Ceramic cooker and preparation method thereof
By forming a micron-scale aluminum layer on the inner surface of the ceramic substrate of the ceramic cooker and covering the refractory composite layer, the problems of low heat transfer efficiency and short service life of the ceramic cooker are solved, and efficient heating and durability are achieved.
Patent Information
- Application Number
- CN202211144459.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-20
AI Technical Summary
The existing ceramic cookware has low heat transfer efficiency and short service life when using electromagnetic induction heating. The air gap between the metal magnetic permeable sheet and the ceramic substrate leads to low heat transfer efficiency. The large difference in thermal expansion coefficient may lead to ceramic rupture, and the magnetic permeable film is easily Ablation or shedding, and the power is reduced.
A composite layer of 20μm-100μm thick is formed on the inner surface of the ceramic substrate and covered with a composite layer composed of refractory materials and cosolvents. It is formed by melting and spraying technology. The composite layer is in a compressive stress state to improve the heat resistance of the magnetically conductive layer. Sex and service life.
The heat transfer efficiency and service life of ceramic cookware are improved. The aluminum layer heats food through induction eddy current. The composite layer protects the magnetic-conductive layer from scratches and corrosion, extending the service life of the cookware.
Smart Images

Figure BDA0003854725630000091 
Figure BDA0003854725630000101
Abstract
Description
Technical Field
[0001] The present invention relates to the field of kitchen utensils, and more particularly to a ceramic cooker and a preparation method thereof. Background Art
[0002] Ceramics cannot be heated by electromagnetic induction because they have no electrical conductivity.
[0003] In the prior art, a metal magnetic sheet is usually embedded on a ceramic substrate, or a layer of magnetic film is applied on the ceramic substrate, and then a glazing process is performed, and finally sintering is performed to obtain a magnetically conductive ceramic cookware. However, for the technical solution of embedding a metal magnetic sheet on a ceramic substrate, the metal magnetic sheet cannot fit tightly with the ceramic substrate due to the air gap between the metal magnetic sheet and the ceramic substrate, resulting in low heat transfer efficiency, and the difference in thermal expansion coefficients between the two is very large, so the stress of the metal magnetic sheet cannot be released, which may cause the ceramic substrate to crack; in addition, for the technical solution of applying a magnetic film on a ceramic substrate, the magnetic film applied on the outer surface is easily burned due to the large amount of heat generated by the slow thermal conductivity of the ceramic substrate cannot be discharged, or the ceramic glaze is scratched or peeled off and exposed to oxidation, resulting in reduced power, which greatly reduces the service life of the ceramic cookware.
[0004] Therefore, how to propose a ceramic cooker that can utilize electromagnetic induction for heating and can extend the service life and improve the heat transfer efficiency has become a problem that needs to be solved urgently. Summary of the invention
[0005] The present invention provides a ceramic cooker and a method for preparing the same. The present invention can prepare a ceramic cooker with high heat transfer efficiency and long service life.
[0006] According to aspects of the present inventive concept, there is provided a ceramic cooker, comprising: a ceramic substrate; an aluminum layer, disposed on at least a portion of an inner surface of the ceramic substrate, wherein the thickness of the aluminum layer is in the range of 20 μm-100 μm; and a composite layer, covering the aluminum layer on the ceramic substrate, the composite layer comprising a refractory material and a flux.
[0007] The composite layer may be in a compressive stress state.
[0008] The refractory material may include SiO2, TiO2, NiO and Al2O3, and the flux may include CaF2, Na2O, K2O, B2O3 and Li2O.
[0009] The composite layer may include: 10-20 parts by mass of SiO2; 3-6 parts by mass of TiO2; 1-2 parts by mass of NiO; 20-40 parts by mass of Al2O3; 5-10 parts by mass of CaF2; 20-40 parts by mass of Li2O; 10-15 parts by mass of B2O3; 10-20 parts by mass of NaO2; and 5-10 parts by mass of K2O.
[0010] According to other aspects of the present invention, a method for preparing ceramic cookware is provided, the method comprising the following steps: providing a ceramic substrate; applying aluminum to at least a portion of the inner surface of the ceramic substrate (for example, the inner surface of the bottom) using a spraying process to form an aluminum layer, wherein the aluminum layer has a thickness in the range of 20 μm-100 μm; and forming a composite layer covering the aluminum layer on the substrate using a spraying process, wherein the composite layer includes a refractory material and a flux.
[0011] The spraying process may include an arc spraying process.
[0012] The composite layer may be in a compressive stress state.
[0013] The refractory material may include SiO2, TiO2, NiO and Al2O3, and the flux may include CaF2, Na2O, K2O, B2O3 and Li2O, wherein the composite layer may include: 10-20 parts by mass of SiO2; 3-6 parts by mass of TiO2; 1-2 parts by mass of NiO; 20-40 parts by mass of Al2O3; 5-10 parts by mass of CaF2; 20-40 parts by mass of Li2O; 10-15 parts by mass of B2O3; 10-20 parts by mass of NaO2; and 5-10 parts by mass of K2O.
[0014] The composite layer may be formed by dry electrostatic spraying to cover the aluminum layer.
[0015] The method may further include the step of sintering the resulting material after the composite layer is formed.
[0016] Through the above brief description and the following detailed description of the inventive concept, the inventive concept mainly adopts the inner bottom spraying aluminum + low-temperature enamel to prepare the protective layer, and uses the high hardness and density of the enamel to effectively protect the magnetic conductive layer of the aluminum layer from being scratched and corroded, so as to improve the life of the magnetic conductive layer. In addition, the inner surface of the ceramic cookware of the inventive concept is sprayed with aluminum, and the heat of the aluminum magnetic conductive layer can transfer heat to the food faster, thereby improving the heat transfer efficiency. DETAILED DESCRIPTION
[0017] Now, the present invention will be described more fully hereinafter. However, the present invention can be implemented in many different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.
[0018] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting.
[0019] It will also be understood that when the terms "include" and / or "comprises" are used in this specification, it indicates the presence of the stated features, regions, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components and / or groups thereof.
[0020] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs. It will also be understood that, unless expressly defined herein, terms such as those defined in general dictionaries should be interpreted as having a meaning consistent with the meaning of the terms in the context of the relevant art and the present disclosure, and should not be interpreted in an idealized or overly formal manner.
[0021] Now, a ceramic cooker according to an exemplary embodiment of the present invention will be described hereinafter.
[0022] The ceramic cooker according to an exemplary embodiment of the present inventive concept may have a three-layer structure. Specifically, the three-layer structure may include a ceramic substrate, an aluminum layer disposed on at least a portion of the inner surface of the ceramic substrate, and a composite layer covering the aluminum layer on the ceramic substrate.
[0023] The ceramic substrate can be made of a ceramic material, and therefore, the present invention has no particular limitation on the material of the ceramic substrate, and those skilled in the art can select a suitable ceramic material as the material for forming the ceramic substrate according to the present invention. In addition, the ceramic substrate of the present invention needs to provide a receiving space as the substrate of the ceramic cooker, and therefore, the shape of the ceramic substrate can be adapted to the shape of the ceramic cooker to be formed in the end, and the present invention is not limited thereto.
[0024] The aluminum layer is formed on the ceramic substrate, specifically, it can be formed on at least part of the inner surface of the ceramic substrate. Here, the aluminum layer is used to provide magnetic conductivity, so it can be, but is not limited to, arranged at the bottom of the ceramic substrate adjacent to the induction cooker, and those skilled in the art can appropriately select the laying position and laying area of the aluminum layer according to the concept of the present invention. For example, when the electromagnetic device for heating is adjacent to the side wall of the ceramic cooker, the aluminum layer can be arranged on the inner side wall of the ceramic substrate instead of the bottom of the ceramic substrate, but is not limited thereto.
[0025] In addition, the aluminum layer can have a thickness range of 20 μm-100 μm. This is because: aluminum cookware cannot conduct magnetism on an induction cooker, not because aluminum cannot conduct magnetism, but because the electrical resistance of aluminum is too small. To enable aluminum to generate induction heat on an induction cooker, it is necessary to reduce the cross-sectional area of aluminum to increase its electrical resistance. The present invention can use the spraying technology to prepare an aluminum layer with a micron-level thickness, so that the aluminum layer with a micron-level thickness can generate an induced eddy current on the induction cooker to generate heat and heat food.
[0026] The composite layer (enamel glaze) is arranged on the ceramic substrate to cover the aluminum layer. According to an exemplary embodiment, the composite layer may include an enamel material, for example, a low-temperature enamel material. The enamel material is a metal and a non-metallic inorganic material that are physically and chemically connected in the form of a chemical bond through a special process, and the composite layer including the enamel material has an amorphous structure similar to glass, and its microstructure is very dense and has a low porosity, which can effectively reduce the water absorption rate of the ceramic cookware. At the same time, the enamel material has a high hardness and can effectively protect the magnetic aluminum layer from being scratched.
[0027] In addition, one of the most important properties of ceramic cookware is its thermal shock resistance. It requires that the thermal expansion coefficient of the composite layer including the enamel on the surface is similar to that of the ceramic matrix, so that when it is heated to a certain temperature and then cooled suddenly, the tensile stress generated by the volume change is less than the corresponding tensile strength (because the compressive strength of the enamel material is generally 10-20 times the tensile strength, the failure of the enamel is generally caused by the tensile stress being greater than the tensile strength, resulting in enamel cracking). Therefore, when designing the enamel material, the expansion coefficient of the enamel material is generally similar to or slightly smaller than the magnetic aluminum layer, so that it is in a compressive stress state.
[0028] Since the expansion coefficient of the enamel material is related to its chemical composition, according to an exemplary embodiment, the composite material including the enamel material may include a refractory material and a flux, the refractory material may include SiO2, TiO2, NiO and Al2O3, and the flux includes CaF2, Na2O, K2O, B2O3 and Li2O. According to the present invention, Na2O, K2O and Li2O can increase the expansion coefficient, especially Li2O. Therefore, when the composite material including the enamel material includes the above materials, the composite material may include: 10-20 parts by mass of SiO2; 3-6 parts by mass of TiO2; 1-2 parts by mass of NiO; 20-40 parts by mass of Al2O3; 5-10 parts by mass of CaF2; 20-40 parts by mass of Li2O; 10-15 parts by mass of B2O3; 10-20 parts by mass of NaO2; 5-10 parts by mass of K2O.
[0029] According to the present invention, because the composite material of the exemplary embodiment includes a large content of Na2O, K2O, and Li2O, the increase in the content of these components can increase the thermal expansion coefficient and reduce the firing temperature, thereby improving the thermal shock resistance of the product and making it difficult for the ceramic matrix and the aluminum layer to delaminate.
[0030] The ceramic cooker of the present inventive concept is described above in conjunction with exemplary embodiments. In the following, a method for manufacturing the ceramic cooker will be described in detail in conjunction with specific examples.
[0031] A method of manufacturing a ceramic cooker according to the inventive concept may include: providing a ceramic substrate; forming an aluminum layer at at least a portion of the ceramic substrate; and forming a composite layer covering the aluminum layer on the substrate using a spraying process.
[0032] The step of providing a ceramic base may include providing a ceramic material and forming a ceramic base having an accommodation space using the ceramic material.
[0033] According to an exemplary embodiment, the material used to form the ceramic substrate can be various ceramic materials known in the art for forming cookware, and various methods known in the art can be used to form a ceramic substrate having a specific shape of a receiving space. The inventive concept does not limit the material of the ceramic substrate, its process, and the shape of the formed ceramic substrate, and those skilled in the art can reasonably design this according to the inventive concept.
[0034] After providing the ceramic substrate, an aluminum layer may be formed on at least a portion of the inner surface of the ceramic substrate by a spraying process. Here, the "partial inner surface" of the ceramic substrate may be understood as an inner surface that can generate electromagnetic induction when the ceramic cookware to be formed is used in an induction cooker. In other words, the partial inner surface may be the inner bottom surface of the ceramic substrate or other inner surfaces other than the inner bottom surface or the entire inner surface of the ceramic substrate, and those skilled in the art may reasonably select the laying position of the aluminum layer according to the teachings of the inventive concept.
[0035] According to an exemplary embodiment, the process of spraying the aluminum layer may include a thermal spraying process. According to a specific example, the aluminum layer may be formed by arc spraying technology. Through the spraying process, an aluminum layer with a micron-level thickness in the range of 20 μm-100 μm may be formed on the ceramic substrate. Since the aluminum layer with a micron-level thickness is formed, the aluminum layer may generate an induced eddy current on a device such as an induction cooker, thereby generating heat to heat the food.
[0036] According to a specific example, when arc spraying is used to form an aluminum layer on a ceramic substrate, the specific process parameters are as follows: the diameter of the aluminum wire is 2 mm, the voltage is 30V-40V, the current is 200A-250A, the spraying distance is 200mm, and the arc gun travel speed is 600mm / s.
[0037] After forming the micrometer-sized aluminum layer, a composite layer covering the aluminum layer may be formed on the ceramic substrate. However, optionally, after forming the aluminum layer, the aluminum layer may be sanded to reduce the surface roughness of the aluminum layer, and then the composite layer may be formed on the sanded aluminum layer so that the composite layer has a smooth and fine surface after sintering. However, the inventive concept is not limited thereto, and the sanding step may be omitted.
[0038] According to an exemplary embodiment, the composite layer may include an enamel material, for example, a low-temperature enamel material. The enamel material is a metal and a non-metallic inorganic material that are physically and chemically connected in a chemical bond through a special process, and the composite layer including the enamel material has an amorphous structure similar to glass, and its microstructure is very dense and has a low porosity, which can effectively reduce the water absorption rate of the ceramic cookware. At the same time, the enamel material has a high hardness and can effectively protect the magnetic aluminum layer from being scratched.
[0039] The material for forming the composite layer according to the exemplary embodiment may include a refractory material and a flux, the refractory material may include SiO2, TiO2, NiO and Al2O3, and the flux includes CaF2, Na2O, K2O, B2O3 and Li2O. Specifically, 10-20 parts by mass of SiO2, 3-6 parts by mass of TiO2, 1-2 parts by mass of NiO, 20-40 parts by mass of Al2O3, 5-10 parts by mass of CaF2, 20-40 parts by mass of Li2O, 10-15 parts by mass of B2O3, 10-20 parts by mass of NaO2 and 5-10 parts by mass of K2O may be selected, and the composite layer may be formed using the above materials by a spraying process.
[0040] According to a specific example, dry electrostatic spraying can be used to form the composite layer. Here, the parameters of electrostatic spraying are: using compressed air + electrostatic force to atomize the material (glaze) forming the composite layer, electrostatic high voltage 50KV-80KV, electrostatic current 10μA-20μA, flow rate pressure 0.3MPa-0.55MPa, atomization pressure 0.3MPa0.45MPa, spraying distance 150mm-300mm, and single or multiple spraying deposition coatings can be used.
[0041] After the spraying process, a composite layer with a thickness in the range of 150 μm-300 μm according to the present invention may be formed.
[0042] Then, the composite layer may be sintered using a sintering process to obtain the ceramic cookware that can be used for an induction cooker according to an exemplary embodiment of the present inventive concept.
[0043] The above is a detailed description of the method for preparing ceramic cookware according to the present invention in conjunction with exemplary embodiments. Since the present invention adopts the spraying technology, an aluminum layer with a thickness of micrometer level can be formed. Due to the micrometer level aluminum layer, it is possible to generate induced eddy currents on the induction cooker, thereby generating heat to heat the food. In addition, since the material included in the composite layer of the present invention has an expansion coefficient similar to or slightly smaller than the expansion coefficient of the aluminum layer, so that it has a compressive stress state, the composite layer with a compressive stress state improves the thermal shock resistance of the ceramic cookware, and makes it difficult for the ceramic substrate and the aluminum layer to delaminate, thereby increasing the service life of the cookware.
[0044] In the following, the beneficial effects of the present invention will be demonstrated in combination with specific embodiments and comparative examples.
[0045] Example 1
[0046] A ceramic substrate for preparing a ceramic pot is provided.
[0047] The arc spraying technology is used to form an aluminum layer with a thickness of 20 μm on the inner surface of the bottom of the ceramic pot. Here, the parameters of the arc spraying process are: the diameter of the aluminum wire is 2 mm, the voltage is 30 V, the current is 250 A, the spraying distance is 200 mm, and the arc gun travel speed is 600 mm / s.
[0048] A composite layer with a thickness of 150 μm is formed on the inner surface of the ceramic substrate on which the aluminum layer is formed by dry electrostatic spraying process. Here, the materials forming the composite layer are (by mass): SiO2: 20 parts; TiO2: 5 parts; NiO: 2 parts; Al2O3: 30 parts. CaF2: 5 parts; Li2O: 40 parts; B2O3: 10 parts; NaO2: 20 parts; K2O: 10 parts. In addition, the parameters of electrostatic spraying are: compressed air + electrostatic force is used to atomize the material forming the composite layer, the electrostatic high voltage is 80KV, the electrostatic current is 20μA, the flow rate pressure is 0.4MPa, the atomization pressure is 0.45MPa, and the spraying distance is 200mm.
[0049] After the electrostatic spraying is completed, sintering at 680° C. is performed to form the ceramic cookware of Example 1.
[0050] Example 2
[0051] The difference from Example 1 is that the thickness of the aluminum layer is 50 μm.
[0052] Example 3
[0053] The difference from Example 1 is that the thickness of the aluminum layer is 75 μm.
[0054] Example 4
[0055] The difference from Example 1 is that the thickness of the aluminum layer is 100 μm.
[0056] Example 5
[0057] The difference from Example 1 is that the amount of Li2O is 30 parts.
[0058] Example 6
[0059] The difference from Example 1 is that the amount of Li2O is 20 parts.
[0060] Example 7
[0061] The difference from Example 1 is that the amount of SiO2 is 10 parts.
[0062] Example 8
[0063] The difference from Example 1 is that the amount of SiO2 is 15 parts.
[0064] Example 9
[0065] The difference from Example 1 is that the amount of TiO2 is 3 parts.
[0066] Example 10
[0067] The difference from Example 1 is that the amount of TiO2 is 6 parts.
[0068] Embodiment 11
[0069] The difference from Example 1 is that the amount of NiO is 1 part.
[0070] Example 12
[0071] The difference from Example 1 is that the amount of NiO is 1.5 parts.
[0072] Example 13
[0073] The difference from Example 1 is that the amount of Al2O3 is 20 parts.
[0074] Embodiment 14
[0075] The difference from Example 1 is that the amount of Al2O3 is 40 parts.
[0076] Embodiment 15
[0077] The difference from Example 1 is that CaF2 is 7 parts
[0078] Example 16
[0079] The difference from Example 1 is that CaF2 is 10 parts
[0080] Embodiment 17
[0081] The difference from Example 1 is that the amount of B2O3 is 13 parts.
[0082] Embodiment 18
[0083] The difference from Example 1 is that the amount of B2O3 is 15 parts.
[0084] Embodiment 19
[0085] The difference from Example 1 is that the amount of NaO2 is 10 parts.
[0086] Embodiment 20
[0087] The difference from Example 1 is that the amount of NaO2 is 15 parts.
[0088] Embodiment 21
[0089] The difference from Example 1 is that the amount of K2O is 5 parts.
[0090] Embodiment 22
[0091] The difference from Example 1 is that the amount of K2O is 7 parts.
[0092] Comparative Example 1
[0093] The difference from Example 1 is that the material forming the composite layer does not include Li2O, NaO2 and K2O.
[0094] Comparative Example 2
[0095] The difference from Example 1 is that the material forming the composite layer does not include Li2O.
[0096] Comparative Example 3
[0097] The difference from Example 1 is that the material forming the composite layer does not include NaO2.
[0098] Comparative Example 4
[0099] The difference from Example 1 is that the material forming the composite layer does not include K2O.
[0100] Comparative Example 5
[0101] The difference from Example 1 is that the amount of Li2O is 10 parts.
[0102] Comparative Example 6
[0103] The difference from Example 1 is that the amount of Li2O is 50 parts.
[0104] Comparative Example 7
[0105] The difference from Example 1 is that the amount of NaO2 is 5 parts.
[0106] Comparative Example 8
[0107] The difference from Example 1 is that the amount of NaO2 is 25 parts.
[0108] Comparative Example 9
[0109] The difference from Example 1 is that the amount of K2O is 3 parts.
[0110] Comparative Example 10
[0111] The difference from Example 1 is that the amount of K2O is 12 parts.
[0112] Comparative Example 11
[0113] The difference from Example 1 is that a 120 μm aluminum layer is formed.
[0114] Comparative Example 12
[0115] The difference from Example 1 is that an aluminum layer with a thickness of 400 μm is formed.
[0116] The following tests were conducted using the ceramic cookware of Examples 1-22 and the ceramic cookware of Comparative Examples 1-12, and the test structures are recorded in Table 1.
[0117] (1) Test heating efficiency: record the time it takes to boil 2L of water on an induction cooker;
[0118] (2) Testing the magnetic conductivity life of ceramic cookware: Place the sample on an induction cooker, cook commercially available hot pot soup in the pot, and record the cooking time of the hot pot soup;
[0119] (3) Test the thermal shock resistance of ceramic cookers. The test method refers to the industry standard QBT 2580-2018 Fine Ceramic Cookers;
[0120]
[0121]
[0122] By comparing Examples 1-22 with Comparative Examples 1-12, the ceramic cookware according to the present invention has beneficial magnetic conductivity, long service life and good shock resistance.
[0123] Although one or more embodiments of the present invention have been described, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit and scope of the present invention as defined by the claims.
Claims
1. A ceramic cooker, It is characterized in that The ceramic cooker comprises: Ceramic substrate; an aluminum layer disposed on at least a portion of the inner surface of the ceramic substrate, wherein the aluminum layer has a thickness in the range of 20 μm to 100 μm; A composite layer is formed on the ceramic substrate and covers the aluminum layer. The composite layer includes a refractory material and a flux. The refractory material is composed of SiO 2 、TiO 2 , NiO and Al 2 O 3 The co-solvent is composed of CaF 2 、Na 2 O.K 2 O.B 2 O 3 and Li 2 O, the composite layer comprises: 10-20 parts by mass of SiO 2 ; 3-6 parts by mass of TiO 2 ; 1-2 parts by mass of NiO; 20-40 parts by mass of Al 2 O 3 ; 5-10 parts by mass of CaF 2 ; 20-40 parts by mass of Li 2 O; 10-15 parts by mass of B 2 O 3 ; 10-20 parts by mass of NaO 2 ; 5-10 parts by mass of K 2 O.
2. The ceramic cooker according to claim 1, It is characterized in that The composite layer is in a compressive stress state.
3. The ceramic cooker according to claim 1, It is characterized in that The thickness of the composite layer is 150 μm-300 μm.
4. A method for preparing ceramic cookware, It is characterized in that The method comprises the following steps: providing a ceramic substrate; Applying aluminum to at least a portion of the inner surface of the ceramic substrate by a spraying process to form an aluminum layer, wherein the aluminum layer has a thickness in the range of 20 μm-100 μm; A composite layer covering the aluminum layer is formed on the substrate by a spraying process, wherein the composite layer comprises a refractory material and a flux, and the refractory material is composed of SiO 2 、TiO 2 , NiO and Al 2 O 3 The co-solvent is composed of CaF 2 、Na 2 O.K 2 O.B 2 O 3 and Li 2 O, the composite layer comprises: 10-20 parts by mass of SiO 2 ; 3-6 parts by mass of TiO 2 ; 1-2 parts by mass of NiO; 20-40 parts by mass of Al 2 O 3 ; 5-10 parts by mass of CaF 2 ; 20-40 parts by mass of Li 2 O; 10-15 parts by mass of B 2 O 3 ; 10-20 parts by mass of NaO 2 ; 5-10 parts by mass of K 2 O.
5. The method according to claim 4, It is characterized in that The spraying process includes an arc spraying process.
6. The method according to claim 4, It is characterized in that The composite layer is in a compressive stress state.
7. The method according to claim 4, It is characterized in that The composite layer is formed by dry electrostatic spraying to cover the aluminum layer.
8. The method according to claim 4, It is characterized in that The method further comprises the step of sintering the resulting material after the composite layer is formed.