A type of heterogeneous polymer donor material and its preparation method and application in the photovoltaic field

By constructing isomerized diazine polymer materials, the problems of complexity and high cost of synthesis of polymer donor materials in the prior art are solved, and efficient photoelectric conversion efficiency and low-cost organic solar cell materials are achieved.

CN115521444BActive Publication Date: 2024-11-12WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211230847.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-12
Estimated Expiration
2042-09-30

AI Technical Summary

Technical Problem

The synthesis steps of existing high-performance polymer donor materials are complex and costly, limiting the commercial application of organic solar cells.

Method used

The diazine polymer material constructed by isomerial strategies consists of different electron-donating units and diazine-containing electronic-deficient units. By optimizing the structure of the electron-deficient units and its preparation process, the cost is reduced and the photoelectric conversion efficiency is improved.

Benefits of technology

It realizes a low-cost and easy charge transport polymer material, with good planarity and adjustable energy levels, and is suitable for organic solar cells, significantly improving the photoelectric conversion efficiency and reducing synthesis complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115521444B_ABST
    Figure CN115521444B_ABST
Patent Text Reader

Abstract

The present invention discloses a type of isomeric polymer donor material. The structural formula of the polymer is shown in Formula I, II or III: #imgabs0# wherein R1 is C1-C 20 The alkyl group or one carbon atom on the alkyl group is replaced by an oxygen atom or a sulfur atom; X1 and X2 are selected from CN, F, Cl, CH3, OCH3, ester group or alkylthiophene. The present invention can effectively adjust the energy level and absorption spectrum of the polymer donor material; and the preparation cost involved is low and the reaction is easy, which will greatly reduce the synthesis cost of the polymer, and belongs to a photovoltaic material with good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optoelectronic materials and devices thereof, and in particular relates to a type of isomeric polymer donor material and a preparation method thereof and application in the photovoltaic field. Background Art

[0002] With the increasing global demand for natural resources such as coal, oil, and natural gas, and the increasingly prominent harm caused by traditional fuel energy to the environment, people are paying more and more attention to the research on renewable energy. Among various renewable energy sources, solar energy has become the focus of people's attention due to its unique advantages such as inexhaustible, clean and pollution-free. In recent years, countries around the world have begun to realize the importance of solar energy research and development, and have started to develop solar energy application technologies to improve the current situation of human dependence on traditional energy. Organic solar cells use organic semiconductors as active layer materials, with unique advantages such as simple material synthesis, low preparation cost, light weight, simple process, spin coating, evaporation, inkjet printing, screen printing and other methods to prepare films, can be prepared on flexible substrates, and easy to produce on a large scale. It shows great potential for research and development of organic solar cells, making this type of battery one of the frontier hotspots in the research of organic optoelectronic materials and devices in recent years.

[0003] Among the many existing polymer donor materials, DA-type polymers obtained by copolymerization of electron-donating units (D) and electron-deficient units (A) have advantages such as adjustable absorption spectra, molecular energy levels, and morphology, and are widely used to construct material skeleton structures. At present, although the reported high-performance polymer donor materials, such as PM6 / D18 (Adv. Mater., 2020, 32, 1908205; Adv. Funct. Mater. 2021, 2107934), show high photoelectric conversion efficiency, these polymers usually involve more synthesis steps and high preparation costs, which is not conducive to the commercial application of devices; how to effectively reduce the cost of active layer materials while ensuring high photovoltaic performance is an important research direction to accelerate the commercial application of organic solar cells. Summary of the invention

[0004] The main purpose of the present invention is to provide a diazine polymer material with good planarity, easy charge transfer, low cost and easy chemical modification in view of the problems and shortcomings of the prior art. By optimizing the structure of the electron-deficient unit and its preparation process, the obtained polymer is used as a donor material in an organic solar cell, thereby reducing the cost and still achieving a high photoelectric conversion efficiency.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A class of polymer donor materials constructed by isomerization strategy, which is composed of different electron-donating (D) units and electron-deficient (A) units containing diazine structures, and its structural formula is shown in Formula I, II or III:

[0007]

[0008] In the formula, R1 is C1~C 20 The alkyl group or one carbon atom on the alkyl group is substituted by an oxygen atom or a sulfur atom; X1 and X2 are selected from CN, F, Cl, CH3, OCH3, an ester group or an alkylthiophene.

[0009] In the above solution, the molecular weight of the polymer material is 30,000 to 600,000.

[0010] In the above scheme, the structural formula of the electron donating unit is shown in Formula IV;

[0011]

[0012] In the formula, Y is selected from H, F or Cl; R2 is C1~C 20 The alkyl group or one of the carbon atoms on the alkyl group is replaced by an oxygen atom or a sulfur atom.

[0013] The preparation method of the above-mentioned polymer material with a diazine structure includes the following steps: adding an electron-donating unit monomer, an electron-deficient unit monomer and a catalyst into an organic solvent and mixing them evenly, carrying out a heat-insulating reaction at 100 to 150° C. and in a protective atmosphere, reacting for 12 to 96 hours, and then settling and extracting to obtain the diazine polymer material.

[0014] In the above scheme, the molar ratio of the electron-donating unit monomer, the electron-deficient unit monomer and the catalyst is 1:1:(0.03-0.15).

[0015] In the above scheme, the structural formula of the electron-deficient unit monomer is shown in Formula V, and the structural formula of the electron-donating unit monomer is shown in Formula VI;

[0016]

[0017]

[0018] Wherein, Y is selected from H, F, Cl; R1, R2 are C1~C 20 The alkyl group or one carbon atom on the alkyl group is substituted by an oxygen atom or a sulfur atom; X1 and X2 are selected from CN, F, Cl, CH3, OCH3, an ester group or an alkylthiophene.

[0019] In the above scheme, the catalyst is tetrakis(triphenylphosphine)palladium or tris(dibenzylideneacetone)dipalladium, etc.; the organic solvent is toluene, o-xylene, chlorobenzene or a mixed solvent formed by any one of the three solvents and DMF.

[0020] Furthermore, in the mixed solvent, the volume ratio of any one of toluene, o-xylene, and chlorobenzene to DMF is (15-1):1.

[0021] In the above scheme, the protective atmosphere can be nitrogen or argon.

[0022] In the above scheme, the method for preparing the electron-deficient unit monomer described in formula I comprises the following steps:

[0023] 1) Using bromoalkane as a raw material, a Grignard reagent is prepared in the presence of magnesium chips, iodine and an organic solvent, and the Grignard reagent is added dropwise to a 3-bromothiophene solution to react and prepare an alkylthiophene; then, under the conditions of n-butyl lithium and tributyltin chloride, hydrogen is extracted from the 5th position of the alkylthiophene and stannane is added to obtain an alkyl-containing thiophene stannane;

[0024] 3-amino-6-bromopyrazine-2-carbonitrile is subjected to diazotization reaction (the amino group is converted into bromine) to prepare 3,6-dibromopyrazine-2-carbonitrile;

[0025] 2) subjecting the obtained alkyl-containing thienylstannane to a dehalogenation coupling reaction with 3,6-dibromopyrazine-2-carbonitrile to obtain a precursor of the acceptor (A) unit, which is then subjected to a bromination reaction with N-bromosuccinimide (NBS) to obtain the electron-deficient unit monomer (A unit monomer).

[0026] In the above scheme, the number of carbon atoms in the brominated alkane is 1 to 20.

[0027] In the above scheme, the temperature of the diazotization reaction is -10 to 50°C and the time is 2 to 12 hours.

[0028] In the above scheme, the temperature of the dehalogenation coupling reaction is 80-120° C. and the time is 5-24 hours.

[0029] The present invention also includes the use of polymer donor materials with different electron-donating (D) units and electron-deficient (A) units containing diazine structures as active layer materials or transport layer materials in optoelectronic devices.

[0030] Specifically, the above polymer materials can be used in organic solar cells, perovskite solar cells, organic light emitting diodes, organic detectors, etc.

[0031] The six-membered monocyclic diazines electron-deficient unit containing two nitrogen atoms used in the present invention has two nitrogen atoms on the ring that are sp 2Hybridization, an electron on the p orbital participates in cyclic conjugation, so that it has excellent photoelectric properties; its good planarity makes it easy to form π-π stacking, which is conducive to charge transfer within the molecule, and isomerization will lead to different electron cloud densities; and its strong electron-withdrawing ability, with different electron-donating (D) units, prepares different DA copolymers; in the polymer donor material, by modifying the active site of the diazine electron-deficient unit, the energy level and absorption spectrum of the polymer donor material can be effectively adjusted; in addition, the present invention also has the advantages of low price and easy preparation, which will greatly reduce the synthesis cost of the polymer, and belongs to a photovoltaic material with good application prospects.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] 1) The polymer of the present invention is an electron-deficient unit of a diazine structure prepared from 3-amino-6-bromopyrazine-2-carbonitrile as a raw material, which has a large number of chemically modifiable sites, can effectively adjust the absorption and energy level of the polymer molecule, and is applied to optoelectronic materials to greatly improve the photovoltaic performance of the polymer donor material;

[0034] 2) The electron-deficient unit of the diazine structure has good planarity and is easy to form π-π stacking, which is conducive to charge transfer within the molecule; the preparation method is simple, other raw materials for preparing monomers are relatively common, and the synthesis steps are relatively few; it is applied to polymer donor materials for organic solar cells, reducing the complexity of polymer donor synthesis; BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The structural formula of the bit polymers PDz-1 and IT-4F;

[0036] Figure 2 The UV-visible absorption spectra of the polymer PDz-1 obtained in the present invention in o-dichlorobenzene solution (room temperature) and in a thin film state;

[0037] Figure 3 The electrochemical cyclic voltammetry curve of the polymer PDz-1 obtained in the present invention is shown in FIG. 1 , using a 0.1 M tetrabutylammonium hexafluorophosphate anhydrous acetonitrile solution as the electrolyte solution, and a scan rate of 0.1 V / s;

[0038] Figure 4 Energy level distribution diagram of polymer PDz-1 and IT-4F;

[0039] Figure 5 This is the JV curve of the organic solar cell prepared by PDz-1:Y6 prepared using the polymer donor and small molecule acceptor Y6 obtained in the practice of the present invention. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0041] In the following examples, chlorothienylbenzodithiophene (BDT-2Cl; chloroBDT) was prepared according to the reference (NanoEnergy, 2018, 48: 413-420).

[0042] Example 1

[0043] A polymer with chloro-BDT (BDT-2Cl) as D unit and 3,5-di(2-ethylhexane)thiophene-substituted s-trichloroazine as A unit, and a preparation method thereof comprises the following steps:

[0044] 1) Preparation of dialkylthiophene-substituted diazines electron-deficient unit monomers, the synthesis route is as follows:

[0045]

[0046] The specific preparation steps are as follows:

[0047] 1) Under anhydrous and oxygen-free conditions, bromoisooctane (57.97 g, 300 mmol) and tetrahydrofuran (15 mL) were placed in a constant pressure dropping funnel, and slowly added dropwise to a 250 mL three-necked flask containing magnesium chips (14.58 g, 600 mmol), iodine (2-3 grains) and tetrahydrofuran (30 mL). After the addition was complete, the mixture was refluxed for 2 h to obtain a Grignard reagent; the obtained Grignard reagent was slowly added dropwise to a 500 mL three-necked flask containing a tetrahydrofuran solution (50 mL) of 3-bromothiophene (45.65 g, 280 mmol) at 0°C, and refluxed for 12 h; after the reaction was completed, the mixture was quenched with deionized water, extracted with dichloromethane, the organic phase was dried with anhydrous NaSO4, and the solvent was removed; and compound 1 was obtained by distillation under reduced pressure with a yield of 80%; 1 HNMR (400MHz, CDCl3), δ (ppm): 7.23 (m, 1H), 6.92 (s, 1H), 6.91 (d, J = 3.6Hz, 1H), 2.58 (d, J = 6.8Hz, 2H), 1.56 (m, 1H), 1.27 (m, 8H), 0.88 (m, 6H);

[0048] 2) Under nitrogen atmosphere, the obtained compound 1 (25.56 g, 120 mmol) and tetrahydrofuran (120 mL) were placed in a two-necked flask, and n-butyl lithium (48 mL, 120 mmol) was added dropwise at -78 ° C. After stirring for 1 h, tributyltin chloride (20.13 g, 126 mmol) was slowly added, and the mixture was reacted at -78 ° C. After 30 min, the mixture was moved to room temperature for reaction for 12 h, and the reaction was completed; the mixture was extracted with dichloromethane, washed with saturated sodium chloride, dried over anhydrous sodium sulfate, the solvent was removed by rotation, and the mixture was distilled under reduced pressure to obtain compound 2, which was directly used in the next step without post-treatment;

[0049] 3) Under nitrogen atmosphere, 3-amino-6-bromopyrazine-2-carbonitrile (0.38 g, 2 mmol), copper bromide (0.07 g, 3 mmol), t-BuONO (0.4953 g, 4.8 mmol) and 20 mL of anhydrous acetonitrile were placed in a two-necked flask and reacted at room temperature for 2 h. After the reaction, 0.3 g of aminosulfonic acid in a 3 mmol / L hydrochloric acid solution was poured into the mixture, and dichloromethane was added for extraction. After drying over anhydrous NaSO4, the solvent was removed, and the mixture was separated and purified by silica gel column chromatography with petroleum ether / dichloromethane (volume ratio of 1:1) as the eluent to obtain compound 3 with a yield of 75%; 1 HNMR (400MHz, CDCl3), δ (ppm): 8.55 (s, 1H);

[0050] 4) Under nitrogen protection, compound 2 (1.91 g, 4 mmol) and compound 3 (0.52 g, 2 mmol), catalyst Pd(PPh3)4 (0.14 g, 0.12 mmol) and 10 mL of anhydrous toluene were added in sequence, and the reaction was carried out at 100° C. for 48 h. After the reaction was completed, the mixture was quenched with deionized water, and dichloromethane was added for extraction. After drying with anhydrous NaSO4, the solvent was removed, and the mixture was separated and purified by silica gel column chromatography. The eluent was petroleum ether / dichloromethane (volume ratio of 4:1), and compound 4 was obtained with a yield of 80%; 1 HNMR(400MHz, CDCl3), δ(ppm):8.92(s,1H),8.08(s,1H),7.55(s,1H),7.19(s,1 H),7.12(s,1H),2.59(d,J=6.8Hz,4H),1.64(m,2H),1.30(m,16H),0.90(m,12H);

[0051] 5) Compound 4 (0.50 g, 1 mmol) was dissolved in 15 mL of chloroform, and NBS (0.356 g, 2 mmol) was added after dissolution, and the reaction was allowed to react overnight; the mixture was quenched with deionized water, and dichloromethane was added for extraction. After drying with anhydrous NaSO4, the solvent was removed, and the mixture was separated and purified by silica gel column chromatography, and the eluent was petroleum ether / dichloromethane (volume ratio of 4:1), to obtain compound 5 (dialkylthiophene substituted diazirine electron-deficient unit monomer), with a yield of 85%; 1 HNMR (400MHz, CDCl3), δ (ppm): 8.85 (s, 1H), 7.97 (s, 1H), 7.41 (s, 1H), 2.53 (d, J = 6.8Hz, 4H), 1.64 (m, 2H), 1.30 (m, 16H), 0.90 (m, 12H);

[0052] (2) Preparation of diazine polymers, the synthetic route is as follows:

[0053]

[0054] The specific preparation steps are as follows: under nitrogen protection, compound 5 (0.1298 g, 0.2 mmol) and chlorothienylbenzodithiophene (BDT-2Cl) (0.1950 g, 0.2 mmol), catalyst Pd(PPh3)4 (0.0138 g, 0.012 mmol) and 5 mL of anhydrous toluene were added in sequence, and the reaction was carried out at 100°C for 48 h; the crude product was precipitated with methanol, and then extracted with acetone, n-hexane, dichloromethane and chloroform in sequence; chloroform was rotary evaporated, methanol was added for precipitation, and the final polymer product PDz-1 was obtained by suction filtration with a yield of 80%.

[0055] The polymer PDz-1 obtained in this example was tested for optical properties, electrochemical properties, photovoltaic properties, etc. The results are shown below: Figures 2 to 5 .

[0056] Depend on Figure 2 As shown, at a concentration of 10 -2 The absorption peak of the obtained polymer PDz-1 in the solution of 0.1 g / mL of o-dichlorobenzene was located at 552 nm, which was attributed to the electronic transition of the main structure of the compound. PDz-1 was dissolved in o-dichlorobenzene to prepare a solution with a concentration of 0.1 g / mL, and then a film with a thickness of 80 to 160 nm was obtained by rotary evaporation coating. The polymer PDz-1 showed a high molar absorption coefficient at 400 to 630 nm, indicating that it was sensitive to light absorption in this wavelength range, which was conducive to the generation of excitons and would greatly increase the short-circuit current (J) of the device. sc), in the thin film state, polymer PDz-1 shows strong π-π stacking, which is beneficial to the transport of carriers. The edge absorption of polymer PDz-1 film is 636nm. According to formula E g =1240 / λ, band gap E g It is 1.94eV.

[0057] The redox process of polymer PDz-1 was tested by electrochemical cyclic voltammetry to obtain the initial redox potential relative to ferrocene, and then the frontier orbital energy levels (HUMO level and LUMO level) of the corresponding material can be estimated: using a three-electrode system, the synthesized polymer PDz-1 was dissolved in chloroform, a solution with a concentration of 10 mg / mL was dropped on a glassy carbon electrode to prepare a thin film, which was then placed in an acetonitrile electrolyte solution containing 0.1 M tetrabutylammonium hexafluorophosphate for testing. The entire test process required nitrogen protection, and the scan rate was 0.1 V / s. The results are shown in Figure 3 .from Figure 3 It can be seen that polymer PDz-1 has an irreversible redox process only at the anode, and the corresponding initial oxidation potential is 0.76 eV. According to the formula HOMO = -(E Ox,onset +4.8)eV, we can calculate the HOMO energy level of polymer PDz-1 to be -5.56eV. The LUMO energy level is -3.62eV (LUMO = HUMO + Eg) based on the optical band gap and HUMO of the material. The LUMO energy level difference between the polymer and the receptor is 0.3eV, which ensures that there is enough driving force to promote the dissociation of excitons, so that the charge is effectively transferred and a higher short-circuit current (J sc ).

[0058] Depend on Figure 4 It can be seen that there is a good energy level match between polymer PTz-1 and Y6. At the same time, the polymer exhibits a high absorption coefficient in the range of 400-630nm and is a good donor material.

[0059] Solar cells were fabricated using a conventional device configuration of ITO / PEDOT:PSS / PDz-1:Y6 / PDINN / Ag. Polyethylenedioxythiophene:polystyrene sulfonate (PEDOT:PSS weight ratio of 1:1) was spin-coated onto an ITO substrate at 4000 rpm for 30 s and then dried at 150 °C for 15 min. A donor and acceptor mixture (donor to acceptor weight ratio of 1:1.05) was dissolved in chloroform (the total concentration of the mixture solution was 10–20 mg mL -1, DIO was selected as an additive with a volume ratio of 0.25%) and stirred at room temperature overnight. The blended solution was spin coated at 1800r / min for 30s. After coating, the active layer was annealed on a hot plate at 100°C for 3 minutes. A PDINN layer was coated on the active layer, and then a metallic silver layer with a thickness of about 50-200nm was vacuum evaporated on the active layer as the cathode of the photovoltaic device. According to the obtained JV curve ( Figure 5 ), we can measure the short-circuit current J of the resulting device sc 26.877 mA cm -2 , open circuit voltage V oc It is 0.846V, the fill factor FF is 71.06%, and the energy conversion efficiency PCE is 16.16%.

[0060] The polymer PDz-1 obtained by the present invention is used as a donor material in an organic solar cell to obtain a higher photoelectric conversion efficiency, and is a good organic photovoltaic material.

[0061] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A class of heterogeneous polymer donor materials, characterized in that: Its structural formula is as follows: Among them, the structural formula of the electron donating unit is: Wherein, Y is selected from Cl; the structural formula of R2 is The preparation method of the electron-deficient unit monomer comprises the following steps: 1) Using bromoalkane as a raw material, a Grignard reagent is prepared in the presence of magnesium chips, iodine and an organic solvent, and the Grignard reagent is added dropwise to a 3-bromothiophene solution to react and prepare an alkylthiophene; then, under the conditions of n-butyl lithium and tributyltin chloride, hydrogen is extracted from the 5th position of the alkylthiophene and stannane is added to obtain an alkyl-containing thiophene stannane; 3-amino-6-bromopyrazine-2-carbonitrile is subjected to diazotization reaction to prepare 3,6-dibromopyrazine-2-carbonitrile; 2) subjecting the obtained alkyl-containing thienylstannane to a dehalogenation coupling reaction with 3,6-dibromopyrazine-2-carbonitrile to obtain a precursor of the acceptor unit, and then subjecting the precursor to a bromination reaction with N-bromosuccinimide to obtain the electron-deficient unit monomer.

2. The heterogeneous polymer donor material according to claim 1, characterized in that Its molecular weight is 30,000 to 600,000.

3. The method for preparing the isomeric polymer donor material according to any one of claims 1 to 2, characterized in that: The method comprises the following steps: adding electron-donating unit monomers, electron-deficient unit monomers and catalysts into an organic solvent and mixing them uniformly; carrying out heat preservation reaction under heating and protective atmosphere; and then carrying out sedimentation and extraction to obtain the isomeric polymer donor material.

4. The preparation method according to claim 3, characterized in that: The molar ratio of the electron-donating unit monomer, the electron-deficient unit monomer and the catalyst is 1:1:(0.03-0.15).

5. The preparation method according to claim 3, characterized in that: The insulation reaction temperature is 100-150° C. and the time is 12-96 hours.

6. The preparation method according to claim 3, characterized in that: The catalyst is tetrakis(triphenylphosphine)palladium or tris(dibenzylideneacetone)dipalladium; the organic solvent is one or more of toluene, o-xylene and chlorobenzene, or a mixed solvent formed by any one of the three solvents and DMF.

7. Use of the heterogeneous polymer donor material according to any one of claims 1 to 2 or the heterogeneous polymer donor material prepared by the preparation method according to any one of claims 3 to 6 in an organic solar cell.