A method for controlling the local flatness of a single crystal silicon wafer for integrated circuits
The key factors in the double-sided chemical mechanical polishing process are determined through empirical equations, which solves the problem of local flatness control of single crystal silicon wafers, achieves high-precision flatness requirements for integrated circuit chips, and meets the technical indicators of advanced processes.
Patent Information
- Application Number
- CN202110723069.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-06-29
AI Technical Summary
In large-scale integrated circuit manufacturing, the local flatness of single-crystal silicon wafers caused by the double-sided chemical mechanical polishing process is difficult to control, which affects the reliability and integration of integrated circuit chips. The existing process parameters are fixed and cannot meet the requirements of different technical indicators.
The key factors of double-sided chemical mechanical polishing are determined through empirical equations, such as the rotation speed and pressure of the disk and planetary wafers, etc. to control the local flatness of the single crystal silicon wafer. Empirical equations (1) to (4) are used to calculate the rotation and pressure. The contribution coefficient and compensation constant of flatness determine the optimal process parameters.
It achieves precise control of the local flatness of single-crystal silicon wafers and meets the technical requirements of the integrated circuit process of 100nm and below, especially the advanced process requirements of 28nm and below, ensuring the stability and quality of the product.
Smart Images

Figure CN115533624B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of processing and manufacturing large-size single-crystal silicon wafers for large-scale integrated circuits, specifically to a method for controlling local flatness in a double-sided polishing process for silicon wafers, and in particular to a method for controlling the number of revolutions and pressure in the double-sided polishing process. Background Art
[0002] Single crystal silicon wafers are the basic key materials for the manufacture of ultra-large-scale integrated circuit chips, accounting for about 30% of the total cost of integrated circuit chips. As the diameter of single crystal silicon wafers becomes larger and larger, the feature size of integrated circuit chips becomes smaller and smaller, and the integration of integrated circuits becomes higher and higher, the flatness error of single crystal silicon wafers will directly affect the focus of the photolithography system, the roughness affects the size and accuracy of the scribed lines, and the number and depth of defects will affect the reliability and integration of components. Therefore, there are higher technical requirements for the flatness of the surface of single crystal silicon wafers, so chemical mechanical polishing technology has become a key technology in large-scale integrated circuit manufacturing. Chemical mechanical polishing technology is a combination of mechanical polishing and chemical corrosion. In the actual production and processing process, chemical and mechanical actions alternate with each other, and multiple variables interact with each other. Slight changes in variables will affect the relationship between the contact between the silicon wafer, the polishing liquid and the polishing pad, resulting in uneven polishing and excessive local flatness.
[0003] When the silicon wafer diameter reaches 200mm or more, and the line width reaches below 100nm, especially below 28nm, most processes use double-sided chemical mechanical polishing. There are many factors that affect the local flatness of the double-sided chemical mechanical polishing process, including the polishing disc speed, the planetary disc speed, the pressure of the disc, the particle size of the particles in the polishing liquid, the concentration of the polishing liquid, the pH value of the polishing liquid, the flow rate of the polishing liquid, the inlet layout of the polishing liquid, the temperature of the polishing liquid, the type of polishing pad, the performance of the polishing pad, the service life of the polishing pad, the type of disc material, the disc cooling method, the cooling water flow and temperature of the upper and lower discs, etc. Although these factors all affect the final quality of the product and are the subject of theoretical analysis and research, in the actual processing process, these factors are mostly divided into three categories. The first category is non-adjustable factors, that is, factors that have been solidified before processing, such as the particle size of particles in the polishing liquid, the concentration of the polishing liquid, the pH value of the polishing liquid, the inlet layout of the polishing liquid, the type of polishing pad, the performance of the polishing pad, the type of disk material, the cooling method of the disk, etc.; the second category is factors with relatively small influencing coefficients, that is, factors with a very small adjustment range during the processing process and little effect on the flatness of the single silicon wafer, such as the flow rate of the polishing liquid, the temperature of the polishing liquid, the service life of the polishing pad, the cooling water flow and temperature of the upper and lower disks, etc.; the third category is key factors, that is, factors that play a key role in the performance of single crystal silicon wafers, such as the speed of the polishing disk, the speed of the planetary disk, the pressure of the disk, etc.
[0004] The influence of double-sided chemical mechanical polishing process factors on the local flatness of single-crystal silicon wafers is mutually restricted, especially the selection and control of key factors directly affect the local flatness of single-crystal silicon wafers. Therefore, most manufacturers currently use the method of fixing the key factor process parameters for processing, that is, the key factors are processed using the same fixed process parameters during the processing. In this way, when the local flatness technical indicators required by the integrated circuit process are different, it is easy to produce that the local flatness of the final product does not meet the requirements, and cannot meet the large-scale stable supply of integrated circuit chips or the indicator requirements of customers. Summary of the invention
[0005] To solve the above problems, the purpose of the present invention is to provide a method for controlling the local flatness of single-crystal silicon wafers for integrated circuits. According to the technical index requirements of the local flatness of single-crystal silicon wafers required for integrated circuit chip manufacturing, the values of the key factors affecting double-sided chemical mechanical polishing are determined through empirical equations summarized on the basis of a large number of experiments, thereby achieving a method for controlling the local flatness.
[0006] To achieve the above purpose, the present invention adopts the following steps:
[0007] The first step is to determine the local flatness of the single crystal silicon wafer according to the customer's technical requirements for the single crystal silicon wafer. The applicable scope of the present invention is .
[0008] The second step is to determine the rotational flatness according to the empirical equation (1): ,
[0009] (1)
[0010] In the formula, It is the local flatness of the single crystal silicon wafer caused by the rotation of the large disk and the planetary wafer, referred to as rotation flatness; is the mean TTV of incoming materials, and the applicable range of this equation is: ; is the rotation contribution coefficient, and the empirical value of the present invention is: ; is the disk rotation speed; is the rotation speed of the planetary piece, and the applicable range of this equation is ; is the rotation compensation constant, and the empirical value of the present invention is ; is the rotation index, and the empirical value of the present invention is: ;
[0011] According to the research results of double-sided chemical mechanical polishing mechanism, it is required that the upper and lower disks rotate in opposite directions, and the planetary sheet rotates at the same speed relative to the upper and lower disks. According to the empirical equation (1), it can be seen that as the disk rotates The increase in the rotation of the large disk affects the local flatness of the single crystal silicon wafer caused by the rotation of the large disk and the planetary sheet. The impact gradually decreases;
[0012] when When , the disk speed is determined to be the minimum disk speed, recorded as: ;
[0013] when When , the disk speed is determined to be the maximum disk speed, recorded as: ;
[0014] The present invention requires that in the empirical equation (1) The value of and between.
[0015] The third step is to determine the rotation speed of the large plate in the actual process. After that, the rotation flatness in the actual process can be determined according to the empirical equation (1): Then, according to the empirical equation (2), the maximum value of the rotation pressure flatness is determined .
[0016] (2)
[0017] The fourth step is to determine the pressure flatness according to the empirical equation (3): ,
[0018] (3)
[0019] In the formula, is the pressure contribution coefficient, and the empirical value of the present invention is: ; is the pressure compensation constant, and the empirical value of the present invention is: ; is the polishing pad coefficient, and the empirical value of the present invention is: ; is the hardness of the polishing pad; is the Poisson's ratio of the polishing pad; n is the pressure index, and the empirical value of the present invention is: ;
[0020] It can be seen from the empirical equation (3) that as the pressure Increase in pressure flatness Rising, when pressure After rising to a certain value, the pressure flatness There will be an inflection point drop. This is because when the pressure increases to a certain level, the polishing liquid on the polishing pad is squeezed out, forming a situation where the polishing is performed by the polishing pad itself. At this time, although the pressure flatness changes little, the polishing speed will be greatly reduced. Therefore, the present invention takes the pressure at which the pressure flatness appears an inflection point as the theoretical maximum pressure. At this time, the pressure flatness obtained according to the empirical equation (3) is the maximum value of the theoretical pressure flatness .
[0021] The fifth step is to determine the maximum value of pressure flatness in the actual process. According to the empirical equation (4), the maximum value of theoretical pressure flatness is taken. and maximum value of rotation pressure flatness The minimum value in
[0022] (4)
[0023] Step 6: Calculate the maximum pressure in the actual process according to the empirical equation (3): , and according to the maximum pressure Determine the production process.
[0024] The large-size polished silicon wafer produced by the present invention fully meets the local flatness technical index requirements of the integrated circuit process of 100nm and below, especially the requirements of the advanced integrated circuit process of 28nm and below. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the change in the local flatness of the single crystal silicon wafer caused by the rotation of the large disk and the planetary wafer.
[0026] Figure 2 It is the local flatness change of single crystal silicon wafer caused by polishing pressure. DETAILED DESCRIPTION
[0027] Example 1
[0028] Polishing 300mm silicon wafers, customer technical requirements for local flatness of 0.5μm, incoming material TTV average of 1.5μm, planetary wafer rotation speed of 30rpm; according to the empirical equation (1) of the present invention, the minimum disk speed is determined to be 12.49rpm, the maximum disk speed is 14.98rpm, and this experiment uses a disk rotation speed of 12.49rpm as the production process; according to the equation (2) of the present invention, the maximum rotation pressure flatness is determined to be 0.25μm; according to the equation (3) of the present invention, the maximum theoretical pressure flatness is determined to be 0.35μm; according to the empirical equation (4), the minimum value of the maximum theoretical pressure flatness and the maximum rotation pressure flatness is taken as 0.25μm, and then according to the equation (3) of the present invention, the maximum pressure in the actual process is determined to be 14.47kpa.
[0029] 150 300mm silicon wafers were polished using this process, and the average local flatness was 0.36μm, which fully met customer requirements.
[0030] Example 2
[0031] Polishing 200mm silicon wafers, customer technical requirements for local flatness of 0.5μm, incoming material TTV average of 1.44μm, planetary wafer rotation speed of 30rpm; according to the empirical equation (1) of the present invention, the minimum disk speed is determined to be 12.49rpm, the maximum disk speed is 14.98rpm, and this experiment uses a disk rotation speed of 14.98rpm as the production process; according to the equation (2) of the present invention, the maximum rotation pressure flatness is determined to be 0.375μm; according to the equation (3) of the present invention, the maximum theoretical pressure flatness is determined to be 0.35μm; according to the empirical equation (4), the minimum value of the maximum theoretical pressure flatness and the maximum rotation pressure flatness is taken as 0.35μm, and then according to the equation (3) of the present invention, the maximum pressure in the actual process is determined to be 28.58kpa.
[0032] 150 200mm silicon wafers were polished using this process, and the average local flatness was 0.34μm, which fully met customer requirements.
[0033] Example 3
[0034] Polishing 300mm silicon wafers, customer technical requirements for local flatness of 0.15μm, incoming material TTV average of 0.85μm, planetary wafer rotation speed of 20rpm; according to the empirical equation (1) of the present invention, the minimum disk speed is determined to be 14.15rpm, the maximum disk speed is 14.74rpm, and this experiment uses a disk rotation speed of 14.15rpm as the production process; according to the equation (2) of the present invention, the maximum rotation pressure flatness is determined to be 0.075μm; according to the equation (3) of the present invention, the maximum theoretical pressure flatness is determined to be 0.11μm; according to the empirical equation (4), the minimum value of the maximum theoretical pressure flatness and the maximum rotation pressure flatness is taken as 0.075μm, and then according to the equation (3) of the present invention, the maximum pressure in the actual process is determined to be 14.34kpa.
[0035] 75 300mm silicon wafers were polished using this process, and the average local flatness was 0.12μm, fully meeting customer requirements.
[0036] Example 4
[0037] Polishing 200mm silicon wafers, customer technical requirements for local flatness of 0.15μm, incoming material TTV average of 0.78μm, planetary wafer rotation speed of 20rpm; according to the empirical equation (1) of the present invention, the minimum disk speed is determined to be 14.15rpm, the maximum disk speed is 14.74rpm, and this experiment uses a disk rotation speed of 14.74rpm as the production process; according to the equation (2) of the present invention, the maximum rotation pressure flatness is determined to be 0.1125μm; according to the equation (3) of the present invention, the maximum theoretical pressure flatness is determined to be 0.106μm; according to the empirical equation (4), the minimum value of the maximum theoretical pressure flatness and the maximum rotation pressure flatness is taken as 0.106μm, and then according to the equation (3) of the present invention, the maximum pressure in the actual process is determined to be 28.75kpa.
[0038] 75 200mm silicon wafers were polished using this process, and the average local flatness was 0.115μm, fully meeting customer requirements.
[0039] Example 5
[0040] Polishing 300mm silicon wafers, customer technical requirements for local flatness of 0.3μm, incoming material TTV average of 1.0μm, planetary wafer rotation speed of 40rpm; according to the empirical equation (1) of the present invention, the minimum disk speed is determined to be 13.32rpm, the maximum disk speed is 15.81rpm, and this experiment uses a disk rotation speed of 13.32rpm as the production process; according to the equation (2) of the present invention, the maximum rotation pressure flatness is determined to be 0.15μm; according to the equation (3) of the present invention, the maximum theoretical pressure flatness is determined to be 0.21μm; according to the empirical equation (4), the minimum value of the maximum theoretical pressure flatness and the maximum rotation pressure flatness is taken as 0.15μm, and then according to the equation (3) of the present invention, the maximum pressure in the actual process is determined to be 14.68kpa.
[0041] 150 300mm silicon wafers were polished using this process, and the average local flatness was 0.17μm, which fully met customer requirements.
[0042] Example 6
[0043] Polishing 200mm silicon wafers, customer technical requirements for local flatness of 0.3μm, incoming material TTV average of 1.12μm, planetary wafer rotation speed of 40rpm; according to the empirical equation (1) of the present invention, the minimum disk speed is determined to be 13.32rpm, the maximum disk speed is 15.81rpm, and this experiment uses a disk rotation speed of 15.81rpm as the production process; according to the equation (2) of the present invention, the maximum rotation pressure flatness is determined to be 0.225μm; according to the equation (3) of the present invention, the maximum theoretical pressure flatness is determined to be 0.21μm; according to the empirical equation (4), the minimum value of the maximum theoretical pressure flatness and the maximum rotation pressure flatness is taken as 0.21μm, and then according to the equation (3) of the present invention, the maximum pressure in the actual process is determined to be 28.27kpa.
[0044] 150 200mm silicon wafers were polished using this process, and the average local flatness was 0.23μm, which fully met customer requirements.
[0045] Example 7
[0046] Polishing 300mm silicon wafers, customer technical requirements for local flatness of 0.3μm, incoming material TTV average of 2.2μm, planetary wafer rotation speed of 30rpm; according to the empirical equation (1) of the present invention, the minimum disk speed is determined to be 15.85rpm, the maximum disk speed is 19.13rpm, and this experiment uses a disk rotation speed of 16.64rpm as the production process; according to the equation (2) of the present invention, the maximum rotation pressure flatness is determined to be 0.18μm; according to the equation (3) of the present invention, the maximum theoretical pressure flatness is determined to be 0.21μm; according to the empirical equation (4), the minimum value of the maximum theoretical pressure flatness and the maximum rotation pressure flatness is taken as 0.18μm, and then according to the equation (3) of the present invention, the maximum pressure in the actual process is determined to be 20.11kpa.
[0047] 75 300mm silicon wafers were polished using this process, and the average local flatness was 0.14μm, fully meeting customer requirements.
Claims
1. A method for controlling the local flatness of a single crystal silicon wafer for integrated circuits, according to the technical requirements for the local flatness of a single crystal silicon wafer in integrated circuit chip manufacturing and the technical specifications of the polishing material, the rotation speed of the large plate and the rotation speed of the planetary sheet in double-sided chemical mechanical polishing are determined by the rotation flatness calculation equation; The maximum value of the rotation pressure flatness is obtained, and the maximum value of the theoretical pressure flatness when the pressure flatness has an inflection point is obtained through the pressure flatness calculation equation; the minimum value between the theoretical maximum value of the pressure flatness and the maximum value of the rotation pressure flatness is taken, and the maximum value of the pressure in the actual process is determined through the pressure flatness calculation equation; it is characterized in that it comprises the following steps: The first step is to determine the local flatness TTV of the monocrystalline silicon wafer according to the customer's technical requirements for the monocrystalline silicon wafer. spec ; Step 2: Rotational flatness TTV ω According to equation (1), TTV ω =TTV wafer ·A·[arccot(ω up -oh planet +B)] n (1) In the formula, TTV ω The local flatness of the single crystal silicon wafer caused by the rotation of the disk and the planetary wafer, referred to as rotation flatness; TTV wafer is the mean value of incoming material TTV; A is the rotation contribution coefficient, and the empirical value is: A=1.282; ω up is the rotation speed of the disk; ω planet is the rotation speed of the planetary piece; B is the rotation compensation constant, and its empirical value is B=20.85; n is the rotation index, and its empirical value is: n=1.56; when When , the disk speed is determined to be the minimum disk speed, recorded as: ω up,min ; when When , the disk speed is determined to be the maximum disk speed, recorded as: ω up,max ; In equation (1), ω up The value of ω up,min and ω up,max between; The third step is to determine the actual process of the large plate rotation speed ω up,op Then, the rotation flatness TTV in the actual process is determined according to equation (1): ω,op , maximum value of rotation pressure flatness According to equation (2), Step 4: Pressure flatness TTV P According to equation (3), Wherein, K is the pressure contribution coefficient, and its empirical value is: K = 0.025; P is the polishing pressure; D is the pressure compensation constant, and its empirical value is: D = 0.13; C is the polishing pad coefficient, and its empirical value is: C = 1.94; H is the polishing pad hardness; σ is the polishing pad Poisson's ratio; n is the pressure index, and its empirical value is: n = 8.69; Step 5: Maximum value of pressure flatness TTV in actual process P,max The value of is: in, It is the maximum value of theoretical pressure flatness when the pressure flatness has an inflection point; Step 6: Calculate the maximum pressure P in the actual process according to equation (3): op,max , and according to the maximum pressure P op,max Determine the production process; 2. The method for controlling the local flatness of a single crystal silicon wafer for integrated circuits according to claim 1, characterized in that: The range of local flatness is: TTV spec =0.2~0.5μm.
3. The method for controlling the local flatness of a single crystal silicon wafer for integrated circuits according to claim 1, characterized in that: The range of the incoming material TTV mean is: TTV wafer ≤1.5μm 4. The method for controlling the local flatness of a single crystal silicon wafer for integrated circuits according to claim 1, characterized in that: The range of the planetary piece rotation speed is ω planet =20~40rpm.
Citation Information
Patent Citations
Wafer edge area flatness optimizing method suitable for chemical-mechanical planarization process
CN107052984A
Technology for improving geometric parameters of 8-inch silicon wafer
CN107855922A
Rough polishing process for reducing overall flatness of gallium arsenide double-polished sheet
CN107978522A
Chemical-mechanical planarization method for optimizing surface morphologies of wafers
CN108059921A
Technique for nanometer grade super smooth processing gallium phosphide wafer
CN1947944A