LED epitaxial wafer and preparation method thereof

By growing the quantum well structure layer in stages and covering the V-shaped defects, the problem of reducing luminescence efficiency caused by lattice mismatch in long-wave LEDs is solved, and the luminescence efficiency of LEDs is significantly improved.

CN115513347BActive Publication Date: 2024-11-26MAANSHAN JASON SEMICON CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211113410.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-14
Publication Date
2024-11-26
Estimated Expiration
2042-09-14

AI Technical Summary

Technical Problem

When growing long-wave LEDs, V-shaped defects occur due to different sizes of InN and GaN, resulting in a decrease in the internal luminous efficiency of the quantum well.

Method used

By growing the quantum well structure layer in stages, first, the quantum well layer with low In content is grown slowly reduces the lattice mismatch, and then the quantum well layer with high In content is grown, and the V-shaped defect is covered by controlling the growth direction of the carrier disk to avoid it Influence the underlying structure.

Benefits of technology

The luminous efficiency of LED is effectively improved, and the problem of luminous efficiency decrease is solved by covering V-shaped defects, thus achieving the improvement of brightness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115513347B_ABST
    Figure CN115513347B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of semiconductor lighting technology, and provides an LED epitaxial wafer and a preparation method thereof. The preparation method provided by the present invention comprises the following steps: S1, purifying the substrate; S2, growing a non-doped gallium nitride layer on the substrate after high-temperature purification; S3, growing an N-type gallium nitride layer on the non-doped gallium nitride layer; S4, growing n quantum well light-emitting layers on the N-type gallium nitride layer; S5, growing an electron blocking layer Al on the quantum well light-emitting layer. x Ga 1‑x N; S6, in the electron blocking layer Al x Ga 1‑x The preparation method provided by the present invention can reduce the density and size of V-shaped defects in GaN-based LED quantum wells, and solve the problem of reduced luminous efficiency caused by V-shaped defects penetrating quantum wells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor lighting, and in particular to an LED epitaxial wafer and a preparation method thereof. Background Art

[0002] During the growth of light-emitting diodes, the growth of heterojunction interfaces determines the quality of the crystal. The luminous efficiency of light-emitting diodes depends on the internal quantum efficiency of the quantum well, which is closely related to the well barrier structure design, doping, and the density of V-type defects of the quantum well. What has a decisive influence on these is the treatment method of different substances at the interface. When growing long-wave LEDs, it is necessary to adjust the band gap width of the quantum well, and the doping amount of In must be increased. When increasing In doping, due to the different lattice sizes of InN and GaN, V-type defects will be generated, thereby reducing the internal luminous efficiency of the quantum well. V-type defects are more likely to be generated at the atomic steps of crystal growth, and the direction of the atomic steps is in one direction. This direction has a certain relationship with the lattice orientation of the substrate and the rotation direction of the carrier during the growth process.

[0003] Therefore, how to reduce the density of V-shaped defects during the crystal growth process, thereby improving the luminescence efficiency inside the quantum well, has become an urgent problem that technicians in this field need to solve. Summary of the invention

[0004] In view of this, the present invention provides an LED epitaxial wafer and a method for preparing the same, the purpose of which is to solve the problem of reduced luminous efficiency caused by V-shaped defects penetrating quantum wells.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] The present invention provides a method for preparing an LED epitaxial wafer, comprising the following steps:

[0007] S1. Purify the substrate;

[0008] S2, growing a non-doped gallium nitride layer on the substrate after high-temperature purification treatment;

[0009] S3, growing an N-type gallium nitride layer on the non-doped gallium nitride layer;

[0010] S4, growing n quantum well light-emitting layers on the N-type gallium nitride layer;

[0011] S5. Grow an electron blocking layer Al on the quantum well light-emitting layer x Ga 1-x N;

[0012] S6, in the electron blocking layer Al x Ga 1-xA P-type gallium nitride layer is grown on N to obtain an LED epitaxial wafer.

[0013] Furthermore, in step S1, the purification treatment temperature is 1000-1100° C., the purification treatment time is 250-350 seconds, and the purification treatment pressure is 100-300 Torr;

[0014] The purification process is carried out in a H2 atmosphere with a flow rate of H2 of 100 to 150 L / min.

[0015] Furthermore, in step S2, the temperature for growing the undoped gallium nitride layer is 1000-1100° C. and the pressure is 400-500 Torr;

[0016] The thickness of the undoped gallium nitride layer is 1000 to 1500 nm;

[0017] The growth of the non-doped gallium nitride layer is carried out under a mixed gas, the mixed gas comprises N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 70-80:140-160:50-60.

[0018] Furthermore, in step S3, the temperature for growing the N-type gallium nitride layer is 1000-1100° C., and the pressure is 100-300 Torr;

[0019] The thickness of the N-type gallium nitride layer is 800 to 1200 nm;

[0020] The growth of the N-type gallium nitride layer is carried out under a mixed gas, the mixed gas comprises N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 60-70:100-150:40-60.

[0021] Furthermore, in step S4, n≥3; the quantum well light-emitting layer comprises a first quantum barrier GaN, In a Ga 1-a N、In b Ga 1-b N、In c Ga 1-c N and second quantum barrier GaN;

[0022] Growth of the first quantum barrier GaN, In a Ga 1-a N、In b Ga 1-b N、In c Ga 1-c Both N and the second quantum barrier GaN are grown under mixed gas, the mixed gas independently contains N2 and NH3, the flow rate ratio of N2 to NH3 is independently 70-80:30-50; the growth pressure is independently 100-300 Torr.

[0023] Further, the temperature for growing the first quantum barrier GaN is 800-1000° C., the thickness of the first quantum barrier GaN is 2-10 nm, and the growth is carried out on a turntable, the turntable rotates clockwise, and the speed of the turntable is 400-600 r / min;

[0024] Growth a Ga 1-a The temperature of N is 700~800℃, In a Ga 1-a The thickness of N is 1-2 nm, and the growth is carried out on a turntable, which rotates clockwise at a speed of 300-1200 r / min, and the value of a is 0.01-0.05;

[0025] Growth b Ga 1-b The temperature of N is 700~800℃, In b Ga 1-b The thickness of N is 1 to 6 nm, and the growth is carried out on a turntable, which rotates clockwise at a speed of 300 to 1200 r / min, and the value of b is 0.2 to 0.25;

[0026] Growth c Ga 1-c The temperature of N is 700~800℃, In c Ga 1-c The thickness of N is 1-2 nm, and the growth is carried out on a turntable, which rotates counterclockwise at a speed of 300-1200 r / min, and the value of c is 0.01-0.05;

[0027] The temperature for growing the second quantum barrier GaN is 800-1000°C, the thickness of the second quantum barrier GaN is 2-10nm, and the growth is carried out on a turntable, which rotates clockwise at a speed of 400-600r / min.

[0028] Furthermore, in step S5, an electron blocking layer Al is grown. x Ga 1-x The temperature of N is 800-1000°C and the pressure is 100-300 Torr;

[0029] Electron blocking layer Al x Ga 1-x The thickness of N is 100-150 nm, and the value of x is 0.05-0.2;

[0030] The electron blocking layer Al x Ga 1-xThe reaction is carried out under a mixed gas, the mixed gas comprises N2 and NH3, and the flow rate ratio of N2 to NH3 is 100-110:5-15.

[0031] Furthermore, in step S6, the temperature for growing the P-type gallium nitride layer is 900-1000° C., and the pressure is 100-300 Torr;

[0032] The thickness of the P-type gallium nitride layer is 100 to 300 nm;

[0033] The growth of the P-type gallium nitride layer is carried out under a mixed gas, the mixed gas contains N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 60-70:100-150:40-60.

[0034] Furthermore, the growth of step S1, step S2, step S3, step S5 and step S6 are all carried out on a turntable, the rotation direction of the turntable is independently clockwise, and the rotation speed of the turntable is independently 800-1500 r / min.

[0035] The invention also provides an LED epitaxial wafer prepared by the preparation method.

[0036] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:

[0037] When growing a quantum well structure layer, the present invention grows the quantum well in stages. First, a quantum well layer with a low In content is grown to slowly reduce the lattice mismatch to a certain extent, and then a quantum well layer with a high In content is grown. After the quantum well layer with a high In content is grown, the V-shaped defects are covered by controlling the growth direction of the carrier and the growth direction of the quantum well layer with a low In content, so that the V-shaped defects will not affect the underlying quantum well structure, thereby solving the problem of reduced luminous efficiency caused by the cumulative effect of the V-shaped defects. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The schematic diagram of the structure of the LED epitaxial wafer prepared by the present invention, wherein 1 is a substrate, 2 is a non-doped gallium nitride layer, 3 is an N-type gallium nitride layer, 4 is a quantum well light-emitting layer, and 5 is an electron blocking layer Al x Ga 1-x N, 6 are P-type gallium nitride layers;

[0039] Figure 2 Schematic diagram of the structure of a traditional quantum well;

[0040] Figure 3 This is a schematic diagram of the structure of the quantum well prepared in the present invention. DETAILED DESCRIPTION

[0041] The present invention provides a method for preparing an LED epitaxial wafer, comprising the following steps:

[0042] S1. Purify the substrate;

[0043] S2, growing a non-doped gallium nitride layer on the substrate after high-temperature purification treatment;

[0044] S3, growing an N-type gallium nitride layer on the non-doped gallium nitride layer;

[0045] S4, growing n quantum well light-emitting layers on the N-type gallium nitride layer;

[0046] S5. Grow an electron blocking layer Al on the quantum well light-emitting layer x Ga 1-x N;

[0047] S6, in the electron blocking layer Al x Ga 1-x A P-type gallium nitride layer is grown on N to obtain an LED epitaxial wafer.

[0048] In the present invention, in the step S1, the temperature of the purification treatment is 1000-1100°C, preferably 1020-1080°C, and more preferably 1040-1060°C; the time of the purification treatment is 250-350s, preferably 260-340s, and more preferably 280-320s; the pressure of the purification treatment is 100-300Torr, preferably 120-280Torr, and more preferably 150-250Torr; the purification treatment is carried out in a H2 atmosphere, and the flow rate of H2 is 100-150L / min, preferably 115-140L / min, and more preferably 120-130L / min; the purification treatment is carried out on a turntable, the turntable rotates clockwise, and the rotation speed of the turntable is 800-1500r / min, preferably 900-1400r / min, and more preferably 1000-1200r / min.

[0049] In the present invention, in the step S2, the temperature for growing the non-doped gallium nitride layer is 1000-1100°C, preferably 1020-1080°C, and more preferably 1040-1060°C; the pressure is 400-500 Torr, preferably 420-480 Torr, and more preferably 440-460 Torr; the thickness of the non-doped gallium nitride layer is 1000-1500nm, preferably 1100-1400nm, and more preferably 1200-1300nm; the non-doped gallium nitride layer is grown in the mixed gas The process is carried out under a gas atmosphere, wherein the mixed gas comprises N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 70-80: 140-160: 50-60, preferably 72-78: 144-157: 52-58, and further preferably 74-76: 149-153: 54-56; the growth of the undoped gallium nitride layer is carried out on a turntable, which rotates clockwise, and the rotation speed of the turntable is 800-1500 r / min, preferably 900-1400 r / min, and further preferably 1000-1200 r / min.

[0050] In the present invention, in step S3, the temperature for growing the N-type gallium nitride layer is 1000-1100° C., preferably 1020-1080° C., and more preferably 1040-1060° C.; the pressure is 100-300 Torr, preferably 120-280 Torr, and more preferably 150-250 Torr; the thickness of the N-type gallium nitride layer is 800-1200 nm, preferably 900-1100 nm, and more preferably 950-100 nm; the growing of the N-type gallium nitride layer is carried out under the mixed gas The mixed gas comprises N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 60-70: 100-150: 40-60, preferably 62-68: 110-140: 44-57, and further preferably 65-66: 120-130: 48-52; the growth of the N-type gallium nitride layer is carried out on a turntable, the turntable rotates clockwise, and the rotation speed of the turntable is 800-1500r / min, preferably 900-1400r / min, and further preferably 1000-1200r / min.

[0051] In the present invention, in step S4, n≥3, preferably n≥4, and more preferably 5, 6, 7, 8; the quantum well light-emitting layer comprises a first quantum barrier GaN, In a Ga 1-a N、In b Ga 1-b N、In c Ga 1-c N and second quantum barrier GaN;

[0052] Growth of the first quantum barrier GaN, Ina Ga 1-a N、In b Ga 1-b N、In c Ga 1-c Both N and the second quantum barrier GaN are grown under a mixed gas, the mixed gas independently contains N2 and NH3, the flow rate ratio of N2 and NH3 is independently 70-80:30-50, preferably 72-78:34-46, and more preferably 74-76:36-43; the growth pressure is independently 100-300 Torr, preferably 120-280 Torr, and more preferably 150-250 Torr.

[0053] In the present invention, the temperature for growing the first quantum barrier GaN is 800-1000°C, preferably 840-960°C, and more preferably 860-920°C; the thickness of the first quantum barrier GaN is 2-10nm, preferably 3-8nm, and more preferably 4-6nm; the growth is carried out on a turntable, the turntable rotates clockwise, and the rotation speed of the turntable is 400-600r / min, preferably 450-580r / min, and more preferably 460-550r / min.

[0054] In the present invention, the growth of In a Ga 1-a The temperature of N is 700 to 800°C, preferably 720 to 780°C, and more preferably 740 to 760°C; In a Ga 1-a The thickness of N is 1 to 2 nm, preferably 2 nm; the growth is carried out on a turntable, the turntable rotates clockwise, the rotation speed of the turntable is 300 to 1200 r / min, preferably 500 to 1000 r / min, and more preferably 600 to 800 r / min; the value of a is 0.01 to 0.05, preferably 0.02 to 0.04, and more preferably 0.03.

[0055] In the present invention, the growth of In b Ga 1-b The temperature of N is 700 to 800°C, preferably 720 to 780°C, and more preferably 740 to 760°C; In b Ga 1-b The thickness of N is 1 to 6 nm, preferably 2 to 5 nm, and more preferably 3 to 4 nm; the growth is carried out on a turntable, the turntable rotates clockwise, and the rotation speed of the turntable is 300 to 1200 r / min, preferably 500 to 1000 r / min, and more preferably 600 to 800 r / min; the value of b is 0.2 to 0.25, preferably 0.21 to 0.24, and more preferably 0.22 to 0.23.

[0056] In the present invention, the growth of In c Ga 1-c The temperature of N is 700 to 800°C, preferably 720 to 780°C, and more preferably 740 to 760°C; In c Ga 1-c The thickness of N is 1-2nm, preferably 2nm; the growth is carried out on a turntable, the turntable rotates counterclockwise, the rotation speed of the turntable is 300-1200r / min, preferably 500-1000r / min, and more preferably 600-800r / min; the value of c is 0.01-0.05, preferably 0.02-0.04, and more preferably 0.03.

[0057] In the present invention, a represents In in In a Ga 1-a N content, b represents In in In b Ga 1-b N content, c represents the content of In in In c Ga 1-c The content of N; In a Ga 1-a N、In b Ga 1-b N and In c Ga 1-c The In source in N is trimethylindium.

[0058] In the present invention, the temperature for growing the second quantum barrier GaN is 800-1000°C, preferably 840-960°C, and more preferably 880-920°C; the thickness of the second quantum barrier GaN is 2-10nm, preferably 4-8nm, and more preferably 5-6nm; the growth is carried out on a turntable, which rotates clockwise at a speed of 400-600r / min, preferably 450-580r / min, and more preferably 460-550r / min.

[0059] In the present invention, a Ga 1-a N、In b Ga 1-b N and In c Ga 1-c The total thickness of the three N layers is preferably 2 to 10 nm, more preferably 5 to 8 nm.

[0060] In the present invention, the total thickness of one quantum well light-emitting layer is preferably 5 to 20 nm, more preferably 10 to 15 nm.

[0061] In the present invention, in step S5, an electron blocking layer Al is grown. x Ga1-x The temperature of N is 800-1000°C, preferably 850-960°C, and more preferably 880-940°C; the pressure is 100-300 Torr, preferably 120-280 Torr, and more preferably 150-250 Torr; the electron blocking layer Al x Ga 1-x The thickness of N is 100-150 nm, preferably 110-140 nm, and more preferably 120-130 nm; the value of x is 0.05-0.2, preferably 0.08-0.18, and more preferably 0.12-0.15; the growth electron blocking layer Al x Ga 1-x N is carried out under a mixed gas, the mixed gas comprises N2 and NH3, the flow rate ratio of N2 to NH3 is 100-110:5-15, preferably 102-108:6-12, and more preferably 104-106:8-10; the electron blocking layer Al is grown x Ga 1-x N is performed on a turntable, which rotates clockwise at a speed of 800 to 1500 r / min, preferably 900 to 1400 r / min, and more preferably 1000 to 1200 r / min.

[0062] In the present invention, the electron blocking layer Al x Ga 1-x The Al source in N is trimethylaluminum, and the Ga source is triethylgallium.

[0063] In the present invention, in step S6, the temperature for growing the P-type gallium nitride layer is 900-1000° C., preferably 920-980° C., and more preferably 940-960° C.; the pressure is 100-300 Torr, preferably 120-280 Torr, and more preferably 150-250 Torr; the thickness of the P-type gallium nitride layer is 100-300 nm, preferably 120-260 nm, and more preferably 150-220 nm; the growth of the P-type gallium nitride layer is carried out under a mixed gas, and the mixed gas is The combined gas comprises N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 60-70:100-150:40-60, preferably 62-68:110-140:43-57, and further preferably 63-65:120-130:47-52; the growth of the P-type gallium nitride layer is carried out on a turntable, which rotates clockwise, and the rotation speed of the turntable is 800-1500r / min, preferably 900-1400r / min, and further preferably 1000-1200r / min.

[0064] The invention also provides an LED epitaxial wafer prepared by the preparation method.

[0065] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0066] Example 1

[0067] S1. Place a sapphire (Pattern Sapphire Substrate, PSS) substrate into the reaction chamber, adjust the flow rate of H2 to 120L / min, adjust the pressure of the reaction chamber to 200Torr, adjust the carrier speed to 1200r / min, rotate clockwise, increase the temperature to 1080°C, and purify for 300s;

[0068] S2, setting the temperature to 1050°C, the flow rates of N2, H2 and NH3 to 75 L / min, 150 L / min and 56 L / min respectively, adjusting the pressure of the reaction chamber to 450 Torr, adjusting the rotation speed of the carrier to 1000 r / min, rotating clockwise, and growing a 1200 nm thick non-doped gallium nitride U-GaN layer on the substrate;

[0069] S3, setting the temperature to 1050°C, the flow rates of N2, H2 and NH3 to 64 L / min, 120 L / min and 50 L / min respectively, adjusting the pressure of the reaction chamber to 200 Torr, adjusting the rotation speed of the carrier to 1000 r / min, rotating clockwise, and growing an N-type gallium nitride N-GaN layer with a thickness of 1000 nm on the undoped gallium nitride U-GaN layer;

[0070] S4, the temperature is adjusted to 850°C, the flow rates of N2 and NH3 are 72L / min and 40L / min respectively, the pressure of the reaction chamber is adjusted to 200Torr, the carrier speed is adjusted to 500r / min, and the rotation is clockwise to grow a first quantum barrier GaN with a thickness of 3.0nm on the N-type gallium nitride N-GaN layer; then the temperature is lowered to 750°C, and an In layer with a thickness of 2.0nm is grown on the first quantum barrier GaN. 0.05 GA 0.95 N; Under the same conditions, at In 0.05 GA 0.95 In with a thickness of 4.0 nm is grown on N 0.2 GA 0.8 N; while keeping the airflow, temperature and pressure of the reaction chamber unchanged, rotate the carrier counterclockwise and adjust the carrier speed to 500r / min. 0.2 GA 0.8In with a thickness of 2.0 nm is grown on N 0.05 GA 0.95 N; after the growth is completed, the temperature is raised to 850 ° C, and the growth speed of the carrier is controlled at 500r / min, rotating clockwise, while maintaining the airflow and pressure of the reaction chamber unchanged. 0.05 GA 0.95 A second quantum barrier GaN with a thickness of 6.0 nm is grown on N to obtain a quantum well light-emitting layer. Repeat the above steps to grow a total of three quantum well light-emitting layers;

[0071] S5, the temperature is adjusted to 900 ° C, the flow rates of N2 and NH3 are 105L / min and 10L / min respectively, the pressure of the reaction chamber is adjusted to 200Torr, the carrier speed is controlled at 1000r / min, and rotates clockwise to grow Al with a thickness of 120nm on the quantum well light-emitting layer. 0.12 GA 0.88 N layers;

[0072] S6, the temperature was adjusted to 950 ° C, the flow rates of N2, H2 and NH3 were 64 L / min, 120 L / min and 50 L / min respectively, the pressure of the reaction chamber was adjusted to 200 Torr, the speed of the carrier was adjusted to 1000 r / min, and it rotated clockwise. 0.12 GA 0.88 A P-type gallium nitride P-GaN layer with a thickness of 200nm is grown on the N layer, and after the growth is completed, an LED epitaxial wafer is obtained.

[0073] Example 2

[0074] S1. Place a sapphire (Pattern Sapphire Substrate, PSS) substrate into the reaction chamber, adjust the flow rate of H2 to 150L / min, adjust the pressure of the reaction chamber to 300Torr, adjust the carrier speed to 1000r / min, rotate clockwise, increase the temperature to 1050°C, and perform purification for 300s;

[0075] S2. The temperature is set to 1080°C, the flow rates of N2, H2 and NH3 are 76 L / min, 140 L / min and 57 L / min respectively, the pressure of the reaction chamber is adjusted to 500 Torr, the rotation speed of the carrier is adjusted to 1000 r / min, and the carrier rotates clockwise to grow a non-doped gallium nitride U-GaN layer with a thickness of 1300 nm on the substrate;

[0076] S3, setting the temperature to 1050°C, the flow rates of N2, H2 and NH3 to 66 L / min, 122 L / min and 55 L / min respectively, adjusting the pressure of the reaction chamber to 200 Torr, adjusting the rotation speed of the carrier to 1000 r / min, rotating clockwise, and growing an N-type gallium nitride N-GaN layer with a thickness of 1200 nm on the undoped gallium nitride U-GaN layer;

[0077] S4, the temperature is adjusted to 860°C, the flow rates of N2 and NH3 are 76L / min and 40L / min respectively, the pressure of the reaction chamber is adjusted to 200Torr, the carrier speed is adjusted to 500r / min, and the carrier rotates clockwise to grow a first quantum barrier GaN with a thickness of 3.0nm on the N-type gallium nitride N-GaN layer; then the temperature is lowered to 750°C, and an In layer with a thickness of 1.0nm is grown on the first quantum barrier GaN. 0.05 GA 0.95 N; Under the same conditions, 0.05 GA 0.95 In with a thickness of 4.0 nm is grown on N 0.2 GA 0.8 N; while keeping the airflow, temperature and pressure of the reaction chamber unchanged, rotate the carrier counterclockwise and adjust the carrier speed to 500r / min. 0.2 GA 0.8 In with a thickness of 2.0 nm is grown on N 0.05 GA 0.95 N; after the growth is completed, the temperature is raised to 850 ° C, and the growth speed of the carrier is controlled at 500r / min, rotating clockwise, while maintaining the airflow and pressure of the reaction chamber unchanged. 0.05 GA 0.95 N grows a second quantum barrier GaN with a thickness of 6.0nm, thus obtaining a quantum well light-emitting layer. Repeat the above steps to grow a total of 4 quantum well light-emitting layers;

[0078] S5, the temperature is adjusted to 900 ° C, the flow rates of N2 and NH3 are 107L / min and 11L / min respectively, the pressure of the reaction chamber is adjusted to 200Torr, the carrier speed is controlled at 1100r / min, and rotates clockwise to grow Al with a thickness of 120nm on the quantum well light-emitting layer. 0.12 GA 0.88 N layers;

[0079] S6, the temperature was adjusted to 950 ° C, the flow rates of N2, H2 and NH3 were 65 L / min, 120 L / min and 50 L / min respectively, the pressure of the reaction chamber was adjusted to 200 Torr, the speed of the carrier was adjusted to 1200 r / min, and the rotation was clockwise. 0.12 GA 0.88A P-type gallium nitride P-GaN layer with a thickness of 200nm is grown on the N layer, and after the growth is completed, an LED epitaxial wafer is obtained.

[0080] Example 3

[0081] S1. Place a sapphire (Pattern Sapphire Substrate, PSS) substrate into the reaction chamber, adjust the flow rate of H2 to 120L / min, adjust the pressure of the reaction chamber to 200Torr, adjust the carrier speed to 1200r / min, rotate clockwise, increase the temperature to 1080°C, and perform purification treatment for 320s;

[0082] S2, setting the temperature to 1050°C, the flow rates of N2, H2 and NH3 to 77L / min, 150L / min and 54L / min respectively, adjusting the pressure of the reaction chamber to 450Torr, adjusting the rotation speed of the carrier to 1200r / min, rotating clockwise, and growing a non-doped gallium nitride U-GaN layer with a thickness of 1200nm on the substrate;

[0083] S3, setting the temperature to 1050°C, the flow rates of N2, H2 and NH3 to 62 L / min, 120 L / min and 53 L / min respectively, adjusting the pressure of the reaction chamber to 200 Torr, adjusting the rotation speed of the carrier to 1000 r / min, rotating clockwise, and growing an N-type gallium nitride N-GaN layer with a thickness of 1100 nm on the undoped gallium nitride U-GaN layer;

[0084] S4, the temperature is adjusted to 850°C, the flow rates of N2 and NH3 are 72L / min and 40L / min respectively, the pressure of the reaction chamber is adjusted to 200Torr, the carrier speed is adjusted to 500r / min, and the rotation is clockwise to grow a first quantum barrier GaN with a thickness of 3.0nm on the N-type gallium nitride N-GaN layer; then the temperature is lowered to 750°C, and an In layer with a thickness of 2.0nm is grown on the first quantum barrier GaN. 0.05 GA 0.95 N; Under the same conditions, 0.05 GA 0.95 In with a thickness of 4.0 nm is grown on N 0.2 GA 0.8 N; while keeping the airflow, temperature and pressure of the reaction chamber unchanged, rotate the carrier counterclockwise and adjust the carrier speed to 500r / min. 0.2 GA 0.8 In with a thickness of 2.0 nm is grown on N 0.05 GA 0.95N; after the growth is completed, the temperature is raised to 850 ° C, and the growth speed of the carrier is controlled at 500r / min, rotating clockwise, while maintaining the airflow and pressure of the reaction chamber unchanged. 0.05 GA 0.95 N grows a second quantum barrier GaN with a thickness of 6.0nm to obtain a quantum well light-emitting layer. Repeat the above steps to grow a total of 5 quantum well light-emitting layers;

[0085] S5, the temperature is adjusted to 900 ° C, the flow rates of N2 and NH3 are 108 L / min and 10 L / min respectively, the pressure of the reaction chamber is adjusted to 200 Torr, the carrier speed is controlled at 1100 r / min, and rotates clockwise to grow Al with a thickness of 120 nm on the quantum well light-emitting layer. 0.12 GA 0.88 N layers;

[0086] S6, the temperature was adjusted to 950 ° C, the flow rates of N2, H2 and NH3 were 66 L / min, 120 L / min and 52 L / min respectively, the pressure of the reaction chamber was adjusted to 200 Torr, the speed of the carrier was adjusted to 1000 r / min, and it rotated clockwise. 0.12 GA 0.88 A P-type gallium nitride P-GaN layer with a thickness of 200nm is grown on the N layer, and after the growth is completed, an LED epitaxial wafer is obtained.

[0087] Performance Testing

[0088] The LED epitaxial wafers prepared in Examples 1 to 3 of the present invention are Figure 2 The epitaxial wafers of the conventional quantum well structure shown were made into chips of 168 μm×216 μm, a current of 20 mA was passed through them, and the luminous brightness at a wavelength of 530 nm was measured at a voltage of 2.8 V. The test results are shown in Table 1.

[0089] Table 1 Test results of luminous brightness

[0090] Example 1 Example 2 Example 3 Traditional chips Luminous brightness (mW) 14.5 14.9 15.2 13

[0091] As shown in Table 1, compared with the conventional chip, the brightness of Example 1 of the present invention is increased by 11.5%, compared with the conventional chip, the brightness of Example 2 is increased by 14.6%, and compared with the conventional chip, the brightness of Example 3 is increased by 16.9%. The above test results show that the technical solution provided by the present invention can effectively solve the problem of decreased luminous efficiency caused by the cumulative effect of V-shaped defects.

[0092] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0093] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing an LED epitaxial wafer, characterized in that: The following steps are involved: S1. Purify the substrate; S2, growing a non-doped gallium nitride layer on the substrate after high-temperature purification treatment; S3, growing an N-type gallium nitride layer on the non-doped gallium nitride layer; S4, growing n quantum well light-emitting layers on the N-type gallium nitride layer; S5. Grow an electron blocking layer Al on the quantum well light-emitting layer x Ga 1-x N; S6, in the electron blocking layer Al x Ga 1-x A P-type gallium nitride layer is grown on N to obtain an LED epitaxial wafer; In the step S4, n≥3; the quantum well light-emitting layer includes a first quantum barrier GaN, In a Ga 1-a N、In b Ga 1-b N、In c Ga 1-c N and second quantum barrier GaN; Growth of the first quantum barrier GaN, In a Ga 1-a N、In b Ga 1-b N、In c Ga 1-c Both N and the second quantum barrier GaN are grown under mixed gas, the mixed gas independently contains N2 and NH3, the flow rate ratio of N2 to NH3 is independently 70-80:30-50; the growth pressure is independently 100-300 Torr; The temperature for growing the first quantum barrier GaN is 800-1000°C, the thickness of the first quantum barrier GaN is 2-10nm, and the growth is carried out on a turntable, which rotates clockwise at a speed of 400-600r / min; Growth a Ga 1-a The temperature of N is 700~800℃, In a Ga 1-a The thickness of N is 1-2 nm, and the growth is carried out on a turntable, which rotates clockwise at a speed of 300-1200 r / min, and the value of a is 0.01-0.04; Growth b Ga 1-b The temperature of N is 700~800℃, In b Ga 1-b The thickness of N is 1 to 6 nm, and the growth is carried out on a turntable, which rotates clockwise at a speed of 300 to 1200 r / min, and the value of b is 0.2 to 0.25; Growth c Ga 1-c The temperature of N is 700~800℃, In c Ga 1-c The thickness of N is 1-2 nm, and the growth is carried out on a turntable, which rotates counterclockwise at a speed of 300-1200 r / min, and the value of c is 0.01-0.04; The temperature for growing the second quantum barrier GaN is 800-1000°C, the thickness of the second quantum barrier GaN is 2-10nm, and the growth is carried out on a turntable, which rotates clockwise at a speed of 400-600r / min.

2. The preparation method according to claim 1, characterized in that: In step S1, the purification treatment temperature is 1000-1100° C., the purification treatment time is 250-350 seconds, and the purification treatment pressure is 100-300 Torr; The purification process is carried out in a H2 atmosphere with a flow rate of H2 of 100 to 150 L / min.

3. The preparation method according to claim 2, characterized in that: In the step S2, the temperature for growing the undoped gallium nitride layer is 1000-1100° C. and the pressure is 400-500 Torr; The thickness of the undoped gallium nitride layer is 1000 to 1500 nm; The growth of the non-doped gallium nitride layer is carried out under a mixed gas, the mixed gas comprises N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 70-80:140-160:50-60.

4. The preparation method according to any one of claims 1 to 3, characterized in that: In the step S3, the temperature for growing the N-type gallium nitride layer is 1000-1100° C. and the pressure is 100-300 Torr; The thickness of the N-type gallium nitride layer is 800 to 1200 nm; The growth of the N-type gallium nitride layer is carried out under a mixed gas, the mixed gas includes N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 60-70:100-150:40-60.

5. The preparation method according to claim 1, characterized in that: In step S5, an electron blocking layer Al is grown. x Ga 1-x The temperature of N is 800-1000°C and the pressure is 100-300 Torr; Electron blocking layer Al x Ga 1-x The thickness of N is 100-150 nm, and the value of x is 0.05-0.2; The electron blocking layer Al x Ga 1-x The reaction is carried out under a mixed gas, the mixed gas comprises N2 and NH3, and the flow rate ratio of N2 to NH3 is 100-110:5-15.

6. The preparation method according to claim 5, characterized in that: In step S6, the temperature for growing the P-type gallium nitride layer is 900-1000° C. and the pressure is 100-300 Torr; The thickness of the P-type gallium nitride layer is 100 to 300 nm; The growth of the P-type gallium nitride layer is carried out under a mixed gas, the mixed gas includes N2, H2 and NH3, and the flow rate ratio of N2, H2 and NH3 is 60-70:100-150:40-60.

7. The preparation method according to claim 1 or 6, characterized in that: The growth of step S1, step S2, step S3, step S5 and step S6 are all carried out on a turntable, the rotation direction of the turntable is independently clockwise, and the rotation speed of the turntable is independently 800-1500r / min.

8. An LED epitaxial wafer prepared by the preparation method according to any one of claims 1 to 7.