Bacteria-responsive nanofiber membrane, nanofiber material and preparation method thereof

Through the design of the shell and core layers of the bacteria-responsive nanofiber membrane, the combination of bacterial degradable materials and antibacterial drugs is used to solve the problem that the release rate of antibacterial drugs cannot be dynamically adjusted during tympanic membrane repair, and realize adaptive antibacterial and antibacterial drugs. The effect of mechanical support reduces the risk of bacterial infection and drug burst release.

CN115518202BActive Publication Date: 2024-10-29THE UNIV OF NOTTINGHAM NINGBO CHINA
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211046199.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-30
Publication Date
2024-10-29
Estimated Expiration
2042-08-30

AI Technical Summary

Technical Problem

It is difficult for the existing technology to simultaneously provide support for epithelial cell layer repair and adaptive antibacterial effects during the tympanic membrane repair process, and the release rate of antibacterial drugs cannot be dynamically adjusted, resulting in problems of bacterial infection risk and drug burst release.

Method used

It uses a bacterial-responsive nanofiber membrane, which is composed of a shell layer composed of synthetic polymer materials and bacterial-degradable natural polymer materials. The nanofibers overlap with each other to provide mechanical support, and release antibacterial drugs through bacterial degradation during bacterial infection, using coaxial Electrospinning technology prepares nanofiber membranes to achieve sustained drug release.

Benefits of technology

It achieves the adaptive antibacterial effect and mechanical support during the tympanic membrane repair process, avoids the toxic side effects of antibacterial drugs on normal cells, improves drug stability and release efficiency, and reduces the risk of bacterial infection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115518202B_ABST
    Figure CN115518202B_ABST
Patent Text Reader

Abstract

The present invention provides a bacteria-responsive nanofiber membrane, a nanofiber material and a preparation method thereof, and relates to the technical field of biomaterials. The bacteria-responsive nanofiber membrane is used for tympanic membrane repair, and comprises a plurality of overlapping nanofibers, wherein the nanofiber comprises a shell layer and a core layer, the components of the shell layer comprise synthetic polymer materials and bacteria-degradable natural polymer materials, the components of the core layer comprise antibacterial drugs, and can simultaneously achieve the effect of supporting the repair of the tympanic membrane epithelial cell layer and the adaptive antibacterial effect; the nanofiber material is a bioactive layer arranged on the outer side of the bacteria-responsive nanofiber membrane, the bioactive layer comprises bioactive components, and the bioactive components comprise one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor, and can simultaneously achieve the multi-stage sustained release effect of the bioactive components in the bioactive layer, the shell layer and the core layer and the effect of providing different types of regenerated materials for different stages of tympanic membrane repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomaterials, and in particular to a bacteria-responsive nanofiber membrane, a nanofiber material and a preparation method thereof. Background Art

[0002] The tympanic membrane is a translucent, thin-film-like soft tissue located between the external auditory canal and the middle ear. It includes an outer epithelial cell layer, an intermediate fiber layer, and an inner mucosal layer. It plays an important role in protecting the middle ear. Damage to the tympanic membrane can affect hearing conduction, leading to middle ear infection and hearing loss, and requires trauma repair. During the tympanic membrane trauma repair process, the repair and regeneration of the epithelial cell layer is faster than the repair and regeneration of the intermediate fiber layer, resulting in a lack of necessary mechanical support for the epithelial cell layer during regeneration, causing the epithelial cell layer to turn inward along the edge of the perforation, affecting the closure and repair of the tympanic membrane perforation.

[0003] In order to solve the above problems, myringoplasty under general anesthesia is usually used to repair tympanic membrane trauma. In most cases, autologous temporalis fascia or cartilage is used as a graft. However, the mechanical and acoustic properties of these autologous transplant materials are quite different from those of the human tympanic membrane, and they cannot compensate for hearing loss. In addition, autologous materials cause additional trauma to patients, and low-survival rate grafts also bring pain and burden to patients through secondary surgery. Furthermore, although implantable tissue repair materials can be used to promote the growth of induced tissue cells, this also faces the risk of bacterial infection. Therefore, high doses of antibacterial drugs are often used at the implant site in clinical surgery. However, excessive dosage of antibacterial drugs and improper use methods will cause "explosive release" of antibacterial drugs, which will have toxic side effects on normal human cells and produce multiple drug-resistant bacteria.

[0004] In order to reduce the risk of bacterial infection and eliminate the "burst release phenomenon" of antibacterial drugs, the existing technology uses polymers to coat antibacterial drugs and uses material post-modification methods to construct antibacterial materials to achieve the sustained release effect of antibacterial drugs, improve drug stability and efficacy, and reduce the dosage of antibacterial drugs. However, due to the constant changes in the number of bacterial infections and the toxicity of bacterial infections during tympanoplasty, this polymer coating structure cannot dynamically adjust the release rate of antibacterial drugs according to the number of bacterial infections and toxicity, and thus cannot achieve the effect of simultaneously reducing the risk of bacterial infection and eliminating the "burst release phenomenon" of antibacterial drugs. Summary of the invention

[0005] The problem solved by the present invention is how to provide a fiber membrane with the effect of supporting the repair of the tympanic membrane epithelial cell layer and the adaptive antibacterial effect.

[0006] The present invention provides a bacteria-responsive nanofiber membrane for tympanic membrane repair, comprising a plurality of overlapping nanofibers, wherein the nanofibers comprise a shell layer and a core layer, wherein the components of the shell layer comprise synthetic polymer materials and bacteria-degradable natural polymer materials, and the components of the core layer comprise antibacterial drugs.

[0007] Compared with the prior art, the present invention selects synthetic polymer materials and bacterially degradable natural polymer materials as shell components, wherein the synthetic polymer materials have excellent mechanical properties and low biodegradation rates, and multiple shell-core structured nanofibers overlap each other to provide necessary mechanical support for the repair of the epithelial cell layer of the tympanic membrane, and the bacterially degradable natural polymer materials have excellent bacterial degradation performance. When bacterial infection occurs near the nanofibers, the infected site is slightly acidic, and the bacteria release enzymatic virulence factors and degrade the bacterially degradable natural polymer materials, so that pores appear in the nanofiber shell within the bacterial action range, and the antibacterial drugs in the core layer are released, thereby achieving an antibacterial effect. In addition, since the nanofiber has a relatively large specific surface area, the drug can be efficiently loaded in the nanofiber. Furthermore, in the early stage of bacterial infection, the number of bacteria in the infected part will gradually increase, the bacterial degradation type natural polymer material in the shell layer will also be gradually degraded by bacteria, the shell layer pores will gradually increase, and the antibacterial drugs will be released faster to eliminate more bacteria, avoid the risk of more normal cells being infected by bacteria due to the slow release of antibacterial drugs, and be beneficial to the migration, value-added, differentiation and regeneration repair of tissue cells. Furthermore, when there is no bacterial infection, the antibacterial components loaded by the nanofibers will not be released, avoiding toxic and side effects on normal tissue cells of the human body, and ensuring good biocompatibility. It can be seen that the bacterial responsive nanofiber membrane of the present invention utilizes the difference between the normal tissue microenvironment of the human body and the part infected by bacteria to construct a bacterial responsive antibacterial nanofiber membrane, which can achieve the simultaneous support of the tympanic membrane epithelial cell layer repair effect and adaptive antibacterial effect.

[0008] Preferably, the synthetic polymer material is one or more of polylactic acid, polylactic acid-glycolic acid, polycaprolactone, polylactic acid-caprolactone copolymer and polylactic acid-glycolic acid-caprolactone copolymer.

[0009] Preferably, the bacterially degradable natural polymer material is one or more of hyaluronic acid, collagen, gelatin and polypeptide.

[0010] Preferably, the components of the shell layer also include biologically active components, and the biologically active components are one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor.

[0011] Preferably, the antibacterial drug is one or more of levofloxacin, ciprofloxacin hydrochloride, tetracycline hydrochloride, amoxicillin and nanosilver.

[0012] Preferably, the core layer also includes one or more of bioactive ingredients, synthetic polymer materials and bacteria-degradable natural polymer materials.

[0013] The present invention also provides a method for preparing a bacteria-responsive nanofiber membrane, which is used to prepare the aforementioned bacteria-responsive nanofiber membrane, comprising the following steps:

[0014] Step S1, taking a synthetic polymer material, a bacterially degradable natural polymer material and a bioactive component, dissolving them in a first solvent to obtain a shell solution with a mass fraction of 20-40%;

[0015] Step S2, taking an antibacterial drug and dissolving it in a second solvent to obtain a core layer solution with a mass fraction of 0.1-10%;

[0016] Step S3, using coaxial electrospinning technology, the shell layer solution and the core layer solution are respectively loaded into the coaxial outer spinning needle and inner spinning needle to prepare the bacteria-responsive nanofiber membrane.

[0017] In the prior art, synthetic polymer materials have excellent mechanical properties, but are limited to biocompatibility and bioactivity, and bacterial degradable natural polymer materials have excellent biocompatibility, but their mechanical strength is limited, and the spinning difficulty is relatively high. The bacterial responsive nanofiber membrane preparation method of the present invention uses coaxial electrostatic spinning technology to make a shell layer of synthetic polymer materials, bacterial degradable natural polymer materials and bioactive components, solves the problem that polymers are not easy to spin, and then loads antibacterial drugs on the core layer to improve drug stability, so as to obtain a bacterial responsive nanofiber membrane with a repair effect of supporting the tympanic epithelial cell layer and an adaptive antibacterial effect. In addition, the bacterial responsive nanofiber membrane obtained by the coaxial electrostatic spinning technology of the present invention has the characteristics of large specific surface area of ​​nanofibers, high porosity, and controllable diameter of nanofibers, which can simulate extracellular matrix fibers and have potential drug sustained release ability.

[0018] Preferably, the first solvent component in step S1 includes one or more of dimethyl sulfoxide, N,N-dimethylformamide, dichloromethane, and acetone, and the second solvent component in step S2 includes one or more of dimethyl sulfoxide, ethanol, ultrapure water, and acetic acid.

[0019] The present invention also provides a nanofiber material, including the aforementioned bacteria-responsive nanofiber membrane, wherein a bioactive layer is provided on the outside of the bacteria-responsive nanofiber membrane, the bioactive layer is composed of bioactive components, and the bioactive components include one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor.

[0020] Compared with the prior art, the nanofiber material of the present invention regulates the regeneration of the epithelial cell layer and the intermediate fiber layer of the tympanic membrane by setting a bioactive layer on the outside of the bacteria-responsive nanofiber membrane, and increases the regeneration speed of the epithelial cell layer and the intermediate fiber layer. When a subsequent bacterial infection occurs, the nanofibers in the bacteria-responsive nanofiber membrane release antibacterial drugs again to achieve the simultaneous promotion of cell proliferation and differentiation and antibacterial effects. The nanofiber material of the present invention can achieve a multi-stage sustained release effect of bioactive components in the bioactive layer, shell layer and core layer by adjusting the surface components of the bacteria-responsive nanofiber membrane, and provide different types of regeneration materials for different stages of tympanic membrane repair.

[0021] The present invention also provides a method for preparing a nanofiber material, comprising the following steps:

[0022] Step D1, obtaining the aforementioned bacteria-responsive nanofiber membrane;

[0023] Step D2, taking the bioactive component, dissolving it in a first solvent to obtain a first growth factor solution, and spraying the first growth factor solution onto the surface of the bacteria-responsive nanofiber membrane using an electrostatic spraying technique to obtain a primary nanofiber material;

[0024] Step D3, taking the bioactive component, dissolving it in the first solvent to obtain a second growth factor solution, and using an immersion method to immerse the primary nanofiber material in the second growth factor solution to obtain a secondary nanofiber material;

[0025] Step D4, repeating step D2 and / or step D3 until the desired nanofiber material is obtained.

[0026] Compared with the prior art, the method for preparing nanofiber materials of the present invention obtains bioactive layers of different thicknesses by repeatedly electrostatically spraying and impregnating bioactive components on bacteria-responsive nanofiber membranes, which can be applied to tissue regeneration in different patients and different parts to meet the needs of different bioactive components. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a scanning electron microscope image of the bacteria-responsive nanofiber membrane in Test Example 1 of the present invention;

[0028] Figure 2 The fluorescence images of the bacteria-responsive nanofiber membrane in Test Example 2 of the present invention, wherein the green fluorescence in (A) is the fluorescence image of the shell solution, the red fluorescence in (B) is the fluorescence image of the core solution, and the yellow fluorescence in (C) is the fluorescence image after the green fluorescence is superimposed and merged with the red fluorescence;

[0029] Figure 3The contact angle measurement results of the bacteria-responsive nanofiber membrane in Test Example 3 of the present invention, wherein (a) is the contact angle measurement result of the side of the bacteria-responsive nanofiber membrane away from the roller collector, and (b) is the contact angle measurement result of the side of the bacteria-responsive nanofiber membrane in contact with the roller collector;

[0030] Figure 4 The mechanical properties measurement results of the coaxial drug-loaded fiber membrane and the blended drug-loaded fiber membrane in Test Example 4 of the present invention;

[0031] Figure 5 The cumulative release rate measurement results of antimicrobial drugs of the coaxial drug-loaded fiber membrane and the blended drug-loaded fiber membrane in Test Example 5 of the present invention;

[0032] Figure 6 The antibacterial performance test results of the non-drug-loaded fiber membrane, the blended drug-loaded fiber membrane and the coaxial drug-loaded fiber membrane in Test Example 6 of the present invention, wherein (a) is the antibacterial rate result of the above three fiber membranes against Staphylococcus aureus, and (b) is the antibacterial rate result of the above three fiber membranes against Pseudomonas aeruginosa;

[0033] Figure 7 The bacterial response performance test results of the non-drug-loaded fiber membrane, the blended drug-loaded fiber membrane and the coaxial drug-loaded fiber membrane in Test Example 7 of the present invention, wherein (a) is the representative test result of the inhibition zone of Staphylococcus aureus and Pseudomonas aeruginosa and (b) is the quantitative result of the inhibition zone;

[0034] Figure 8 These are the test results of the adaptive antibacterial properties of the non-drug-loaded fiber membrane, the blended drug-loaded fiber membrane and the coaxial drug-loaded fiber membrane in Test Example 8 of the present invention, wherein (a) is the antibacterial drug release results of the above three fiber membranes under bacterial conditions, and (b) is the antibacterial drug release results of the above three fiber membranes under fibroblast conditions. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0036] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] In the description of the present invention, it should be noted that the terms "one side", "both sides", "the other side", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, or are the orientations or positional relationships in which the inventive product is usually placed when in use. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0038] In addition, the terms "comprising", "containing", and "having" are not restrictive, that is, other steps and other components that do not affect the results can be added. Unless otherwise specified, materials, equipment, and reagents are commercially available.

[0039] In addition, the terms "disposed", "provided with", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0040] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0041] The embodiment of the present invention provides a bacteria-responsive nanofiber membrane for tympanic membrane repair, including multiple overlapping nanofibers, the nanofibers including a shell layer and a core layer, the components of the shell layer including synthetic polymer materials and bacterially degradable natural polymer materials, and the components of the core layer including antibacterial drugs. Compared with the prior art, the embodiment of the present invention selects synthetic polymer materials and bacterially degradable natural polymer materials as shell layer components, wherein the synthetic polymer materials have excellent mechanical properties and low biodegradation rates, and multiple shell-core structured nanofibers overlap each other to provide necessary mechanical support for the repair of the epithelial cell layer of the tympanic membrane, and the bacterially degradable natural polymer materials have excellent bacterial degradation performance. When bacterial infection occurs near the nanofibers, the infected site is slightly acidic, and the bacteria will release enzymatic virulence factors and degrade the bacterially degradable natural polymer materials, so that pores appear in the nanofiber shell layer within the bacterial action range, and the antibacterial drugs in the core layer are released, thereby achieving an antibacterial effect. In addition, due to the small size of the nanofibers, the nanofibers in the bacterial infection site can release the amount of antibacterial drugs more accurately, avoiding the excessive release of antibacterial drugs and causing super bacteria, thereby causing harm to the human body. Furthermore, in the early stage of bacterial infection, the number of bacteria in the bacterial infection site will gradually increase, the bacterial degradation type natural polymer material in the shell layer will also be gradually degraded by bacteria, the fiber shell layer pores will gradually increase, and the antibacterial drugs will be released faster to eliminate more bacteria, avoid the risk of more normal cells being infected by bacteria due to the slow release of antibacterial drugs, and benefit the migration, value-added, differentiation and regeneration repair of tissue cells. Furthermore, when there is no bacterial infection, the antibacterial components loaded by the nanofibers will not be released, avoiding toxic and side effects on normal tissue cells of the human body, and ensuring good biocompatibility. It can be seen that the bacterial responsive nanofiber membrane of the embodiment of the present invention utilizes the difference between the normal tissue microenvironment of the human body and the bacterial infection site to construct a bacterial responsive antibacterial nanofiber membrane, which can achieve the simultaneous support of the tympanic epithelial cell layer repair effect and adaptive antibacterial effect.

[0042] As another embodiment, the synthetic polymer material is one or more of polylactic acid, polylactic acid-glycolic acid, polycaprolactone, polylactic acid-caprolactone copolymer and polylactic acid-glycolic acid-caprolactone copolymer. Among them, polylactic acid (PLA), also known as polylactide, is a polyester polymer biodegradable material obtained by polymerization with lactic acid as the main raw material. It has high tensile strength, high elongation and slow degradation rate. It can be used as the middle fiber layer of the tympanic membrane and provide mechanical support for the repair and regeneration of the epithelial cell layer. It can also be degraded and absorbed by normal human cells and various microorganisms. However, because its degradation rate is lower than that of bacterially degradable natural polymer materials, the nanofiber shell layer at the site infected by bacteria forms a porous structure. Polylactic acid-glycolic acid (PLGA) is a degradable polyester-type material made by copolymerization of lactic acid and glycolic acid (hydroxyacetic acid). It has good controllable degradation rate and biocompatibility. This is because the degradation of polylactic acid-glycolic acid is mainly through the hydrolysis of ester bonds. Due to the presence of hydroxyl groups in glycolic acid, the hydrophilicity of glycolic acid is stronger than that of lactic acid. As the proportion of glycolic acid in polylactic acid-glycolic acid increases, the hydrophilicity of polylactic acid-glycolic acid copolymer increases, absorbs more water, and the degradation rate increases; the degradation time of polylactic acid-glycolic acid with a ratio of 50 / 50 is 50-60 days, and the degradation time of polylactic acid-glycolic acid with a ratio of 85 / 15 is 150 days. Polycaprolactone (PCL) is an aliphatic polyester that can be degraded by hydrolysis under physiological conditions. It has many advantages such as no immunogenicity, no acid accumulation during degradation, good biocompatibility, strong flexibility, high mechanical strength and good blending compatibility. It can be used as a controlled release drug carrier, cell and tissue culture medium frame. In addition, polycaprolactone (PCL) has good drug permeability, but due to its strong crystallinity, its biodegradation rate is slow. The degradation half-life of high molecular weight polycaprolactone is more than one year, while the biodegradation rate of polylactide (PLA) is between that of polycaprolactone and polyglycolide (PGA). By adjusting the ratio of polylactide and polycaprolactone in the copolymer, a polylactic acid-caprolactone copolymer with excellent polymer degradation rate controllability, biocompatibility and biodegradability can be obtained. Polylactic acid-glycolic acid-caprolactone copolymer has the characteristics of fast degradation rate, good mechanical strength, strong collagen activity and fiber directionality, and can be used to improve the effect of bone tissue repair.

[0043] As another embodiment, the bacterial degradable natural polymer material is one or more of hyaluronic acid, collagen, gelatin and polypeptide. The embodiment of the present invention is used to respond to bacterial infection on the nanofiber by adding a bacterial degradable natural polymer material that matches the enzyme property virulence factor secreted by bacteria in the shell layer of the nanofiber, thereby achieving the adaptive antibacterial effect of the nanofiber. Specifically, hyaluronic acid is an important component of the extracellular matrix and constitutes an inter-tissue barrier in a significant amount. The hyaluronidase secreted by bacteria is a hydrolase that cuts hyaluronic acid into D-glucuronic acid and N-acetylglucosamine, which is used to increase the permeability of the interstitial matrix and can provide favorable conditions for the release of antibacterial drugs in the core layer of the nanofiber. Collagen, as an important component in human cells, supports the structure of cells and can prevent the loss of water in cells. The collagenase secreted by bacteria can specifically hydrolyze the three-dimensional helical structure of collagen under physiological pH and temperature conditions without damaging other proteins and tissues, further providing favorable conditions for the release of antibacterial drugs in the core layer of the nanofiber. Gelatin is a macromolecular hydrophilic colloid, which is the product of partial hydrolysis of collagen. The gelatinase secreted by bacteria can specifically interact with collagen and other extracellular matrix molecules, hydrolyze various types of animal proteins at a certain temperature and pH value, and can achieve the effect of macromolecular protein decomposition by controlling the degree of hydrolysis of animal proteins, thereby obtaining the required polypeptides, small peptides, and amino acid products. Polypeptides are formed by dehydration condensation of 10-100 amino acid molecules and are intermediate products of protein hydrolysis. The peptidases secreted by bacteria can decompose protein short peptides, among which the gelatinase in the peptidase can cut the GPLAV sequence (glycine-proline-leucine-glycine-valine) in the polypeptide to achieve degradation, and the coagulase in the peptidase can cut the G(D)FPAGA sequence (glycine-D-phenylalanine-proline-arginine-glycine-alanine) in the polypeptide to achieve degradation. As another embodiment, the components of the shell layer also include biologically active ingredients, and the biologically active ingredients are one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor, and transforming growth factor. The bioactive components are arranged in the nanofiber shell to improve the bioactivity and biocompatibility of the nanofiber membrane. Specifically, recombinant human epidermal growth factor (EGF) can promote wound healing, activate tyrosine kinase receptors, amino acid enzymes and protein kinase C, regulate the proliferation of various types of cells, and thus promote epidermal cell regeneration. Recombinant fibroblast growth factor is mainly divided into two categories: acidic fibroblast growth factor and basic fibroblast growth factor, both of which have the function of promoting the division and proliferation of various mammalian cells derived from the mesoderm and neuroectoderm, such as epithelial cells, endothelial cells, muscle cells, fibroblasts, etc. Transforming growth factor plays an important role in cell proliferation, differentiation, embryonic development, extracellular matrix formation, bone marrow formation and reconstruction, as well as tumor inhibition and metastasis and spread.

[0044] As another embodiment, the antibacterial drug is one or more of levofloxacin, ciprofloxacin hydrochloride, tetracycline hydrochloride, amoxicillin and nanosilver. Antibacterial drugs can effectively kill different types of bacteria, thereby avoiding bacterial infection. Specifically, levofloxacin has the advantages of high antibacterial activity, high bacterial clearance rate and good stability, and the effect of local medication in treating middle ear infection is better than systemic medication. Ciprofloxacin hydrochloride is a fluoroquinolone synthetic antibacterial drug with a wide antibacterial spectrum and strong antibacterial activity. Tetracycline hydrochloride is a broad-spectrum antibacterial drug that has an inhibitory effect on most Gram-positive and Gram-negative bacteria, and can inhibit Rickettsia, trachoma virus, etc. Amoxicillin belongs to a broad-spectrum antibacterial drug of the penicillin class, which has the characteristics of strong bactericidal and anti-inflammatory properties and strong cell membrane penetration ability. Nanosilver will continuously release silver ions. Due to its extremely small particle size, silver ions have a very strong binding ability with the cell wall / membrane of pathogens. They can freely enter the bacterial cell membrane at very low concentrations and quickly combine with the thiol of oxygen metabolism, blocking metabolism and making it inactive. In addition, when the bacteria are killed by silver ions, the silver ions remain on the original contact body and continue to repeat the action on the living bacteria until all bacteria are eliminated. Therefore, nanosilver can be used as a long-acting antibacterial material.

[0045] As another embodiment, the core layer also includes one or more of a bioactive component, a synthetic polymer material, and a bacterially degradable natural polymer material. Adding a bioactive component to the core layer can further enhance the bioactivity and biocompatibility of the nanofibers, adding a synthetic polymer material can further enhance the mechanical properties of the nanofibers, and adding a bacterially degradable natural polymer material can further enhance the biocompatibility of the nanofibers.

[0046] The present invention also provides a method for preparing a bacteria-responsive nanofiber membrane, which is used to prepare the aforementioned bacteria-responsive nanofiber membrane, and comprises the following steps:

[0047] Step S1, taking appropriate amounts of synthetic polymer materials, bacterially degradable natural polymer materials and bioactive components, dissolving them in a first solvent, and obtaining a shell solution with a mass fraction of 20-40%;

[0048] Step S2, taking an appropriate amount of antibacterial drug and dissolving it in a second solvent to obtain a core layer solution with a mass fraction of 0.1-10%;

[0049] Step S3, using coaxial electrospinning technology, the shell layer solution and the core layer solution are respectively loaded into the coaxial outer spinning needle and inner spinning needle to prepare the bacteria-responsive nanofiber membrane.

[0050] In the prior art, synthetic polymer materials have excellent mechanical properties, but are limited to biocompatibility and bioactivity. Bacterial degradable natural polymer materials have excellent biocompatibility, but their mechanical strength is limited, and the spinning difficulty is relatively high. The method for preparing the bacterial responsive nanofiber membrane of the embodiment of the present invention uses coaxial electrospinning technology to make a shell layer of synthetic polymer materials, bacterial degradable natural polymer materials and bioactive components, solves the problem that polymers are not easy to spin, and then loads antibacterial drugs on the core layer to improve drug stability, so as to obtain a bacterial responsive nanofiber membrane with a repair effect of supporting the tympanic epithelial cell layer and an adaptive antibacterial effect. In addition, the bacterial responsive nanofiber membrane obtained by the coaxial electrospinning technology of the embodiment of the present invention has the characteristics of large specific surface area of ​​nanofibers, high porosity, and controllable diameter of nanofibers, which can simulate extracellular matrix fibers and have potential drug sustained release ability.

[0051] As an improved method for preparing bacteria-responsive nanofiber membranes, the core layer solution in step S2 also includes one or more of bioactive components, synthetic polymer materials, and bacterially degradable natural polymer materials. Adding bioactive components to the core layer can further enhance the bioactivity and biocompatibility of the nanofibers, adding synthetic polymer materials can further enhance the mechanical properties of the nanofibers, and adding bacterially degradable natural polymer materials can further enhance the biocompatibility of the nanofibers.

[0052] As another improved way of preparing bacteria-responsive nanofiber membrane, the first solvent component in step S1 includes one or more of dimethyl sulfoxide, N,N-dimethylformamide, dichloromethane, and acetone, and the second solvent component in step S2 includes one or more of dimethyl sulfoxide, ethanol, ultrapure water, and acetic acid.

[0053] The embodiment of the present invention also provides a nanofiber material, including the aforementioned bacteria-responsive nanofiber membrane, wherein a bioactive layer is provided on the outside of the bacteria-responsive nanofiber membrane, and the bioactive layer is composed of bioactive components, and the bioactive components include one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor. Compared with the prior art, the nanofiber material of the embodiment of the present invention regulates the regeneration of the epithelial cell layer and the intermediate fiber layer of the tympanic membrane by providing a bioactive layer on the outside of the bacteria-responsive nanofiber membrane, and increases the regeneration speed of the epithelial cell layer and the intermediate fiber layer. When subsequent bacterial infection occurs, the nanofibers in the bacteria-responsive nanofiber membrane release antibacterial drugs again to achieve the simultaneous promotion of cell proliferation and differentiation and antibacterial effects. The nanofiber material of the embodiment of the present invention can achieve a multi-stage sustained release effect of bioactive components in the bioactive layer, shell layer and core layer by adjusting the surface components of the bacteria-responsive nanofiber membrane, and provide different types of regeneration materials for different stages of tympanic membrane repair.

[0054] As an improvement of the nanofiber material, the bioactive layer is located on one or both sides of the bacteria-responsive fiber membrane, and the number of the bioactive layer is one or more layers, so as to achieve different antibacterial drug sustained-release effects on different sides of the nanofiber material.

[0055] The present invention also provides a method for preparing a nanofiber material, comprising the following steps:

[0056] Step D1, obtaining the aforementioned bacteria-responsive nanofiber membrane;

[0057] Step D2, taking an appropriate amount of bioactive components, dissolving them in a first solvent to obtain a first growth factor solution, and spraying the first growth factor solution onto the surface of the bacteria-responsive nanofiber membrane using an electrostatic spraying technique to obtain a primary nanofiber material;

[0058] Step D3, taking an appropriate amount of bioactive components, dissolving them in the first solvent to obtain a second growth factor solution, and using an immersion method to immerse the primary nanofiber material in the second growth factor solution to obtain a secondary nanofiber material;

[0059] Step D4, repeating step D2 and / or step D3 until the desired nanofiber material is obtained.

[0060] Compared with the prior art, the method for preparing the nanofiber material of the embodiment of the present invention obtains bioactive layers of different thicknesses by repeatedly electrostatically spraying and impregnating bioactive components on the bacteria-responsive nanofiber membrane, which can be applied to tissue regeneration of different patients and different parts to meet the needs of different bioactive components. The embodiment of the present invention can release bioactive components in multiple stages to promote tympanic membrane repair. The bioactive components loaded on the surface by the impregnation method have the lowest adhesion and are released first. The bioactive components loaded by the electrostatic spraying method are released in the second stage. The bioactive components directly loaded on the nanofiber shell layer by adding to the shell layer solution are released in the third stage. The bioactive components loaded on the nanofiber core layer by adding to the core layer solution are released last as the polymer material degrades.

[0061] As an improved way of preparing nanofiber materials, the first growth factor solution in step D2 includes one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor, and the second growth factor solution in step D3 includes one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor.

[0062] Embodiment 1

[0063] A method for preparing a nanofiber material comprises the following steps:

[0064] Step S1, taking appropriate amounts of synthetic polymer materials, bacterially degradable natural polymer materials and bioactive components, dissolving them in acetone, and obtaining a shell solution with a mass fraction of 40%;

[0065] Step S2, taking appropriate amounts of antibacterial drugs, polymer materials, bacteria-degradable natural polymer materials and bioactive ingredients, dissolving them in ethanol, and obtaining a core layer solution with a mass fraction of 2%;

[0066] Step S3, using coaxial electrospinning technology, the shell solution and the core solution are respectively loaded into the coaxial outer spinning needle and the inner spinning needle to prepare a bacteria-responsive nanofiber membrane, wherein the outer spinning needle has a diameter of 1.0 mm, the inner spinning needle has a diameter of 0.5 mm, the spinning voltage is 18 kV, the receiving distance is 15 cm, the shell solution propulsion speed is 0.6 mL / h, the core solution propulsion speed is 0.2 mL / h, the temperature is 30°C, the humidity is 30%, and the produced bacteria-responsive nanofiber membrane is collected by a drum collector wrapped with smooth silicone oil paper, and placed in a vacuum drying oven for vacuum drying for 24 hours to remove residual acetone and ethanol;

[0067] Step S4, taking an appropriate amount of bioactive ingredients, dissolving them in acetone to obtain a first growth factor solution, and using electrostatic spraying technology to spray the first growth factor solution on the surface of the bacteria-responsive nanofiber membrane to obtain a primary nanofiber material, wherein the spraying voltage is 5 kV, the receiving distance is 15 cm, the solution propulsion speed is 0.4 mL / h, the temperature is 30° C., and the humidity is 35%. The roller wrapped with the nanofiber membrane collected by coaxial electrospinning is used as a collector to evenly spray the bioactive ingredients on the surface of the fiber membrane;

[0068] Step S5, taking an appropriate amount of bioactive components, dissolving them in acetone to obtain a second growth factor solution, and using an immersion method to immerse the primary nanofiber material in the second growth factor solution to obtain a secondary nanofiber material, wherein the immersion time is 1-8 hours. After the immersion is completed, washing with ultrapure water three times and drying in a vacuum environment;

[0069] Step S6, repeating step S4 and / or step S5 until the desired nanofiber material is obtained.

[0070] Test Example 1

[0071] The bacteria-responsive nanofiber membrane obtained in Example 1 was observed by scanning electron microscopy. The scanning electron microscopy photograph is as follows: Figure 1 As shown, the diameter of the nanofibers is 100-500 nm.

[0072] Test Example 2

[0073] The bacteria-responsive nanofiber membrane obtained in Example 1 was observed under a fluorescence microscope. The fluorescence microscope photo is shown in FIG. Figure 2As shown, the antibacterial drugs are uniformly wrapped in the nanofibers.

[0074] Test Example 3

[0075] The bacteria-responsive nanofiber membrane obtained in Example 1 was measured by a contact angle meter. The measurement results are as follows: Figure 3 As shown in the figure, the contact angle of one side of the bacteria-responsive nanofiber membrane is 130°, which is the hydrophobic side, and the contact angle of the other side of the bacteria-responsive nanofiber membrane is 90°, which is the hydrophilic side. During the coaxial electrospinning process, since the surface of the roller collector is attached with smooth silicone oil paper, the side of the bacteria-responsive nanofiber membrane in contact with the roller collector is smooth and hydrophilic, which can facilitate adhesion to the wound and absorb exudate. The other side of the bacteria-responsive nanofiber membrane is relatively rough and hydrophobic, which helps to block external environmental pollutants.

[0076] Test Example 4

[0077] The coaxial drug-loaded fiber membrane (i.e., bacteria-responsive nanofiber membrane) obtained in Example 1 was subjected to a mechanical property test, and the blended drug-loaded fiber membrane obtained by blending the shell layer and the core layer in Example 1 was subjected to a mechanical property test. The results are as follows: Figure 4 As shown, the Young's modulus of the coaxial drug-loaded fiber membrane and the blended drug-loaded fiber membrane are 425Mpa and 400Mpa, respectively, which is better than the 15-65Mpa of the middle fiber layer of the tympanic membrane, the tensile strength of the coaxial drug-loaded fiber membrane and the blended drug-loaded fiber membrane are 7.2Mpa and 8.5Mpa, respectively, which are between 6-12Mpa of the middle fiber layer of the tympanic membrane, and the elongation of the coaxial drug-loaded fiber membrane and the blended drug-loaded fiber membrane are 20.5% and 18.1%, respectively, which are between 10-20% of the middle fiber layer of the tympanic membrane or better than the elongation of the middle fiber layer of the tympanic membrane. It can be seen that the coaxial drug-loaded fiber membrane and the blended drug-loaded fiber membrane prepared in Example 1 can provide the necessary mechanical support for the repair of the epithelial cell layer in the regeneration of the tympanic membrane.

[0078] Test Example 5

[0079] By adding hyaluronidase to the culture medium, the release of antibacterial drugs by the drug-loaded fiber membrane under bacterial infection conditions was simulated in vitro, and then the coaxial drug-loaded fiber membrane obtained in Example 1 (i.e., the bacteria-responsive nanofiber membrane) and the blended drug-loaded fiber membrane obtained by blending the shell layer and the core layer in Example 1 were placed in the above culture medium to measure the adaptive antibacterial ability. The results are as follows: Figure 5As shown. Under enzyme-free conditions, after 15 days, the cumulative release rate of antibacterial drugs of the coaxial drug-loaded fiber membrane was 37%, and under enzyme conditions, after 15 days, the cumulative release rate of antibacterial drugs of the coaxial drug-loaded fiber membrane reached 98%, proving that the coaxial drug-loaded fiber membrane has adaptive antibacterial ability. Under enzyme-free conditions and enzyme conditions, the cumulative release rate of antibacterial drugs of the blended drug-loaded fiber membrane did not change significantly, indicating that the blended drug-loaded fiber membrane does not have adaptive antibacterial ability.

[0080] Test Example 6

[0081] The un-drug-loaded fiber membrane, the blended drug-loaded fiber membrane and the coaxial drug-loaded fiber membrane were cultured with Staphylococcus aureus and Pseudomonas aeruginosa in the culture medium for 6 h, 8 h and 10 h, respectively, and then the antibacterial performance was tested. The absorbance (OD value) at 600 nm was measured by a spectrophotometer. The results are as follows: Figure 6 As shown in the figure, the absorbance of the bacterial solution with the addition of the blended / coaxial drug-loaded fiber membrane decreased significantly, while the absorbance of the bacterial solution with the addition of the fiber membrane without antimicrobial drug loading remained at a high level, indicating that the two drug-loaded fiber membranes have a strong inhibitory effect on both bacteria.

[0082] Test Example 7

[0083] The antibacterial zone method was used to test the bacterial response performance. The fiber membrane without drug loading, the mixed drug loading fiber membrane containing the same amount of antibacterial drugs, and the coaxial drug loading fiber membrane were placed in the agar plate for diffusion, so that the growth of Staphylococcus aureus and Pseudomonas aeruginosa around the fiber membrane was inhibited to form an antibacterial zone. The results are as follows: Figure 7 The non-drug-loaded fiber membrane did not show an inhibition zone, while the inhibition zone area of ​​the coaxial drug-loaded fiber membrane was larger than that of the blended drug-loaded fiber membrane, indicating that under the premise of containing the same amount of antibacterial drugs, the amount of antibacterial drugs released by the coaxial drug-loaded fiber membrane was larger than that of the blended drug-loaded fiber membrane, confirming that the bacteria-responsive nanofiber membrane of Example 1 has better bacteria-responsive performance.

[0084] Test Example 8

[0085] Six culture media were taken, and un-drug-loaded fiber membranes, blended drug-loaded fiber membranes, and coaxial drug-loaded fiber membranes were added to two of the culture media, respectively. Three culture media with different fiber membranes were taken and added with Staphylococcus aureus for 10 hours, and then the release of the antibacterial drug (levofloxacin) in the above culture media was measured; another three culture media with different fiber membranes were taken and added with Pseudomonas aeruginosa for 10 hours, and then the release of the antibacterial drug (levofloxacin) in the above culture media was measured. The results are as follows: Figure 8 As shown in (a), OD 286 It is the characteristic peak of the antibacterial drug levofloxacin, OD 286The value represents the absorbance of the culture medium at 286nm, which indicates the amount of antimicrobial drugs released. Among them, the absorbance of the non-drug-loaded fiber membrane is mainly determined by the turbidity of the bacterial solution itself, and the absorbance of the blended / coaxial drug-loaded fiber membrane is determined by the bacterial solution, the bacterial fragments remaining after being killed by the released antimicrobial drugs, and the remaining antimicrobial drugs. Figure 8 (a) The results show that the absorbance of the coaxial drug-loaded fiber membrane is greater than that of the blended drug-loaded fiber membrane, indicating that after exerting the same antibacterial effect, the coaxial drug-loaded fiber membrane releases more antibacterial drugs into the culture medium, proving that the coaxial drug-loaded fiber membrane is more sensitive to bacterial infection and releases antibacterial drugs faster.

[0086] Take three culture media containing equal amounts of fibroblasts, add unloaded fiber membrane, blended drug-loaded fiber membrane and coaxial drug-loaded fiber membrane to each culture medium, and culture for 1 day and 2 days, then measure the release amount of antibacterial drug (levofloxacin) in the above culture medium. The results are as follows: Figure 8 (b) As shown. The results showed that the coaxial drug-loaded fiber membrane released a certain amount of antibacterial drugs. This was because during the spinning process of the coaxial drug-loaded fiber membrane, a small amount of core layer components containing antibacterial drugs inevitably adhered to the surface of the coaxial drug-loaded fiber membrane, causing it to release a small amount of antibiotics during the culture process with fibroblasts. Figure 8 (a) Compared with Figure 8 In (b), the antibacterial drug release of the blended / coaxial drug-loaded fiber membrane is in the opposite trend. Specifically, the antibacterial drug release of the blended drug-loaded fiber membrane is greater than that of the coaxial drug-loaded fiber membrane. Figure 8 The data show that in the absence of bacterial infection, the coaxial drug-loaded fiber membrane can better avoid the release of antibacterial drugs, while in the presence of bacterial infection, the coaxial drug-loaded fiber membrane can release antibacterial drugs faster, thereby achieving the effect of adaptive release of antibacterial drugs and adaptive antibacterial properties of the coaxial drug-loaded fiber membrane.

[0087] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing a nanofiber material, characterized in that: The following steps are involved: Step S1, taking a synthetic polymer material, a bacterially degradable natural polymer material and a biologically active component, dissolving them in acetone to obtain a shell solution with a mass fraction of 40%; Step S2, taking antibacterial drugs, synthetic polymer materials, bacterially degradable natural polymer materials and bioactive ingredients, dissolving them in ethanol, and obtaining a core layer solution with a mass fraction of 2%; Step S3, using coaxial electrospinning technology, the shell layer solution and the core layer solution are respectively loaded into the coaxial outer spinning needle and the inner spinning needle to prepare the bacteria-responsive nanofiber membrane, and the produced bacteria-responsive nanofiber membrane is collected by a roller collector wrapped with smooth silicone oil paper, and placed in a vacuum drying oven for vacuum drying for 24 hours to remove residual acetone and ethanol; Step S4, taking the bioactive component, dissolving it in acetone to obtain a first growth factor solution, and spraying the first growth factor solution onto the surface of the bacteria-responsive nanofiber membrane using an electrostatic spraying technique to obtain a primary nanofiber material; Step S5, taking the bioactive component, dissolving it in acetone to obtain a second growth factor solution, and using an immersion method to immerse the primary nanofiber material in the second growth factor solution to obtain a secondary nanofiber material. After the immersion is completed, washing it three times with ultrapure water and drying it in a vacuum environment; Step S6, repeating step S4 and / or step S5 until the desired nanofiber material is obtained; The bacteria-responsive nanofiber membrane is used for tympanic membrane repair; the bacteria-responsive nanofiber membrane comprises a plurality of nanofibers overlapping each other, the nanofibers comprise a shell layer and a core layer, the components of the shell layer comprise synthetic polymer materials, bacterially degradable natural polymer materials and bioactive ingredients, and the components of the core layer comprise antibacterial drugs, synthetic polymer materials, bacterially degradable natural polymer materials and bioactive ingredients; The synthetic polymer material is one or more of polylactic acid, polylactic acid-glycolic acid, polycaprolactone, polylactic acid-caprolactone copolymer and polylactic acid-glycolic acid-caprolactone copolymer; the bacterially degradable natural polymer material is one or more of hyaluronic acid, collagen and gelatin; the bioactive ingredient is one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor.

2. The method for preparing nanofiber material according to claim 1, characterized in that: The antibacterial drug is one or more of levofloxacin, ciprofloxacin hydrochloride, tetracycline hydrochloride, amoxicillin and nanosilver.

3. A nanofiber material, prepared by the nanofiber material preparation method as described in any one of claims 1-2, comprising a bacteria-responsive nanofiber membrane, wherein a bioactive layer is provided on the outside of the bacteria-responsive nanofiber membrane, wherein the bioactive layer is composed of bioactive ingredients, and the bioactive ingredients include one or more of recombinant human epidermal growth factor, recombinant fibroblast growth factor and transforming growth factor.

Citation Information

Patent Citations

  • Antibacterial nanofiber

    US20190091167A1

  • PCL patch tissue regeneration scaffold and method for manufacturing same

    US20200384151A1