A fiber membrane, and its preparation method and application
By preparing a fiber membrane with a porous structure, the problems of low adsorption capacity and poor selectivity of the adsorbent are solved, efficient adsorption and selective separation of chromium ions are achieved, and it is suitable for efficient recovery of chromium ions.
Patent Information
- Application Number
- CN202211176606.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-09-26
AI Technical Summary
Existing adsorbents have problems with low adsorption capacity, poor selectivity, and difficulty in separating from the solution in adsorbing chromium ions.
Polyacrylonitrile and pore-forming agent are mixed in the same solvent, and a porous structure fiber membrane is prepared through electrospinning, heat treatment and oximation modification, which is used for efficient adsorption and selective separation of chromium ions.
It achieves efficient adsorption and selective separation of chromium ions, with an adsorption capacity of up to 124.7mg/g. It still maintains an adsorption capacity of 58.2mg/g after repeated use, and shows an exclusive adsorption effect in the presence of multi-metal ions.
Smart Images

Figure CN115532072B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the fields of environmental management and chromium ion recovery, and in particular to a fiber membrane, and a preparation method and application thereof. Background Art
[0002] Chromium mainly exists in nature as trivalent chromium and hexavalent chromium. Hexavalent chromium is more toxic and is identified as a Class I carcinogen. Its emission concentration is strictly controlled by relevant national departments.
[0003] At present, the commonly used methods for removing hexavalent chromium include redox method, precipitation method, adsorption method, etc. Among them, adsorption method is more effective for treating low-concentration heavy metals. Commonly used adsorbents are mostly powders and granules, and commonly used adsorbents include activated carbon, resin, hydrotalcite, zeolite, etc., which are used for wastewater treatment in the form of adsorption columns / beds or adsorption towers.
[0004] However, due to the limitations of the material, properties and performance of the adsorbent, the prior art still has problems such as low adsorption capacity and poor selectivity for chromium.
[0005] In view of this, it is necessary to provide a fiber membrane, a preparation method and application thereof, so as to at least solve or alleviate one or more technical defects of the above-mentioned adsorbent being difficult to separate from the solution, having a low adsorption capacity for chromium and having poor selectivity. Summary of the invention
[0006] In order to solve the problems of adsorption performance and selectivity of existing adsorbents, the first purpose of the present invention is to provide a fiber membrane and a preparation method thereof, aiming to obtain a chromium adsorbent with high adsorption capacity and good selectivity for chromium.
[0007] The second object of the present invention is to provide an application of a fiber membrane in separating chromium, aiming to specifically achieve efficient and selective separation of chromium.
[0008] To achieve the above object, the present invention provides a method for preparing a fiber membrane, comprising the steps of:
[0009] S1, mixing polyacrylonitrile and a pore-forming agent in the same solvent to obtain a casting solution; wherein the pore-forming agent comprises one or both of polyvinyl pyrrolidone and polyvinyl alcohol;
[0010] S2, subjecting the casting solution to electrostatic spinning to obtain a base film;
[0011] S3, heat-treating the base film in an aqueous solution to obtain a film to be modified;
[0012] S4, performing oximation modification treatment on the membrane to be modified to obtain the fiber membrane.
[0013] Furthermore, the mass ratio of the polyacrylonitrile to the pore-forming agent is 1.5 to 2.5;
[0014] The total mass of the polyacrylonitrile and the pore-forming agent accounts for 18 to 25 wt % of the mass of the casting solution;
[0015] The solvent includes one or two of N,N-dimethylacetamide and N,N-dimethylformamide;
[0016] The voltage of the electrospinning process is 13-15KV;
[0017] The temperature of the heat treatment is 60 to 80°C;
[0018] The oximation modification treatment comprises: placing the membrane to be modified in a modification liquid, and then heating the modification liquid containing the membrane to be modified at 60-70° C. for 60-120 min;
[0019] The modified liquid contains hydroxylamine hydrochloride and sodium carbonate, and the molar ratio of the hydroxylamine hydrochloride to the sodium carbonate is 1.5 to 2.5.
[0020] The present invention provides a fiber membrane, which is prepared by any one of the preparation methods described above.
[0021] The present invention provides a use of a fiber membrane as described in any one of the above items in separating chromium.
[0022] The present invention provides a method for separating chromium, comprising: contacting a liquid to be treated containing chromium ions with a fiber membrane as described in any one of the above items to separate the chromium ions in the liquid to be treated, and obtaining the fiber membrane with chromium ions attached thereto.
[0023] Furthermore, the liquid to be treated contains hexavalent chromium and other metal ions, and the other metal ions include Cu 2+ , Pb 2+ 、Cd 2+ 、Ni 2+ 、Au 3+ One or more of the .
[0024] Furthermore, before the contacting and / or during the contacting, the pH of the liquid to be treated is controlled at 2-4.
[0025] Furthermore, the pH of the liquid to be treated is controlled at 2-3.
[0026] Furthermore, the fiber membrane with chromium ions attached thereto is desorbed and restored, and the restored fiber membrane is brought into contact with another liquid to be treated to separate the chromium ions in the other liquid to be treated.
[0027] Furthermore, the desorption process includes: placing the fiber membrane with chromium ions attached thereto in an alkaline solution;
[0028] The recovery process includes placing the fiber membrane after the desorption in an acid solution.
[0029] Compared with the prior art, the present invention has at least the following advantages:
[0030] 1. The present invention provides a fiber membrane and a preparation method thereof. By introducing a pore-forming agent and performing heat treatment in an aqueous solution, the porous structure of the fiber membrane is laid; after a series of pretreatments, the fiber membrane is oximated to ensure the final formation of the fiber membrane structure, obtain an amidoximated composite porous fiber membrane, and make the composite porous fiber membrane have efficient adsorption and selectivity for chromium.
[0031] 2. The present invention also provides an application of a fiber membrane in separating chromium. That is, through in-depth research on the fiber membrane prepared by the present invention, it is unexpectedly found that the fiber membrane has excellent performance in chromium ion adsorption. For example, the adsorption capacity and adsorption selectivity of chromium ions can be improved.
[0032] Specifically, in the present invention, based on a specific fiber membrane, efficient separation and recovery of chromium ions can be achieved, the operation is simple, and it has better selectivity for chromium, with an adsorption capacity of up to 124.7 mg / g; and after repeated use for 3 times, the fiber membrane provided by the present invention can also achieve an adsorption capacity of 58.2 mg / g for chromium.
[0033] In addition, in the present invention, when chromium ions coexist with other metal ions in the same solution, the specific fiber membrane will also perform exclusive selective adsorption. For example, when one or more metal ions such as lead, nickel, zinc, copper, cadmium, and gold coexist in the mixed solution, the present invention can still selectively separate chromium. Based on this, since the separation method of the present invention has the ability to efficiently and selectively separate chromium ions, and the fiber membrane is easily separated from the solution, it is expected to provide a new strategy for the adsorption and separation of chromium ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0035] Figure 1 is a cross-sectional SEM image of the composite porous fiber membrane prepared in Example 1; Figure 1It can be seen from the figure that there is a rich pore structure inside the fibers of the composite porous fiber membrane.
[0036] Figure 2 is a SEM image of the composite porous fiber membrane obtained in Example 1; Figure 2 It can be seen that there are a large number of pore structures on the surface of a single fiber, which greatly increases the specific surface area of the fiber and creates basic conditions for the adsorption of chromium.
[0037] Figure 3 This is a data effect diagram of the chromium adsorption amount under different adsorption times in Example 1.
[0038] Figure 4 This is a data effect diagram of the chromium adsorption amount at different pH values in Example 2.
[0039] Figure 5 This is a data effect diagram of the composite porous fiber membrane in Example 3 that simultaneously adsorbs multiple ions.
[0040] The realization of the objectives, functional features and advantages of the present invention will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0043] Furthermore, the technical solutions between the various embodiments of the present invention can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention. It should be known to those skilled in the art that due to the existence of experimental errors, even if the tests are conducted under the same conditions twice, the data of the two test results will fluctuate slightly, which does not affect the understanding of this application.
[0044] In order to improve the separation efficiency of chromium, the present invention provides a method for preparing a fiber membrane, comprising the steps of:
[0045] S1, mixing polyacrylonitrile (PAN) and a pore-forming agent in the same solvent to obtain a casting solution.
[0046] Wherein, the molecular weight of the polyacrylonitrile may be 100,000 to 250,000.
[0047] The pore-forming agent includes one or both of polyvinyl pyrrolidone and polyvinyl alcohol; specifically, it may be polyvinyl pyrrolidone.
[0048] The mass ratio of the polyacrylonitrile to the pore-forming agent may be 1.5 to 2.5; the total mass of the polyacrylonitrile and the pore-forming agent in the casting solution may account for 18 to 25 wt %.
[0049] The solvent may include one or both of N,N-dimethylacetamide and N,N-dimethylformamide; specifically, it may be N,N-dimethylacetamide.
[0050] The casting solution can be prepared in a specific manner as follows: polyacrylonitrile and polyvinyl pyrrolidone are added to (N,N-dimethylacetamide) in a certain ratio, and the mixture is mixed evenly at 40-60°C.
[0051] The present invention has found that precise control of the ratio of PAN to pore-forming agent is conducive to obtaining nanofiber membranes with high porosity ratios and helps improve the adsorption capacity and selectivity of the obtained fiber membranes for chromium. When the ratio of the two is too large, not only is the pore structure underdeveloped, but the adsorption capacity of chromium is also reduced; when the ratio of the two is too small, the pore diameter inside the fiber increases, the supporting performance decreases, and the structural strength of the fiber membrane decreases.
[0052] S2, subjecting the casting solution to electrostatic spinning to obtain a base membrane.
[0053] The voltage of the electrospinning process may be 13-15 KV, and the flow rate of the casting solution during the electrospinning process may be 1-2 mL / h.
[0054] It should be understood that the electrospinning process can be specifically as follows: the casting liquid is loaded into a syringe, the syringe and the needle are connected with a Teflon catheter, and the distance between the needle and the roller is adjusted; then, high voltage static electricity is connected to the needle, and the flow rate of the casting liquid and the winding speed of the roller are controlled. After a period of time, the base film can be obtained.
[0055] S3, heat-treating the base film in an aqueous solution to obtain a film to be modified.
[0056] The temperature of the heat treatment may be 60 to 80° C., and the duration of the heat treatment may be 1.5 to 3 hours.
[0057] The heat treatment may specifically be: fixing the base film on a non-woven fabric, then placing the non-woven fabric with the base film fixed thereon in an aqueous solution, and then heating the aqueous solution at 70° C. for 2 hours.
[0058] S4, performing oximation modification treatment on the membrane to be modified to obtain the fiber membrane.
[0059] The oximation modification treatment may include: placing the membrane to be modified in a modification liquid, and then heating the modification liquid containing the membrane to be modified at 60-70° C. for 60-120 min;
[0060] The modified liquid may contain hydroxylamine hydrochloride and sodium carbonate; in the modified liquid, the molar ratio of the hydroxylamine hydrochloride to the sodium carbonate may be 1.5-2.5, and the concentration of the hydroxylamine hydrochloride may be 0.4-0.6 mol / L.
[0061] In the above embodiment, after the polymer polyacrylonitrile (PAN) is mixed with the pore-forming agent in a certain ratio, electrospinning is carried out, and the electrospinning voltage, aqueous solution heat treatment, and oxime modification treatment are jointly controlled to produce a composite nanofiber membrane with a porous structure.
[0062] It should be noted that the present invention can increase the effective area of the fiber membrane and the binding property between the fiber membrane and the substance to be adsorbed by forming a large number of porous structures on the fiber membrane; after oxime modification, a large number of amidoxime functional groups can be loaded in the porous structure of the fiber membrane, which can further ensure the binding property between the fiber membrane and the substance to be adsorbed and enable the fiber membrane to have excellent ion exchange capacity and selectivity.
[0063] It should also be noted that the present invention unexpectedly found that the above fiber membrane has excellent adsorption effect and selectivity for hexavalent chromium anions. That is, the fiber membrane in the present invention is an adsorption-type nanofiber membrane with good morphology, high adsorption capacity and good chromium selectivity.
[0064] Since the above preparation method can obtain a fiber membrane with excellent performance, high adsorption and high selectivity for chromium, the present invention also provides a fiber membrane prepared by any of the preparation methods described above.
[0065] The composite porous fiber membrane for selectively separating chromium ions prepared by the present invention has a developed pore structure; and it is found that the fiber membrane prepared by the present invention can unexpectedly find that the membrane material has an unexpected adsorption effect on chromium. Simply increasing the specific surface area of the fiber or using amidoximation modification cannot achieve the adsorption effect of the fiber membrane prepared by the present invention. The rich pore structure and amidoximation modification give the fiber membrane a new adsorption mechanism and method.
[0066] Therefore, based on the above-mentioned fiber membrane, the present invention also provides an application of a fiber membrane as described in any one of the above items in separating chromium.
[0067] As a specific application of separating chromium by fiber membrane, due to the selectivity and high removal rate of trace components of the adsorption method, the present invention provides a method for separating chromium in combination with the adsorption method, comprising: contacting a liquid to be treated containing chromium ions with the fiber membrane to separate the chromium ions in the liquid to be treated, and obtaining the fiber membrane with chromium ions attached thereto.
[0068] The process of contacting the liquid to be treated and the fiber membrane may be: placing the fiber membrane in the liquid to be treated and oscillating or stirring the liquid to be treated. It may also be: using the fiber membrane as a filter medium and allowing the liquid to be treated to pass through the fiber membrane. It may also be: immersing the fiber membrane in the liquid to be treated.
[0069] As an illustration of the liquid to be treated, the liquid to be treated contains hexavalent chromium and other metal ions, and the other metal ions include Cu 2+ , Pb 2+ 、Cd 2+ 、Ni 2+ 、Au 3+ One or more of the .
[0070] It should be understood that the chromium ion may be hexavalent chromium, which mainly exists in the form of anions of oxygen-containing acid radical ions in the solution, including Cr2O7 2- , HCrO 4- 、CrO4 2- 、Cr2O7 2- wait.
[0071] Under different pH conditions, the main form of hexavalent chromium will change. For example, when the pH exceeds 7, the main form of hexavalent chromium is CrO4 2- ; At pH 7, the main form of hexavalent chromium is HCrO 4- and CrO4 2- Coexistence; when the pH is below 7, the main form of hexavalent chromium is HCrO 4- and Cr2O7 2- .
[0072] In the present invention, Au 3+ Usually comes from the hydrochloric acid system, when Au 3+ When it comes from the hydrochloric acid system, Au also exists in the form of anions, specifically AuCl4 - It should be noted that the liquid to be treated in this application usually comes from a hydrochloric acid system. Therefore, Au 3+ The existing form is usually AuCl4- In the present invention, whether at different pH or in the hydrochloric acid system, Cu 2+ , Pb 2+ 、Cd 2+ 、Ni 2+ The ionic form does not change.
[0073] Exemplarily, the liquid to be treated in the present invention can be derived from a hydrochloric acid leaching solution of electronic waste (containing hexavalent chromium and may also contain the above-mentioned other metal ions), or can be derived from an electrolyte containing hydrochloric acid (containing hexavalent chromium and may also contain the above-mentioned other metal ions).
[0074] It is worth noting that pH will affect the separation effect of chromium in the present invention. Before and / or during the contact, the pH of the liquid to be treated can be controlled at 2-4 to improve the adsorption effect of the fiber membrane on chromium.
[0075] Preferably, in order to further enhance the adsorption effect of the fiber membrane on chromium and ensure the selective separation of chromium, the pH of the liquid to be treated can be controlled at 2-3 before and / or during the contact.
[0076] It should be emphasized that the fiber membrane of the present invention can be reused multiple times. During the reuse process, the fiber membrane with chromium ions attached needs to be desorbed and restored, and then the restored fiber membrane is contacted with another liquid to be treated to separate the chromium ions in the other liquid to be treated.
[0077] The desorption is mainly for separating the chromium attached to the fiber membrane.
[0078] The desorption process may be: placing the fiber membrane with chromium ions attached thereto in an alkaline solution and then oscillating the alkaline solution; the alkaline solution may be a sodium hydroxide solution and / or a potassium hydroxide solution, and the concentration of the alkaline solution is not less than 1 mol / L.
[0079] The recovery is mainly to ensure the chromium adsorption performance of the fiber membrane during the next use.
[0080] The recovery process may be: placing the fiber membrane after the desorption in an acid solution; then oscillating the acid solution; the acid solution may be a hydrochloric acid solution and / or a sulfuric acid solution; + The concentration is not less than 1 mol / L.
[0081] To facilitate those skilled in the art to understand the present invention, examples are given below:
[0082] Example 1
[0083] Preparation of fiber membrane:
[0084] (1) Preparation of casting solution
[0085] Casting solution: 150,000 molecular weight polyacrylonitrile, PVP (polyvinyl pyrrolidone) and solvent (N, N-dimethylacetamide) are mixed uniformly at 60°C;
[0086] The mass ratio of polyacrylonitrile to PVP is 2:1; the total mass of polyacrylonitrile and PVP accounts for 21 wt % in the casting solution.
[0087] (2) Preparation of basement membrane
[0088] The casting liquid obtained in step (1) was loaded into a 10 mL syringe, and the syringe and the needle were connected with a Teflon catheter. The distance between the needle and the roller was adjusted to 15 cm. A 14 KV high voltage static electricity was connected to the needle. The casting liquid flow rate was 1 mL / h, and the roller winding speed was 300 rpm / min. The process was continued for 2 h to obtain a base film.
[0089] (3) Preparation of porous fiber membrane
[0090] The base membrane obtained in step (2) was fixed on the non-woven fabric with a clip and heated in an aqueous solution at 70° C. for 2 h to obtain a porous fiber membrane.
[0091] (4) Preparation of composite porous fiber membrane
[0092] 0.5 g of the porous fiber membrane obtained in step (3) is placed in 100 mL of the modified liquid and treated at 65°C for 90 min; the treated base membrane is then freeze-dried in a vacuum at -23°C (4 h) to obtain a composite porous fiber membrane, i.e., the fiber membrane required in the present invention.
[0093] The modified liquid is a mixed solution of hydroxylamine hydrochloride and anhydrous sodium carbonate (in the modified liquid, the molar concentration of hydroxylamine hydrochloride is 0.5 mol / L, and the molar ratio of hydroxylamine hydrochloride to anhydrous sodium carbonate is 2:1).
[0094] The composite porous fiber membrane prepared in this example is shown in Figure 1-2 As shown:
[0095] from Figure 1 It can be seen from the figure that there are abundant pore structures inside the fibers of the composite porous fiber membrane prepared in this embodiment.
[0096] from Figure 2 It can be seen that there are a large number of pore structures on the surface of the fiber prepared in this embodiment, which creates basic conditions for the adsorption of chromium.
[0097] (5) Composite porous fiber membrane adsorbs Cr(VI) in water
[0098] Weigh 0.05 g of the fiber membrane prepared in step (4) and add it to 50 mL of Cr(VI) solution at room temperature for a static adsorption test.
[0099] The Cr(VI) solution used in the adsorption test was a simulated solution prepared using potassium dichromate, the initial concentration of Cr(VI) was 300 mg / L, and the pH of the solution was 3.0.
[0100] The above adsorption test was conducted under oscillation at room temperature with an oscillation speed of 100 rpm. The supernatant was taken at regular intervals and the concentration change of Cr(VI) in the solution was detected by ICP-OES to calculate the adsorption amount of the adsorption separation membrane.
[0101] See also Figure 3 As shown, the test found that after 5 hours of adsorption, the adsorption capacity of Cr(VI) by the composite porous fiber membrane was 124.7 mg / g.
[0102] After repeating for 3 times, the adsorption amount of Cr(VI) was 58.2 mg / g (adsorption data for 5 h).
[0103] Among them, after each adsorption, the composite porous fiber membrane is desorbed and recovered in turn.
[0104] The desorption process is as follows: the adsorbed fiber membrane is placed in 50 mL of a 1 mol / L NaOH solution, shaken at 100 rpm for 1 h at a room temperature of 25°C, and then the fiber membrane is taken out and rinsed three times in clean water.
[0105] The recovery operation process is as follows: the fiber membrane washed with clean water is placed in 50mL of H2SO4 with a concentration of 0.5mol / L, and oscillated at a speed of 100rpm for 1h at a room temperature of 25°C, and then the fiber membrane is washed in clean water until the pH value is neutral.
[0106] Example 2
[0107] Static adsorption test at different pH:
[0108] The difference between this embodiment and embodiment 1 is that the pH of the Cr(VI) solution in the adsorption process of step (5) is adjusted (see the table below for details), and the other conditions are the same as those in embodiment 1;
[0109] The test results of the first adsorption (5h adsorption data) are shown in the following table:
[0110] pH Adsorption capacity (mg / g) 2 91.5 3 132.4 4 66.7 5 31.2 6 24.6 7 10.8
[0111] See also Figure 4As shown, it can be seen that with the increase of solution pH value, the adsorption amount of chromium by the fiber membrane first increases and then decreases, reaching the highest value when the pH value is equal to 3.
[0112] The results show that the fiber membrane of the present invention has an excellent adsorption effect on chromium, and a specific pH value significantly improves the adsorption effect.
[0113] Example 3
[0114] Static selective adsorption test of multi-ion solution
[0115] A mixed solution is prepared with chromium Cr(VI), copper Cu(Ⅱ), lead Pb(Ⅱ), cadmium Cd(Ⅱ), nickel Ni(Ⅱ) and gold Au(Ⅲ) in a molar concentration ratio of 1:1:1:1:1:1.
[0116] In the mixed solution, the concentration of Cr(VI) is 0.984 mmol / L, the concentrations of copper Cu(Ⅱ), lead Pb(Ⅱ), cadmium Cd(Ⅱ), nickel Ni(Ⅱ), and gold Au(Ⅲ) are all 0.984 mmol / L, and the pH value of the mixed solution is 3.
[0117] In the mixed solution of this embodiment, copper Cu(II), lead Pb(II), cadmium Cd(II), and nickel Ni(II) all exist separately in their respective ionic states; the main existing form of Cr(VI) is HCrO 4- and Cr2O7 2- , Au(Ⅲ) exists in the form of AuCl4 - .
[0118] During adsorption, the fiber membrane prepared in Example 1 was added to the mixed solution at a rate of 0.05 g / L, and then the solution was shaken at room temperature at a rotation speed of 100 rpm.
[0119] After the adsorption is completed, the desorption and recovery process of the fiber membrane is as shown in Example 1.
[0120] The static selective adsorption characteristics of the gold adsorption separation membrane were evaluated. The results of adsorption for 5 hours (first time) are shown in the following table:
[0121] Metal ions Adsorption capacity (mg / g) Cr(Ⅵ) 95.7 Cu(Ⅱ) 4.6 Pb(Ⅱ) 5.5 Ni(Ⅱ) 2.3 Cd(Ⅱ) 3.9 Au(Ⅲ) 35.4
[0122] See also Figure 5 As shown, it can be seen that in water bodies where multiple ions coexist, the fiber membrane will give priority to Cr(VI).
[0123] Among them, Cu(Ⅱ), lead Pb(Ⅱ), cadmium Cd(Ⅱ), and nickel Ni(Ⅱ) mainly exist in the solution in the form of cations, while Cr(Ⅵ) mainly exists in the form of anions. The different existence forms lead to inconsistent adsorption mechanisms. The electrostatic adsorption rate of the fiber membrane and anions is higher than the chelating chemical adsorption of cations.
[0124] Although Au(Ⅲ) and Cr(Ⅵ) exist in the same form in the solution, they have different pH advantage ranges. When the pH is 3.0, it will significantly promote the selective adsorption of Cr(Ⅵ) by the fiber membrane.
[0125] The comprehensive results show that the fiber membrane has very excellent selective adsorption characteristics for chromium.
[0126] Comparative Example 1
[0127] The difference between this comparative example and Example 1 is that no porous structure is constructed and there is no preparation of a porous fiber membrane. The details of this comparative example are as follows:
[0128] (1) Preparation of casting solution
[0129] Casting solution: polyacrylonitrile with a molecular weight of 150,000 and a solvent (N,N-dimethylacetamide) are uniformly mixed at 60° C. in weight percentages of 21 wt % and 79 wt %.
[0130] (2) Preparation of base film (same as Example 1).
[0131] (3) Preparation of composite fiber membrane (same as Example 1, only the porous fiber membrane is replaced by the base membrane of step 2).
[0132] (4) Composite fiber membrane adsorbs Cr(VI) in water; Note: The fiber membrane of this comparative example is derived from step 3 of this comparative example, and the other processes are the same as step 5 of Example 1.
[0133] The test found that in this comparative example, after 5 hours of adsorption, the adsorption amount of Cr(VI) by the composite porous fiber membrane was 28.3 mg / g.
[0134] Comparative Example 2
[0135] The difference between this comparative example and Example 1 is that no amidoximation modification is performed, as follows:
[0136] (1) Preparation of casting solution (same as in Example 1).
[0137] (2) Preparation of base film (same as Example 1).
[0138] (3) Preparation of porous fiber membrane (same as Example 1).
[0139] (4) The porous fiber membrane adsorbs Cr(VI) in water; Note: The fiber membrane of this comparative example is derived from step 3 of this comparative example, and the other processes are the same as step 5 of Example 1.
[0140] The test found that in this comparative example, after adsorption for 5 hours, the adsorption amount of Cr(VI) by the porous fiber membrane was 0.6 mg / g.
[0141] It can be seen that the adsorption effect of the composite porous fiber membrane on Cr(VI) is not simply the sum of the porous structure and the amine oxime modification effect. By controlling the structure and conditions described in the present invention, a material with high adsorption performance for Cr(VI) can be unexpectedly obtained.
[0142] Comparative Example 3
[0143] The difference between this comparative example and Example 1 is that the ratio of PAN and pore-forming agent PVP is changed, as follows:
[0144] (1) Preparation of casting solution
[0145] Casting solution: 150,000 molecular weight polyacrylonitrile, PVP (polyvinyl pyrrolidone) and solvent (N, N-dimethylacetamide) are mixed uniformly at 60°C;
[0146] The mass ratio of polyacrylonitrile to PVP is 1:1; the total mass of polyacrylonitrile and PVP accounts for 21 wt % in the casting solution.
[0147] (2) Preparation of base film (same as Example 1).
[0148] (3) Preparation of porous fiber membrane (same as Example 1).
[0149] (4) Preparation of composite porous fiber membrane (same as Example 1).
[0150] (5) Composite porous fiber membrane adsorbs Cr(VI) in water; Note: The fiber membrane of this comparative example is derived from step 4 of this comparative example, and the other processes are the same as step 5 of Example 1.
[0151] The test found that in this comparative example, after adsorption for 5 hours, the adsorption amount of Cr(VI) by the composite porous fiber membrane was 53.8 mg / g.
[0152] Comparative Example 4
[0153] The difference between this comparative example and Example 1 is that the amidoximation modification of the fiber membrane is changed to carboxylation modification, as follows:
[0154] (1) Preparation of casting solution (same as in Example 1).
[0155] (2) Preparation of base film (same as Example 1).
[0156] (3) Preparation of porous fiber membrane (same as Example 1).
[0157] (4) Preparation of carboxylated porous fiber membrane.
[0158] The specific modification steps are as follows: 0.5 g of the porous fiber membrane in step (3) is mixed with 100 mL of 1 mol / L NaOH solution, shaken at 70°C and 100 rpm for 1 hour, and then washed with clean water to obtain a carboxyl-modified porous fiber membrane material.
[0159] (5) Carboxylated porous fiber membrane adsorbs Cr(VI) in water
[0160] 0.05 g of the carboxyl-modified porous fiber membrane material was added to 50 mL of Cr(VI) solution at room temperature for a static adsorption test with an adsorption time of 5 h.
[0161] The Cr(VI) solution used in the adsorption test was a simulated solution prepared using potassium dichromate, the initial concentration of Cr(VI) was 300 mg / L, and the pH of the solution was 3.0.
[0162] The above adsorption test was conducted under oscillation at room temperature with an oscillation speed of 100 rpm. The supernatant was taken at regular intervals and the concentration change of Cr(VI) in the solution was detected by ICP-OES to calculate the adsorption amount of the adsorption separation membrane.
[0163] The test found that after 5 hours of adsorption, the adsorption capacity of the carboxylated porous fiber membrane in this comparative example for Cr(VI) was 12.7 mg / g.
[0164] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a fiber membrane, characterized in that: Includes steps: S1, mixing polyacrylonitrile and a pore-forming agent in the same solvent to obtain a casting solution; wherein the pore-forming agent comprises one or both of polyvinyl pyrrolidone and polyvinyl alcohol; The mass ratio of the polyacrylonitrile to the pore-forming agent is 1.5-2.5; the total mass of the polyacrylonitrile and the pore-forming agent accounts for 18-25wt% of the mass of the casting solution; the solvent includes one or two of N,N-dimethylacetamide and N,N-dimethylformamide; S2, subjecting the casting solution to electrostatic spinning to obtain a base film; The voltage of the electrospinning process is 13-15 KV, and the flow rate of the casting solution during the electrospinning process is 1-2 mL / h; S3, heat-treating the base film in an aqueous solution to obtain a film to be modified; The temperature of the heat treatment is 60-80°C, and the duration of the heat treatment is 1.5-3h; S4, sequentially performing oximation modification treatment and freeze-vacuum drying on the membrane to be modified to obtain the fiber membrane; The oximation modification treatment includes: placing the membrane to be modified in a modification liquid, and then heating the modification liquid containing the membrane to be modified at 60-70° C. for 60-120 min; wherein the modification liquid contains hydroxylamine hydrochloride and sodium carbonate, the molar ratio of the hydroxylamine hydrochloride to the sodium carbonate is 1.5-2.5, and the concentration of the hydroxylamine hydrochloride is 0.4-0.6 mol / L.
2. A fiber membrane, characterized in that: The preparation is carried out by the preparation method as claimed in claim 1.
3. Use of the fiber membrane as claimed in claim 2 in separating chromium.
4. A method for separating chromium, characterized in that: include: A liquid to be treated containing chromium ions is brought into contact with the fiber membrane as claimed in claim 2 to separate the chromium ions in the liquid to be treated, thereby obtaining the fiber membrane to which the chromium ions are attached.
5. The method for separating chromium according to claim 4, characterized in that: The liquid to be treated contains hexavalent chromium and other metal ions, and the other metal ions include Cu 2+ , Pb 2+ 、Cd 2+ 、Ni 2+ 、Au 3+ One or more of the .
6. The method for separating chromium according to claim 4, characterized in that: Before the contacting and / or during the contacting, the pH of the liquid to be treated is controlled at 2-4.
7. The method for separating chromium according to claim 6, characterized in that: The pH of the liquid to be treated is controlled at 2-3.
8. The method for separating chromium according to any one of claims 4 to 7, characterized in that: The fiber membrane with chromium ions attached thereto is desorbed and restored, and the restored fiber membrane is brought into contact with another liquid to be treated to separate the chromium ions in the other liquid to be treated.
9. The method for separating chromium according to claim 8, characterized in that: The desorption process comprises: placing the fiber membrane with chromium ions attached thereto in an alkaline solution; The recovery process includes placing the fiber membrane after the desorption in an acid solution.