A green and environmentally friendly low-rank coal flotation nanoparticle collector and preparation method

By using lignosulfonate-based polymer nanospheres prepared from wheat and sedge as collectors, the problems of low efficiency and environmental pollution of traditional low-rank coal flotation have been solved, and efficient and environmentally friendly low-rank coal flotation has been achieved. Choose recycling, and the raw materials are renewable and low cost.

CN115487943BActive Publication Date: 2024-10-11JIANGSU VOCATIONAL & TECHNICAL UNIVERSITY OF ARCHITECTURE
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211188684.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-28
Publication Date
2024-10-11
Estimated Expiration
2042-09-28

AI Technical Summary

Technical Problem

Traditional low-rank coal flotation collectors consume a lot of collectors and have low efficiency, and the raw materials are non-renewable, which affects the environment. Existing nanomaterial applications have not yet used environmentally friendly renewable materials as raw materials.

Method used

Using wheat crops and sedge as raw materials, lignosulfonate-based polymers are prepared through sulfate pulping method to form hollow spherical nanospheres, which are combined with ethanol to form a colloidal solution, which can be used for low-rank coal flotation to improve the stability of coal particles. Hydrophobicity and flotation efficiency.

Benefits of technology

It achieves efficient flotation recovery of low-rank coal, reduces raw material costs, and the raw materials and products are green, environmentally friendly and degradable, with good dispersion and ultra-long-term stability, improving flotation efficiency and environmental friendliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115487943B_ABST
    Figure CN115487943B_ABST
Patent Text Reader

Abstract

The invention discloses a green and environmentally friendly low-rank coal flotation nanoparticle collector and a preparation method, belonging to the field of mineral flotation technology. The nanoparticles are hollow nanospheres of lignin sulfonate-based polymers with phenolic hydroxyl groups, carboxyl groups and methoxy groups on their surfaces. The biomass is crushed and dried, and crude sodium lignin sulfonate is obtained by acid precipitation. Then, the obtained crude sodium lignin sulfonate is dissolved in water, the pH of the solution is adjusted, and the reaction solution is heated to 70°C. At this time, C6H 12 Br2 and trace amounts of KI, after polymerization, remove excess C6H 12 Br2 and filter; take the filtrate and desalt it, freeze-dry the filtered solid to obtain a yellow-brown lignin sulfonate-based polymer product; dissolve the lignin sulfonate-based polymer product in water to prepare a lignin sulfonate-based polymer solution, then add ethanol to the lignin sulfonate-based polymer to form a mixed solution and stir to obtain a colloidal solution containing lignin sulfonate-based polymer hollow nanospheres. It is simple to prepare, has good use effect and low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mineral flotation, and relates to a method for preparing a green and environmentally friendly collector, and in particular to a green and environmentally friendly low-rank coal flotation nanoparticle collector and a preparation method thereof. Background Art

[0002] my country has abundant low-rank coal resources and large reserves. Low-rank coal has a low degree of metamorphism, many oxygen-containing functional groups on the surface, developed pores, and poor floatability. If traditional reagents are used for flotation, the consumption is large and the efficiency is low, which is the main technical bottleneck for the clean utilization of low-rank coal. Therefore, many scholars are committed to developing efficient low-rank coal flotation collectors.

[0003] In recent years, nanotechnology has developed rapidly, and nanomaterials have been widely used in many fields. Compared with traditional materials, nanomaterials are mainly characterized by large specific surface area and good adsorption performance. In the flotation of fine-grained minerals, some scholars choose to use nanoparticles as collectors for exploration. This is mainly based on two considerations. On the one hand, nanoparticles can directly change the hydrophobicity of the mineral surface; on the other hand, nanoparticles can construct nano-scale rough structures on the mineral surface to change the hydrophobicity and improve the flotation efficiency of minerals. For example, Chinese patent publication CN106699951A discloses a nanoparticle collector for low-rank coal flotation and a preparation method, Chinese patent publication number CN108855626B discloses a coal slime flotation collector containing nanoparticles and a preparation method, and Chinese patent publication number CN108672098B discloses a coal slime flotation microemulsion collector containing nanoparticles and a preparation method.

[0004] The raw materials used in the above research are chemical products, which are non-renewable resources, not only expensive, but also prone to environmental problems. It has not been reported that environmentally friendly renewable materials are used as raw materials to prepare functionalized nanoparticle collectors. The present invention uses wheat crops and sedge as raw materials to prepare functional lignin nanoparticles for the flotation of low-rank coal, which can realize the flotation recovery of low-rank coal and the comprehensive utilization of biomass resources. Summary of the invention

[0005] In view of the shortcomings of the existing technology, a green and environmentally friendly low-rank coal flotation nanoparticle collector and a preparation method are provided, which can change the floatability of coal particles and improve the flotation efficiency.

[0006] To achieve the above technical objectives, the present invention provides a green and environmentally friendly low-rank coal flotation nanoparticle collector, comprising a colloidal solution and lignin sulfonate-based polymer hollow nanospheres, wherein the colloidal solution comprises water and ethanol, the mass ratio of water to ethanol is 10% and 90%, and the concentration of lignin sulfonate-based polymer hollow nanospheres and the colloidal solution is 0.05 mg / ml.

[0007] Furthermore, the ratio of the number of phenolic hydroxyl groups, carboxyl groups and methoxyl functional groups on the surface of the lignin sulfonate-based polymer hollow nanospheres is 6:5:5.

[0008] Furthermore, the lignin sulfonate-based polymer hollow nanospheres are in the shape of hollow spheres, and the hollow ratio thereof is 23%.

[0009] Furthermore, the particle size of the lignin sulfonate-based polymer hollow nanospheres is 80-200 nm.

[0010] Furthermore, the surface oxygen content of the lignin sulfonate-based polymer hollow nanospheres is 4%-8%.

[0011] A method for preparing a green and environmentally friendly low-rank coal flotation nanoparticle collector, the steps of which are as follows:

[0012] S1. Preparation of lignin: wheat straw and sedge as biomass are crushed and dried, and the biomass is prepared into forage black liquor by a kraft pulping method; then concentrated sulfuric acid is added to the forage black liquor for stirring, wherein the mass ratio of the forage black liquor to the concentrated sulfuric acid is 10:1; after the stirring is completed, 60% lime milk is added to the stirred solution, and the mass ratio of the forage black liquor to the lime milk is 6:1; continue to stir evenly to generate a precipitate, filter to obtain the precipitate, then add 5%-10% dilute sulfuric acid to the precipitate to dissolve it, and the mass ratio of the precipitate to the dilute sulfuric acid is 1:10-1:5, and sodium carbonate powder is added to the dilute sulfuric acid solution to convert it into sodium lignin sulfonate; finally, the obtained solution is concentrated and dried to obtain crude sodium lignin sulfonate powder;

[0013] S2. Synthesis of sodium lignin sulfonate polymer: Dissolve crude sodium lignin sulfonate powder in water to prepare a sodium lignin sulfonate solution with a concentration of 200 g / L, and use sodium hydroxide solution to adjust the pH value of the sodium lignin sulfonate solution; after heating the sodium lignin sulfonate solution to 70° C., add hexamethylene dibromide C 6 H 12 Br 2 And a trace amount of potassium iodide KI, in which the sodium lignin sulfonate solution and C 6 H 12 Br 2 The mass ratio of KI is 4:1 to 3:1, and the amount of KI added is 1:500 to 1:600 ​​according to the mass of the sodium lignin sulfonate solution; after 8 hours of polymerization, the excess C is removed by extraction with hexahexane. 6 H 12 Br 2 and filter; taking the filtrate, diluting the filtrate to 0.15 g / ml and then desalting with an ion exchange resin, and freeze-drying the filtered solid to obtain a yellow-brown lignin sulfonate-based polymer product;

[0014] S3. Preparation of hollow nanospheres: dissolving a lignin sulfonate-based polymer product in water to prepare a lignin sulfonate-based polymer solution, then adding ethanol to the lignin sulfonate-based polymer to form a mixed solution, and finally stirring the mixed solution for 3 hours to obtain a colloidal solution containing lignin sulfonate-based polymer hollow nanospheres.

[0015] Furthermore, in step S1, concentrated sulfuric acid with a concentration of 98% is added to the forage black liquor and stirred for 5 hours.

[0016] Furthermore, in step S2, the pH value of the sodium lignin sulfonate solution is adjusted to 11 using a sodium hydroxide solution; and the concentration of the lignin sulfonate-based polymer solution prepared in step S3 is 0.5 mg / mL.

[0017] Furthermore, the mass ratio of ethanol added to the lignin sulfonate-based polymer to water in the solution was 9:1.

[0018] A green and environmentally friendly low-rank coal flotation nanoparticle collector flotation application: monodisperse spherical hollow lignin nanoparticle collector is added at a ratio of more than 5kg / t and low-rank coal is flotated. At this time, the lignin sulfonate-based polymer hollow nanospheres can selectively adsorb with the oxygen-containing functional groups on the surface of the low-rank coal, and form a nano-scale rough structure on the surface of the low-rank coal, greatly enhancing the hydrophobicity of the low-rank coal surface, thereby effectively improving the clean coal flotation efficiency of the low-rank coal. The beneficial effects of the present invention are:

[0019] The present invention adopts a cross-linking polymerization method to synthesize lignin nanoparticles. The raw materials are wheat straw and sedge, which are rich in sources and low in price, and the raw materials and products are green, environmentally friendly and degradable, with little impact on the environment. The preparation method of the present invention has a simple process and mild conditions, which is convenient for the scale-up production of the preparation process. The prepared nanoparticles have phenolic hydroxyl, carboxyl and methoxy lignin sulfonate-based polymer hollow nanospheres on the surface, which have the characteristics of good dispersibility, ultra-long-term stability and controllable size. Compared with traditional hydrocarbon oil collectors, nanoparticle collectors have better dispersibility, and at the same time have functionalized groups on the surface, which can selectively adsorb with the surface of low-rank coal, have high surface modification efficiency, and can form nano-scale rough structures on the surface of coal particles, enhance the surface hydrophobicity of coal particles by increasing the surface roughness, and improve the flotation index. The preparation method of the nanoparticle collector of the present invention has the advantages of simple process, simple operation and easy control. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of preparing nanoparticle collector by the cross-linking polymerization method of the present invention. DETAILED DESCRIPTION

[0021] The present invention will be further described below in conjunction with the embodiments.

[0022] Example

[0023] like Figure 1 As shown, a green and environmentally friendly low-rank coal flotation nanoparticle collector of the present invention includes a colloidal solution and lignin sulfonate-based polymer hollow nanospheres, wherein the colloidal solution includes water and ethanol, the mass ratio of water to ethanol is 10% and 90%, the concentration of the lignin sulfonate-based polymer hollow nanospheres and the colloidal solution is 0.05 mg / ml, the number ratio of phenolic hydroxyl, carboxyl and methoxy functional groups on the surface of the lignin sulfonate-based polymer hollow nanospheres is 6:5:5, the shape of the lignin sulfonate-based polymer hollow nanospheres is hollow spherical, and the hollow ratio is 23%, the particle size of the lignin sulfonate-based polymer hollow nanospheres is 80-200nm, and the surface oxygen content of the lignin sulfonate-based polymer hollow nanospheres is 4%-8%.

[0024] A method for preparing a green and environmentally friendly low-rank coal flotation nanoparticle collector, the steps of which are as follows:

[0025] S1. Preparation of lignin: First, wheat straw and sedge are crushed and dried, and a sulfate pulping method is used to obtain forage black liquor; then, concentrated sulfuric acid with a concentration of 98% is added to the forage black liquor and stirred for 5 hours (the mass ratio of forage black liquor to concentrated sulfuric acid is 10:1); after the stirring is completed, lime milk with a concentration of 60% is added (the mass ratio of forage black liquor to lime milk is 6:1): after stirring, a precipitate is generated, and the precipitate is obtained by filtration, and then 5%-10% dilute sulfuric acid is added to the precipitate to dissolve it (the mass ratio of the precipitate to the dilute sulfuric acid is 1:10-1:5), and sodium carbonate powder is added to the dilute sulfuric acid solution to convert it into sodium lignin sulfonate; finally, the obtained solution is concentrated and dried to obtain crude sodium lignin sulfonate powder.

[0026] S2. Synthesis of sodium lignin sulfonate polymer: Dissolve crude sodium lignin sulfonate powder in water to prepare a sodium lignin sulfonate solution with a concentration of 200 g / L, and adjust the pH value of the sodium lignin sulfonate solution to 11 using sodium hydroxide solution; after heating the sodium lignin sulfonate solution to 70°C, add C 6 H 12 Br 2 (Sodium lignin sulfonate solution and C 6 H 12 Br 2 The mass ratio of sodium lignin sulfonate solution to KI is 4:1 to 3:1) and a trace amount of KI (the mass ratio of sodium lignin sulfonate solution to KI is 500:1 to 600:1); after polymerization for 8 hours, the excess C is removed by extraction with hexahexane. 6 H 12 Br 2and filter; taking the filtrate, diluting the filtrate to 0.15 g / ml and desalting with ion exchange resin, and freeze-drying the filtered solid to obtain a yellow-brown lignin sulfonate-based polymer product.

[0027] S3. Preparation of hollow nanospheres: dissolving the lignin sulfonate-based polymer product in water to prepare a 0.5 mg / mL lignin sulfonate-based polymer solution, then adding ethanol to the lignin sulfonate-based polymer to dilute it into a 0.05 mg / ml mixed solution, and finally stirring the mixed solution for 3 hours to obtain a colloidal solution containing lignin sulfonate-based polymer hollow nanospheres.

[0028] S4. Flotation test: The pure coal flotation test uses a 0.5LXFD hanging tank flotation machine with a spindle speed of 1800r / min. Weigh 40g of coal sample and pour it into a flotation tank filled with ultrapure water. Add nanoparticle collector at a dosage of 5kg / t~10kg / t and stir for 3min. Add frother (octanol) at a dosage of 200g / t. After stirring for 30s, pass gas to scrape and bubble for 3min. Filter, dry and weigh the scraped and residual samples at the bottom of the tank to obtain the product ash content and combustible body recovery rate. In addition, the same dose of diesel was selected as the collector, and other test conditions were the same for a control test. The test results are shown in the following table:

[0029] Table 1 Test results

[0030]

[0031]

[0032] As can be seen from Table 1, the flotation recovery rate of the nanoparticle collector of the present invention is significantly higher than that of diesel, which reflects the good recovery ability of the nanoparticle collector of the present invention for low-rank coal. As the dosage of the nanoparticle collector increases, the flotation recovery rate also increases. When the dosage of the agent is 8kg / t, the flotation recovery rate reaches 78.92%, and the flotation recovery rate increased by increasing the dosage of the collector is very small. Therefore, the nanoparticle collector of the present invention is more suitable for flotation of low-rank coal at a dosage of 8kg / t.

[0033] The above descriptions are only some embodiments of the present invention and do not limit the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a green and environmentally friendly low-rank coal flotation nanoparticle collector, characterized in that: The green and environmentally friendly low-rank coal flotation nanoparticle collector comprises a colloidal solution and lignin sulfonate-based polymer hollow nanospheres, wherein the colloidal solution comprises water and ethanol, the mass ratio of water to ethanol is 10% and 90%, and the concentration of the lignin sulfonate-based polymer hollow nanospheres and the colloidal solution is 0.05 mg / ml; The preparation method steps are as follows: S1. Preparation of lignin: crush and dry wheat straw and sedge as biomass, and prepare the biomass into forage black liquor by kraft pulping; then add concentrated sulfuric acid to the forage black liquor for stirring, wherein the mass ratio of the forage black liquor to the concentrated sulfuric acid is 10:1; after the stirring is completed, add 60% lime milk to the stirred solution, and the mass ratio of the forage black liquor to the lime milk is 6:1; continue to stir evenly to generate a precipitate, filter to obtain the precipitate, then add 5%-10% dilute sulfuric acid to the precipitate to dissolve it, and the mass ratio of the precipitate to the dilute sulfuric acid is 1:10~1:5, and add sodium carbonate powder to the dilute sulfuric acid solution to convert it into sodium lignin sulfonate; finally, concentrate and dry the obtained solution to obtain crude sodium lignin sulfonate powder; S2. Synthesis of sodium lignin sulfonate polymer: Dissolve crude sodium lignin sulfonate powder in water to prepare a sodium lignin sulfonate solution with a concentration of 200 g / L, and use sodium hydroxide solution to adjust the pH value of the sodium lignin sulfonate solution; after heating the sodium lignin sulfonate solution to 70°C, add hexamethylene dibromide (C6H 12 Br2 and trace amounts of potassium iodide KI, in which the sodium lignin sulfonate solution and C6H 12 The mass ratio of Br2 is 4:1~3:1, and the amount of KI added is 1:500~1:600 ​​according to the mass of sodium lignin sulfonate solution; after 8 hours of polymerization, the excess C6H 12 Br2 and filter; take the filtrate, dilute the filtrate to 0.15g / ml and desalt with ion exchange resin, and freeze-dry the filtered solid to obtain a yellow-brown lignin sulfonate-based polymer product; S3. Preparation of hollow nanospheres: dissolving a lignin sulfonate-based polymer product in water to prepare a lignin sulfonate-based polymer solution, then adding ethanol to the lignin sulfonate-based polymer to form a mixed solution, and finally stirring the mixed solution for 3 hours to obtain a colloidal solution containing lignin sulfonate-based polymer hollow nanospheres.

2. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: The ratio of the number of phenolic hydroxyl groups, carboxyl groups and methoxyl functional groups on the surface of the lignin sulfonate-based polymer hollow nanospheres is 6:5:

5.

3. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: The lignin sulfonate-based polymer hollow nanospheres are in the shape of hollow spheres, and the hollow ratio thereof is 23%.

4. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: The particle size of the lignin sulfonate-based polymer hollow nanospheres is 80-200 nm.

5. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: The surface oxygen content of the lignin sulfonate-based polymer hollow nanospheres is 4%-8%.

6. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: In step S1, concentrated sulfuric acid with a concentration of 98% is added to the forage black liquor and stirred for 5 hours.

7. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: In step S2, the pH value of the sodium lignin sulfonate solution is adjusted to 11 using a sodium hydroxide solution.

8. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: The concentration of the lignin sulfonate-based polymer solution prepared in step S3 is 0.5 mg / mL; the mass ratio of ethanol added to the lignin sulfonate-based polymer to water in the solution is 9:

1.

9. The method for preparing the green and environmentally friendly low-rank coal flotation nanoparticle collector according to claim 1, characterized in that: The monodisperse spherical hollow lignin nanoparticle collector is added at a ratio of more than 5kg / t and low-rank coal is floated. At this time, the lignin sulfonate-based polymer hollow nanospheres can selectively adsorb to the oxygen-containing functional groups on the surface of the low-rank coal and form a nanoscale rough structure on the surface of the low-rank coal, greatly enhancing the hydrophobicity of the low-rank coal surface, thereby effectively improving the clean coal flotation efficiency of the low-rank coal.

Citation Information

Patent Citations

  • Nano-particle collecting agent for low-rank coal floatation and preparation method

    CN106699951A

  • A coal slime flotation microemulsion collector containing nanoparticles and its preparation method

    CN108672098B

  • A coal slime flotation collector containing nanoparticles and its preparation method

    CN108855626B

  • Method for preparing amphiphilic lignin nanoparticle based on pulping black liquor, amphiphilic lignin nanoparticle, and oil sludge detergent

    AU2020103382A4

  • Coal flotation agent and preparation method thereof

    CN103394416A