, reducing costs and broad application prospects.
Smart Images

Figure CN115478177B_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of chemical metallurgy, and in particular to a method for efficiently extracting vanadium, molybdenum and nickel from polymetallic vanadium shale. Background technology:
[0002] my country has rich vanadium shale reserves, ranking first in the world, and is the main source of separation and extraction of metallic vanadium in my country. The valuable metal in vanadium shale is mainly vanadium, and there are fewer minerals containing molybdenum and nickel in vanadium shale. Therefore, there are many technologies for extracting vanadium from vanadium shale, but there is almost no technology for simultaneously separating and extracting vanadium, molybdenum and nickel from vanadium shale. This problem needs to be solved urgently. Summary of the invention:
[0003] The invention solves the problem in the prior art that vanadium, molybdenum and nickel in multi-metal vanadium shale are difficult to be efficiently leached simultaneously, and provides a method for efficiently extracting vanadium, molybdenum and nickel from multi-metal vanadium shale. The method proposed by the invention first uses sulfuric acid and fluorite as an auxiliary agent to efficiently leach vanadium and nickel, then uses hydrogen peroxide and citric acid to efficiently leach molybdenum in steps, and uses vanadium shale to neutralize the acid leaching solution to a pH of 1.5 to 1.8 to stabilize the molybdenum-containing complex therein, and at the same time fully utilizes the residual acid in the acid leaching solution to reduce acid consumption, thereby achieving the purpose of efficiently separating vanadium, molybdenum and nickel from vanadium shale.
[0004] The object of the present invention is to provide a method for efficiently extracting vanadium, molybdenum and nickel from polymetallic vanadium shale, comprising the following steps:
[0005] (1) Using vanadium shale and the neutralized slag produced by neutralizing the acid leaching solution of vanadium shale as acid leaching materials, adding sulfuric acid aqueous solution and fluorite to the acid leaching materials and mixing them evenly, the mass ratio of sulfuric acid aqueous solution to acid leaching materials is 0.8-1:1, the sulfuric acid in the sulfuric acid aqueous solution is 20-25wt% of the mass of the acid leaching materials, and the fluorite is 2.0-3.0wt% of the mass of the acid leaching materials, and then adding hydrogen peroxide, the mass concentration of hydrogen peroxide is 25%-35%, and the hydrogen peroxide is 10-12wt% of the mass of the acid leaching materials, heating to 90° C.-95° C. for acid leaching reaction for 6-10 hours, so that vanadium and nickel in the vanadium shale are leached, after the acid leaching reaction is completed, adding citric acid, the citric acid is 0.2-0.3wt% of the mass of the acid leaching materials, and continuing the reaction for 14-18 hours, and separating the obtained mixed solution into solid-liquid to obtain acid leaching solution and acid leaching slag;
[0006] (2) taking vanadium shale and neutralizing the acid leaching solution obtained in step (1) to a pH of 1.5 to 1.8, filtering and separating, and obtaining an acid solution containing vanadium / molybdenum / nickel for subsequent use in extracting vanadium, molybdenum and nickel, as well as neutralizing slag produced by neutralizing the acid leaching solution;
[0007] (3) The neutralized slag produced by the neutralized acid leaching solution obtained in step (2) is returned to the acid leaching process in step (1) and mixed with the vanadium shale as an acid leaching material for acid leaching.
[0008] The present invention uses sulfuric acid and fluorite as auxiliary agents to efficiently leach vanadium and nickel from polymetallic vanadium shale, uses hydrogen peroxide and citric acid to efficiently leach molybdenum in steps, uses vanadium shale to neutralize the acid leaching solution to a pH of 1.5-1.8, stabilizes the molybdenum-containing complex therein, and fully utilizes the residual acid in the acid leaching solution to reduce acid consumption, thereby achieving the purpose of efficiently separating vanadium, molybdenum and nickel from vanadium shale.
[0009] Preferably, after the acid leaching reaction in step (1) is completed, the pH value of the acid leaching system is 0.6-0.8, citric acid is added, and the reaction is continued for 14-18 hours, and the pH value of the acid leaching liquid obtained by solid-liquid separation is 0.8-1.0.
[0010] Preferably, the mass ratio of the vanadium shale in step (1) to the neutralized slag produced by neutralizing the vanadium shale with the acid leaching solution is 1 to 1.2:1.
[0011] In step (3), the neutralized slag produced by neutralizing the acid leaching liquid is returned to step (1), and the neutralized slag produced by neutralizing the acid leaching liquid and the vanadium shale are used as acid leaching materials to carry out acid leaching reaction. The mass of the acid leaching liquid entrained in the neutralized slag is 13.0-15.0wt% of the mass of the vanadium shale.
[0012] Compared with the prior art, the present invention has the following advantages:
[0013] 1. The present invention uses sulfuric acid and hydrogen peroxide to leach molybdenum in vanadium shale into an acid leaching solution in the form of molybdic acid. After the acid leaching reaction for 8 hours, the acidity of the acid leaching system drops to pH 0.6-0.8. Then, citric acid is added to the reaction system. The reduction in acidity is conducive to the complexation reaction of citric acid. The reaction is continued for 16 hours. During the reaction, citric acid is complexed with molybdic acid entering the acid solution in time, so that molybdic acid is stably present in the solution to prevent its precipitation. After the acid leaching is completed, solid-liquid separation is carried out in time, and the acid leaching solution is neutralized to pH 1.5-1.8 in time with vanadium shale, so that the citric acid molybdenum complex is more stably present in the acid solution to prevent the molybdenum acid from precipitating when the acid leaching solution is left standing for a long time. At the same time, vanadium shale contains acid-consuming components, and the residual acid in the acid leaching solution can be used to neutralize part of the acid-consuming components in the vanadium shale, saving the consumption of this part of sulfuric acid in the acid leaching process and achieving the purpose of reducing acid.
[0014] 2. The present invention realizes efficient leaching of vanadium, molybdenum and nickel through ingenious process design, while achieving the purpose of reducing acid consumption and reducing costs. This method has broad application prospects. Description of the drawings:
[0015] Figure 1 The present invention is a process flow chart of a method for efficiently extracting vanadium, molybdenum and nickel from polymetallic vanadium shale. Specific implementation method:
[0016] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0017] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art. The vanadium shales in the following examples were all crushed and passed through a 80-100 mesh sieve.
[0018] Example 1
[0019] The composition of a polymetallic vanadium shale is: 0.69% vanadium, 0.12% molybdenum, and 0.46% nickel. The following steps are used to separate vanadium, molybdenum, and nickel from vanadium shale. The specific steps are as follows:
[0020] (1) 50 g of neutralized slag produced by neutralizing vanadium shale with acid leaching solution and 50 g of vanadium shale are used to form an acid leaching material, 80 g of sulfuric acid aqueous solution and 3.0 g of fluorite are added to the acid leaching material and mixed evenly, the mass of sulfuric acid in the sulfuric acid aqueous solution is 20 g, the mass of clean water is 60 g, and then 10 g of hydrogen peroxide (mass concentration is 30%) is added, and the mixture is heated to 95° C. for acid leaching reaction for 8 hours to leach vanadium and nickel in the vanadium shale. After the reaction is completed, 0.3 g of citric acid is added, and the reaction is continued for 16 hours. The obtained mixed solution is separated into solid and liquid to obtain an acid leaching solution and an acid leaching slag, and the pH value of the acid leaching solution is 1.0;
[0021] (2) neutralizing the acid leaching solution obtained in step (1) to a pH of 1.8 with vanadium shale, filtering and separating without water washing to obtain an acid solution containing vanadium / molybdenum / nickel for subsequent use, and a neutralized slag containing 15 g of the acid leaching solution;
[0022] (3) The neutralized slag entrained with the acid leaching solution obtained in step (2) is returned to the acid leaching process in step (1) for acid leaching.
[0023] After the polymetallic vanadium shale is treated by the above steps, the leaching rates of vanadium, molybdenum and nickel are 90.5%, 88.2% and 95.63% respectively. The total acid consumption is 20% of the mass of the vanadium shale. The present invention achieves efficient separation of vanadium, molybdenum and nickel in vanadium shale under low acid consumption.
[0024] Example 2
[0025] The composition of a polymetallic vanadium shale is: 0.62% vanadium, 0.10% molybdenum, and 0.42% nickel. The following steps are used to separate vanadium, molybdenum, and nickel from vanadium shale. The specific steps are as follows:
[0026] (1) 45g of neutralized slag produced by neutralizing vanadium shale with acid leaching solution and 55g of fresh vanadium shale are used to form acid leaching materials. 85g of sulfuric acid aqueous solution and 2.0g of fluorite are added to the acid leaching materials. The mass of sulfuric acid in the sulfuric acid aqueous solution is 25g, and the mass of clean water is 60g. 12g of hydrogen peroxide (mass concentration is 30%) is added, and the acid leaching reaction is heated to 90°C for 8 hours to leach vanadium and nickel in the vanadium shale. After the reaction is completed, 0.2g of citric acid is added, and the reaction is continued for 16 hours. The obtained mixed solution is separated into solid and liquid to obtain acid leaching solution and acid leaching residue. The pH of the acid leaching solution is 0.8;
[0027] (2) neutralizing the acid leaching solution obtained in step (1) to a pH of 1.5 with vanadium shale ore powder, filtering and separating without water washing to obtain an acid solution containing vanadium / molybdenum / nickel for subsequent use, and a neutralized slag containing 13 g of the acid leaching solution;
[0028] (3) The neutralized slag entrained with the acid leaching solution obtained in step (2) is returned to the acid leaching process in step (1) for acid leaching.
[0029] After the polymetallic vanadium shale is treated by the above steps, the leaching rates of vanadium, molybdenum and nickel are 92.5%, 89% and 96.62% respectively. The total acid consumption is 25% of the mass of the vanadium shale. The present invention achieves efficient separation of vanadium, molybdenum and nickel in vanadium shale under low acid consumption.
[0030] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for efficiently extracting vanadium, molybdenum and nickel from polymetallic vanadium shale, characterized in that: The steps include: (1) Using vanadium shale and the neutralized slag produced by neutralizing the acid leaching liquid with the vanadium shale as the acid leaching material, the mass ratio of the neutralized slag produced by neutralizing the vanadium shale and the acid leaching liquid is 1-1.2:1, adding sulfuric acid aqueous solution and fluorite to the acid leaching material and mixing them evenly, the mass ratio of sulfuric acid aqueous solution to the acid leaching material is 0.8-1:1, the sulfuric acid in the sulfuric acid aqueous solution is 20-25wt% of the mass of the acid leaching material, and the fluorite is 2.0-3.0wt% of the mass of the acid leaching material, and then adding hydrogen peroxide, the mass concentration of hydrogen peroxide is 25%-35%, and the hydrogen peroxide is 10-12wt% of the mass of the acid leaching material, heating to 90° C.-95° C. for acid leaching reaction for 6-10 hours, so that vanadium and nickel in the vanadium shale are leached, after the acid leaching reaction is completed, adding citric acid, the citric acid is 0.2-0.3wt% of the mass of the acid leaching material, and continuing the reaction for 14-18 hours, and separating the obtained mixed solution into solid-liquid to obtain acid leaching liquid and acid leaching slag; (2) taking vanadium shale and neutralizing the acid leaching solution obtained in step (1) to a pH of 1.5 to 1.8, filtering and separating, and obtaining an acid solution containing vanadium / molybdenum / nickel for subsequent use in extracting vanadium, molybdenum and nickel, as well as neutralizing slag produced by neutralizing the acid leaching solution; (3) The neutralized slag produced by the neutralized acid leaching solution obtained in step (2) is returned to the acid leaching process in step (1) and mixed with the vanadium shale as an acid leaching material for acid leaching.
2. The method according to claim 1, characterized in that After the acid leaching reaction in step (1) is completed, the pH value of the acid leaching system is 0.6-0.8, citric acid is added, and the reaction is continued for 14-18 hours. The pH value of the acid leaching liquid obtained by solid-liquid separation is 0.8-1.0.
Citation Information
Patent Citations
Process for separating molybdenum and nickel form black shale containing molybdenum and nickel
CN101289702A
Method for extracting nickel and molybdenum from nickel-molybdenum symbiotic ore by low-concentration composite acid and oxidizing agent
CN101906538A
Method for extracting vanadium through neutralization of pulverized fuel ash acid leached liquor
CN104131181A
Production process for extracting elements such as aluminum, vanadium, molybdenum and nickel from black shale
CN104152687A
Method for recovering valuable metals from waste chemical catalyst
CN112342389A