Continuous casting method and continuous casting billet for improving the hardness distribution of rail head section

By using electromagnetic stirring technology to regulate the solute element concentration at the casting billet during continuous casting of rails, the problem of uneven hardness distribution of rail heads is solved, and the fatigue performance and service life of the rail are improved.

CN115502347BActive Publication Date: 2024-11-01PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211172004.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-26
Publication Date
2024-11-01
Estimated Expiration
2042-09-26

AI Technical Summary

Technical Problem

The existing technology has failed to effectively solve the problem of uneven distribution of hardness in the cross-section of rail heads, which affects the fatigue performance and service life of rails.

Method used

The crystallizer electromagnetic stirring, second-cold electromagnetic stirring and solidified end electromagnetic stirring technology are adopted to control the magnetic field strength and stirring position, so as to adjust the concentration and hardness distribution of solute elements at the cross-section of the casting billet to achieve uniformity of the cross-sectional hardness of the rail head.

Benefits of technology

By systematically controlling the macrosolute concentration of the casting billet section and combining with the heat treatment process, continuous casting control of the hardness distribution of the rail head section is achieved, the comprehensive mechanical properties and reliability of the rail are improved, and the hardness requirements of the high-end market are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115502347B_ABST
    Figure CN115502347B_ABST
Patent Text Reader

Abstract

The present invention discloses a continuous casting method and continuous casting billet for improving the hardness distribution of the rail head section, comprising electromagnetic stirring of a crystallizer, electromagnetic stirring of secondary cooling and electromagnetic stirring of the solidification end, wherein the central magnetic field strength of the stirring coil of the crystallizer electromagnetic stirring is 0-350×10 ‑4 T; the magnetic field strength of the stirring coil of the secondary cooling electromagnetic stirring is 0 to 300 × 10 ‑4 T; the central magnetic field strength of the stirring coil of the electromagnetic stirring at the end of solidification is 0 to 400×10 ‑4 T. The continuous casting method for improving the hardness distribution of the rail head section provided by the present invention innovatively starts from the continuous casting stage and solves the hardness distribution problem of the rail head section in advance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgical production, and in particular to a continuous casting method and a continuous casting billet for improving the hardness distribution of a rail head section. Background Art

[0002] As the main component of railway transportation construction, rails play an important role. On the one hand, they guide the train forward, and on the other hand, they bear the huge load of the train. Therefore, the quality of rails has an important impact on driving safety. In addition, with the continuous development of railway transportation, the transportation of passenger, high-speed and heavy-load freight has put forward higher requirements on the quality and performance of rails. The service performance of rails greatly determines the service life of rails and their maintenance costs.

[0003] It is necessary to improve the quality and performance of existing products and develop new high-performance products. Many scholars at home and abroad have carried out a lot of research. For example, many researchers have conducted in-depth research on the fatigue damage of rails. Their research usually homogenizes the hardness inside the rails, but actual product testing finds that the hardness inside the rails is not uniform. In addition, some scholars have pointed out that hardness is a very important influencing factor on the fatigue damage of rails. The researchers measured the cross-sectional hardness of rail heads of different varieties of rails, and the results showed that the cross-sectional hardness of the rail head gradually decreases from the surface to the inside. In addition, ASITHAC.ATHUKORALA studied the non-uniform hardness distribution, metallurgy and ratcheting behavior of Australian AS60HH rail steel. The results showed that the non-uniformity of the material will affect the ratcheting effect of the rail as the wear progresses, thereby affecting the service life of the rail.

[0004] Therefore, studying the distribution and control of rail hardness is of great significance to improving rail performance. Reducing the hardness gradient inside the rail head can reduce the difference in results produced by hardness homogenization research. Even for materials with small gradient hardness, the research within a smaller area can be simplified to hardness uniformity, thereby achieving the purpose of simplifying the research. For steel materials, the uniformity of organizational properties is a very important quality indicator. A large gradient of organizational properties will greatly weaken the comprehensive mechanical properties of the material, thereby reducing the reliability of the material performance.

[0005] A large number of scholars have conducted research on the hardness of steel, but most of them focus on heat treatment process research, analysis of the causes of incompatibility between hardness and structure, and the impact of hardness on other application performances. However, research on continuous casting control technology for the cross-sectional hardness distribution of heavy rail head has not yet been involved.

[0006] Based on this, the existing technology still needs to be improved. Summary of the invention

[0007] The main purpose of the present invention is to provide a continuous casting method and a continuous casting billet for improving the hardness distribution of the cross section of the rail head of a steel rail, so as to solve the problem of the hardness distribution of the cross section of the heavy rail head from the continuous casting stage.

[0008] According to one aspect of the present invention, a continuous casting method for improving the hardness distribution of the rail head section is provided, comprising electromagnetic stirring of the crystallizer, electromagnetic stirring of the secondary cooling and electromagnetic stirring of the solidification end, wherein the central magnetic field strength of the stirring coil of the crystallizer electromagnetic stirring is 0 to 350×10 -4 T; the magnetic field strength of the stirring coil of the secondary cooling electromagnetic stirring is 0 to 300 × 10 -4 T; the central magnetic field strength of the stirring coil of the electromagnetic stirring at the end of solidification is 0 to 400×10 -4 T;

[0009] In addition, in order to comprehensively coordinate the reasonable distribution of solute element concentration (mass percentage) in the cross section of the ingot and control the central segregation, the total magnetic field intensity of the electromagnetic stirring in operation must be controlled within 400×10 -4 ~750×10 -4 T.

[0010] In some embodiments, the assembly position of the secondary cooling electromagnetic stirring is a region 4000 to 5000 mm away from the liquid surface of the crystallizer.

[0011] In some embodiments, the assembly position of the electromagnetic stirring at the end of solidification is a region 8000 to 10000 mm away from the liquid surface of the crystallizer.

[0012] In some embodiments, the casting speed during the continuous casting process is 0.60-0.70 m / min.

[0013] In some embodiments, the secondary cooling water ratio of the continuous casting secondary cooling is 0.27-0.47 L / kg steel.

[0014] In some embodiments, the cross section of the continuous casting is 280 mm×380 mm.

[0015] In some embodiments, the parameters of continuous casting are controlled based on the macroscopic solute concentration distribution of key alloying elements in the cross section of the ingot during continuous casting, the macroscopic solute concentration distribution of key alloying elements in the centerline height direction of the rail, the correspondence between the solidification structure of the ingot and the trace area of ​​the solidification structure left on the rail, and the evolution law of the hardness in the centerline height direction of the rail.

[0016] In some embodiments, the key alloying elements include carbon, silicon, and manganese, among which carbon has a more significant effect on the hardness of the rail. In the present invention, carbon is taken as a representative to analyze the effect of continuous casting electromagnetic stirring control on the carbon mass percentage control and its specific effect on the hardness of the rail section.

[0017] In some embodiments, the solidified structure of the ingot is successively fine grain (equiaxed grain) structure of the quench layer, columnar grains, mixed grains, and equiaxed grains from the surface of the ingot to the center of the ingot.

[0018] On the other hand, an embodiment of the present invention further discloses a heavy rail steel continuous casting billet, which is produced by the above-mentioned continuous casting method.

[0019] By adopting the above technical solution, the present invention has at least the following beneficial effects:

[0020] The continuous casting method for improving the hardness distribution of the rail head section provided by the present invention innovatively solves the hardness distribution problem of the rail head section from the continuous casting stage. Aiming at the evolution and distribution law of the hardness of the heavy rail head section, on the basis of mastering its corresponding relationship with the solute concentration in the macroscopic region of the ingot and the migration of the macroscopic region of the rolling, the macroscopic solute concentration of the ingot section is systematically regulated, and matched with a general heat treatment process, the continuous casting regulation of the hardness distribution of the heavy rail head section is realized, providing continuous casting technical support for the control of rail performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The invention shows the detection and result of macro segregation of the ingot disclosed in one embodiment of the invention;

[0023] Figure 2 The invention shows the rail macro segregation detection and results disclosed in one embodiment of the invention;

[0024] Figure 3 The figure shows the hardness test result of the rail head section disclosed in one embodiment of the present invention;

[0025] Figure 4 The invention shows the detection and result of macro segregation of the ingot disclosed in one embodiment of the invention;

[0026] Figure 5 The invention shows the rail macro segregation detection and results disclosed in one embodiment of the invention;

[0027] Figure 6 The figure shows the hardness test result of the rail head section disclosed in one embodiment of the present invention;

[0028] Figure 7The invention shows the detection and result of macro segregation of the ingot disclosed in one embodiment of the invention;

[0029] Figure 8 The invention shows the rail macro segregation detection and results disclosed in one embodiment of the invention;

[0030] Fig. 9 The figure shows the rail head cross-section hardness test and result disclosed in one embodiment of the present invention. DETAILED DESCRIPTION

[0031] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0032] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.

[0033] Some embodiments of the present invention disclose a continuous casting method for improving the hardness distribution of the rail head section, by mastering the evolution law of the macroscopic solute concentration distribution of key alloy elements in the cross section of the ingot, mastering the evolution law of the macroscopic solute concentration distribution of key alloy elements in the center line of the rail, mastering the corresponding relationship between the solidification structure of the ingot and the trace area of ​​the solidification structure left on the rail, and mastering the evolution law of the hardness distribution in the center line of the rail. For example, the magnetic field strength of the electromagnetic stirring coil of the crystallizer is 350×10 -4 T, the magnetic field strength at the center of the secondary cooling electromagnetic stirring coil is 0T, and the magnetic field strength at the center of the electromagnetic stirring coil at the end of solidification is 400×10 -4At T, the segregation degree of C element in the ingot (calculated by concentration, the concentration at a specific position divided by the average concentration) appears the first segregation trough point at 20 mm from the center of the narrow surface of the ingot, corresponding to the negative segregation point at the point where the rail is 5 mm away from the tread; at 80 mm from the center of the narrow surface of the ingot, the C segregation curve quickly changes from positive segregation to negative segregation, corresponding to the point where the rail is 20 mm away from the tread; further, under the action of electromagnetic stirring at the end of solidification (combined with the evolution law of the ingot shell, the end electromagnetic stirring curve is obtained The second trough point of the C element segregation curve was produced at 100mm from the center of the narrow face of the ingot according to the thickness of the ingot shell during stirring, which corresponds to the position of 30mm from the tread of the rail. Furthermore, according to the solidification structure zoning of the ingot, it can be obtained that the columnar crystal zone of the ingot ends at 45mm from the narrow face of the ingot, and the columnar crystal structure trace area on the rail ends at 10mm from the tread; while the equiaxed crystal zone of the ingot starts at 80mm from the center of the narrow face, and the corresponding equiaxed crystal trace area on the rail starts at 20mm from the tread of the rail. Therefore, combined with the position relationship of the characteristic points of the macro-segregation curve and the corresponding relationship of the solidification structure boundary, it can be obtained that the positions of 20mm, 45mm, 80mm, and 100mm from the center of the narrow surface of the ingot correspond to the positions of 5mm, 10mm, 20mm, and 30mm from the tread of the rail, respectively. The concentration of alloy elements at each position directly affects the hardness. Therefore, it can be seen that the distribution of solute concentration in the cross section of the ingot regulated by continuous casting must be inherited to the rail, resulting in the regulation of the macro-solute concentration at each position of the rail, and rails of different hardness states are obtained under the same heat treatment process conditions; then, the macro-solute concentration distribution of alloy elements in the cross section of the heavy rail steel ingot is changed by a multi-stage electromagnetic control technology that integrates electromagnetic stirring of the crystallizer, electromagnetic stirring of the secondary cooling, and electromagnetic stirring at the end of solidification; by adjusting the continuous casting pulling speed, the electromagnetic stirring action position is regulated to interactively and synergistically regulate the macro-solute concentration of alloy elements in the cross section of the ingot by the pulling speed and electromagnetic stirring; the continuous casting secondary cooling control is carried out, and the macro-solute diffusion control and micro-segregation control of the cross section of the ingot are comprehensively realized by regulating the secondary cooling intensity. This will enable fine-grained control of the macroscopic solute concentration of alloy elements in the ingot cross section, while taking into account high-level control of the microscopic segregation of the ingot, and ultimately achieve coordinated control of the cross-sectional hardness and microscopic (phase change) structure of the rail head after the ingot is rolled into a rail.

[0034] Among them, the key alloy elements include carbon and silicon. The solidification structure is the fine-grained structure of the quench layer, columnar crystals, mixed crystals, and equiaxed crystals from the surface of the ingot to the center of the ingot.

[0035] The present invention is mainly based on the analysis results of the genetic correspondence relationship of the key position points from the heavy rail steel ingot to the rail, based on the significant influence of the continuous casting electromagnetic stirring process on the macro-solute element concentration of the ingot cross section, combined with the key influence of the macro-solute element concentration on the hardness, and through the electromagnetic stirring parameters and the pulling speed, the target regulation of the macro-solute element concentration of the ingot cross section is achieved, and then the pre-intervention of the macro-solute element concentration of the rail cross section is achieved and the hardness regulation of the rail cross section is finally achieved. For example, when there is no electromagnetic stirring intervention, the macro-concentration of the cross-section solute elements of the resulting ingot changes slowly, and the homogeneity of the corresponding rail cross section solute elements is good, but the problem of cooling rate differences at different depths inevitably occurs during the heat treatment of the rail, which directly leads to the problem of the hardness gradient of the rail cross section. The present invention can adjust the solute concentration at different positions, which is an important supplement to the actual cooling rate regulation during heat treatment, and achieves the optimization regulation of the cross-section hardness gradient.

[0036] The specific process parameter requirements are mainly:

[0037] (1) Magnetic field strength at the center of the crystallizer electromagnetic stirring coil: 0~350×10 -4 T;

[0038] (2) Secondary cooling electromagnetic stirring: Installed in the area 4000-5000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 0-300×10 -4 T;

[0039] (3) Electromagnetic stirring at the end of solidification: Installed in the area 8000-10000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 0-400×10 -4 T;

[0040] (4) Continuous casting speed is generally controlled at 0.60-0.70 m / min;

[0041] (5) Secondary cooling for continuous casting: The water volume of the secondary cooling is controlled at 0.27-0.47 L / kg steel.

[0042] In addition, the total magnetic field intensity of electromagnetic stirring was controlled at 400×10 -4 ~750×10 -4 T.

[0043] In addition to the above-mentioned key process technology requirements, general technical parameters are also required for implementation, such as a continuous casting section of 280mm×380mm, a superheat of the molten steel during the casting process of 25-35°C, etc. The resulting ingot is heat treated using conventional rolling and cooling systems.

[0044] Implementation effect: A heavy rail product is used for export to a certain international high-end market. The technical agreement requires that the hardness of the rail at 30mm from the tread is ≥M and no other microstructures outside the pearlite are allowed in the area 0-30mm from the tread. Before the implementation of this technical invention, the operation process is: the magnetic field strength at the center of the crystallizer electromagnetic stirring coil is 500×10 -4 T, the electromagnetic stirring of the secondary cooling and the electromagnetic stirring at the end of solidification were not put into operation, that is, 0T was implemented; the continuous casting speed was controlled at 0.65-0.67m / min; the water volume of the secondary cooling of the continuous casting was controlled at 0.37L / kg 钢 . In addition to the above-mentioned key process technology requirements, general technical parameters are also required for implementation, such as the continuous casting section of 280mm×380mm, the superheat of the molten steel during the casting process of 25-35℃, etc. Under this process condition, a large positive segregation appeared in the area 40-80mm from the center of the narrow face of the ingot, among which the maximum value of the C segregation degree reached 1.08, and the maximum value of the C segregation degree in the area 9-20mm from the tread of the corresponding rail reached 1.07, and the C segregation degree at 30mm from the tread of the rail was 0.98. In order to meet the hardness of the rail 30mm away from the tread ≥M, after implementing a strong heat treatment process, the hardness of the rail 30mm away from the tread reached M+2HWB, but different degrees of martensitic structure appeared in the area 10-20mm away from the tread, and the rail did not meet the requirements of the technical agreement. After reducing the cooling intensity of the heat treatment, the rail could not meet the requirement of "hardness ≥M at 30mm away from the tread". Furthermore, by implementing the electromagnetic stirring control technology of the present invention: the magnetic field strength at the center of the crystallizer electromagnetic stirring coil is 200×10 -4 T, secondary cooling electromagnetic stirring 250×10 -4 T, electromagnetic stirring at the end of solidification 0T, the overall continuous casting speed is controlled at 0.65-0.67m / min; the overall water volume of the continuous casting secondary cooling is controlled at 0.37L / kg 钢 . In addition to the above key process technology requirements, general technical parameters are also required for implementation, such as continuous casting section 280mm×380mm, superheat of molten steel during casting 25~35℃, etc. Under this process condition, the maximum C segregation in the area 40~80mm from the center of the narrow face of the ingot is 1.03, and the maximum C segregation in the area 9~20mm from the tread of the corresponding rail is 1.03, and the C segregation at 30mm from the tread of the rail is 1.02. After the same heat treatment cooling process, the hardness of the rail at 30mm from the tread reaches M+4HWB, and the area 0~30mm from the tread of the rail is pearlite. In order to improve the hardness performance margin, after increasing the heat treatment cooling air pressure by 1kPa, the hardness of the rail at 30mm from the tread reaches M+8.5HWB on average, and the area 0~30mm from the tread of the rail is still pearlite, which meets the requirements of the technical agreement.

[0045] Example 1

[0046] This embodiment is a steel mill using the method of the present invention to continuously cast and produce large square billets of U75V heavy rail steel with a cross section of 280mm×380mm. The specific implementation of the present invention is as follows: (1) The magnetic field strength of the center of the electromagnetic stirring coil of the crystallizer is 350×10 - 4 T; (2) Second cooling electromagnetic stirring: installed in the area 4000-5000mm away from the liquid surface of the crystallizer, the magnetic field strength in the center of the stirring coil is 0T; (3) Electromagnetic stirring at the end of solidification: installed in the area 8000-10000mm away from the liquid surface of the crystallizer, the magnetic field strength in the center of the stirring coil is 400×10 -4 T; (4) Continuous casting speed, the overall control is 0.65 ~ 0.67m / min; (5) Continuous casting secondary cooling: the secondary cooling water volume is overall controlled at 0.37L / kg 钢 In addition to the above key process technology requirements, general technical parameters are also required for implementation, such as continuous casting section of 280mm×380mm, superheat of molten steel during casting of 25-35℃, etc. The resulting ingot is heat treated by conventional rolling and cooling system.

[0047] After the implementation of this technology, the segregation evolution and distribution of the typical alloying element C in the cross section of the produced ingots were tested, and the evolution and distribution of C segregation in the centerline rail height direction of the corresponding ingots were tested. The obtained rails were tested for the hardness of the iron standard A line (A1 to A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread, respectively), and the microstructure of the 5mm×5mm area at each hardness test point of the rails was further identified. The results are shown in the figure below. Figure 1 , Figure 2 , Figure 3 The test results show that after the ingot is rolled into rails, the macroscopic solute distribution of the cross section is consistent. The hardness of the rail is affected by the macroscopic solute concentration and the depth of the test position from the tread. The main manifestation is that the depth from the tread increases, the actual cooling rate of heat treatment decreases, the hardness is lower at higher solute concentrations, and the hardness value is even lower at lower solute concentrations. Further microstructure identification of the 5mm×5mm area of ​​each hardness test point of the rail shows that no abnormal structure appears in each area of ​​the rail.

[0048] Example 2

[0049] This embodiment is a steel mill using the method of the invention to continuously cast and produce large square billets of U75V heavy rail steel with a cross section of 280mm×380mm. The specific implementation of the technology of the invention is as follows: (1) The magnetic field strength at the center of the crystallizer electromagnetic stirring coil is 0T; (2) Secondary cooling electromagnetic stirring: installed in the area 4000-5000mm away from the crystallizer liquid surface, the magnetic field strength at the center of the stirring coil is 300×10 -4T; (3) Electromagnetic stirring at the end of solidification: installed in the area 8000-10000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 400×10 -4 T; (4) Continuous casting speed, the overall control is 0.60 ~ 0.63m / min; (5) Continuous casting secondary cooling: the secondary cooling water volume is overall controlled at 0.47L / kg 钢 In addition to the above key process technology requirements, general technical parameters are also required for implementation, such as continuous casting section of 280mm×380mm, superheat of molten steel during casting of 25-35℃, etc. The resulting ingot is heat treated by conventional rolling and cooling system.

[0050] After the implementation of this technology, the segregation evolution and distribution of the typical alloying element C in the cross section of the produced ingots were tested, and the evolution and distribution of C segregation in the centerline rail height direction of the corresponding ingots were tested. The obtained rails were tested for the hardness of the iron standard A line (A1 to A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread, respectively), and the microstructure of the 5mm×5mm area at each hardness test point of the rails was further identified. The results are shown in the figure below. Figure 4 , Figure 5 , Figure 6 The test results show that after the ingot is rolled into rails, the macroscopic solute distribution of the cross section is consistent. The hardness of the rail is affected by the macroscopic solute concentration and the depth of the test position from the tread. The main manifestation is that the depth from the tread increases, the actual cooling rate of heat treatment decreases, the hardness is lower at higher solute concentrations, and the hardness value is even lower at lower solute concentrations. Further microstructure identification of the 5mm×5mm area of ​​each hardness test point of the rail shows that no abnormal structure appears in each area of ​​the rail.

[0051] Example 3

[0052] This embodiment is a steel mill using the method of the invention to continuously cast and produce large square billets of U75V heavy rail steel with a cross section of 280mm×380mm. The specific implementation of the technology of the invention is as follows: (1) The magnetic field strength of the center of the electromagnetic stirring coil of the crystallizer is 200×10 - 4 T; (2) Secondary cooling electromagnetic stirring: installed in the area 4000-5000 mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 200×10 -4 T; (3) Electromagnetic stirring at the end of solidification: installed in the area 8000-10000mm away from the liquid surface of the crystallizer, the magnetic field strength at the center of the stirring coil is 0T; (4) Continuous casting speed, the overall control is 0.68-0.70m / min; (5) Secondary cooling of continuous casting: the water volume of secondary cooling is overall controlled at 0.27L / kg 钢In addition to the above key process technology requirements, general technical parameters are also required for implementation, such as continuous casting section of 280mm×380mm, superheat of molten steel during casting of 25-35℃, etc. The resulting ingot is heat treated by conventional rolling and cooling system.

[0053] After the implementation of this technology, the segregation evolution and distribution of the typical alloying element C in the cross section of the produced ingots were tested, and the evolution and distribution of C segregation in the centerline rail height direction of the corresponding ingots were tested. The obtained rails were tested for the hardness of the iron standard A line (A1 to A4 with a distance of 5mm, 10mm, 15mm, and 20mm from the tread, respectively), and the microstructure of the 5mm×5mm area at each hardness test point of the rails was further identified. The results are shown in the figure below. Figure 7 , Figure 8 , Fig. 9 The test results show that after the ingot is rolled into rails, the macroscopic solute distribution of the cross section is consistent. The hardness of the rail is affected by the macroscopic solute concentration and the depth of the test position from the tread. The main manifestation is that the depth from the tread increases, the actual cooling rate of heat treatment decreases, the hardness is lower at higher solute concentrations, and the hardness value is even lower at lower solute concentrations. Further microstructure identification of the 5mm×5mm area of ​​each hardness test point of the rail shows that no abnormal structure appears in each area of ​​the rail.

[0054] It is not convenient to give an exhaustive comparative description of each parameter here. The key points are exemplified as follows: When the magnetic field strength at the center of the electromagnetic stirring magnetic field coil of the crystallizer exceeds 350×10 -4 At T, the negative segregation at the point 5 mm away from the rail tread is more serious, and the hardness of this point will reach the lower limit of the standard or even be lower than the standard requirement; the magnetic field strength at the center of the secondary cooling electromagnetic stirring coil exceeds 300×10 -4 At T, the corresponding position of the ingot is prone to produce a white bright band structure with negative segregation, and a soft spot appears at about 20 mm from the tread of the corresponding rail, and the hardness is lower than the standard requirement; when the magnetic field intensity at the center of the electromagnetic stirring coil at the end of solidification exceeds 400×10 -4 At T, the segregation degree of the rail at a distance of 30 mm from the tread will reach 0.90 or below, which will drop sharply compared with the hardness at a distance of 25 mm from the tread, causing a sharp increase in the local hardness gradient.

[0055] Comparative Example

[0056] A domestic factory continuously casts large square billets of U75V, U71Mn and U78CrV heavy rail steel with a cross section of 280mm×380mm. The electromagnetic stirring coil of the crystallizer has a central magnetic field strength of 50×10 -4 ~60×10 -4 T, with the magnetic field strength of the secondary cooling electromagnetic stirring coil at the center of 200×10 -4~250×10 -4 The combined electromagnetic stirring of T and the implementation of strong secondary cooling to improve the macroscopic homogeneity have achieved the improvement of the macroscopic homogeneity of the rail head. The extreme difference of C segregation in the rail head area is controlled at 0.03-0.06. However, due to the influence of the heat transfer characteristics of the heat treatment, the hardness of the obtained rail decreases rapidly as it is farther away from the tread. Under large-scale production conditions on site, fluctuations in the reasonable range of the process will cause the hardness at the corresponding position to be lower than the standard requirement, that is, the hardness at a specific position is insufficient.

[0057] The continuous casting process control technology proposed in the present invention is further used to increase the electromagnetic stirring magnetic field strength of the crystallizer to 200×10 -4 T, while matching 270×10 -4 T's secondary cooling electromagnetic stirring, the rail head section C segregation extreme difference of the obtained rail reaches 0.05, while by increasing the macro solute concentration in the area 10-20mm away from the rail tread, the rail hardness surplus in the area is increased by 3HWB, which better meets the needs of on-site process fluctuations, and there is no situation below the standard requirements. That is, the technology of the present invention can achieve the improvement of cross-section homogeneity while further focusing on the specific requirements of rail quality, accurately distributing the solute concentration of the rail section, and realizing the pre-advanced regulation of rail performance.

[0058] The above implementation examples show that after adopting this technical invention, the macroscopic solute concentration distribution of the ingot cross section is differentially controlled, the macroscopic solute concentration distribution of the center line of the rail height direction changes accordingly, and the corresponding hardness distribution of the rail head cross section also changes accordingly. Under the same heat treatment process conditions, the microstructure of the rail hardness detection point is normal. This technology provides a new technical idea for the regulation of rail cross section hardness under specific heat treatment process conditions.

[0059] It should be particularly pointed out that the various components or steps in the above-mentioned embodiments can be cross-linked, replaced, added, or deleted with each other. Therefore, the combinations formed by these reasonable arrangements and combinations should also fall within the scope of protection of the present invention, and the scope of protection of the present invention should not be limited to the embodiments.

[0060] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is only for description and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope (including claims) disclosed in the embodiments of the present invention is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0061] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A continuous casting method for improving the hardness distribution of the rail head section, characterized in that: It includes electromagnetic stirring of the crystallizer, electromagnetic stirring of the secondary cooling and electromagnetic stirring of the solidification end, wherein the central magnetic field strength of the stirring coil of the crystallizer electromagnetic stirring is 0 to 350×10 -4 T; the magnetic field strength of the stirring coil center of the secondary cooling electromagnetic stirring is 0~300×10 -4 T; the central magnetic field strength of the stirring coil of the electromagnetic stirring at the end of solidification is 0~400×10 -4 T; In addition, the total magnetic field intensity of electromagnetic stirring was controlled at 400×10 -4 ~750×10 -4 T; The assembly position of the secondary cooling electromagnetic stirring is an area 4000-5000 mm away from the liquid surface of the crystallizer; the assembly position of the solidification end electromagnetic stirring is an area 8000-10000 mm away from the liquid surface of the crystallizer; The pulling speed during continuous casting is 0.60~0.70m / min; The specific water volume of the secondary cooling of continuous casting is 0.27~0.47L / kg steel; The cross section of continuous casting is 280mm×380mm; Based on the macroscopic solute concentration distribution of key alloying elements in the cross section of the ingot during continuous casting, the macroscopic solute concentration distribution of key alloying elements in the centerline height direction of the rail, the corresponding relationship between the solidification structure of the ingot and the trace area of ​​the solidification structure left on the rail, and the evolution law of the hardness in the centerline height direction of the rail, the continuous casting parameters are controlled; the superheat of the ladle steel liquid during the casting process is 25-35℃.

2. The continuous casting method for improving the hardness distribution of the rail head section according to claim 1, characterized in that: The key alloying elements include carbon, silicon and manganese.

3. The continuous casting method for improving the hardness distribution of the rail head section according to claim 1, characterized in that: The solidified structures are fine grain structures, columnar crystals, mixed crystals and equiaxed crystals of the chilled layer in sequence from the surface of the ingot to the center of the ingot.

4. A heavy rail steel continuous casting billet, characterized in that: It is made by the continuous casting method described in any one of claims 1 to 3.