A method for preparing SmCo alloy permanent magnetic film with single target and high throughput
Through ion beam-assisted multi-target DC magnetron sputtering technology and high-throughput screening, the problems of fixed components and impurities in the preparation of SmCo alloy permanent magnet films have been solved, and efficient, high-purity film preparation has been achieved, which is suitable for studying multi-component doping. system, improving magnetic performance and experimental efficiency.
Patent Information
- Application Number
- CN202211153268.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-21
AI Technical Summary
In the existing SmCo alloy permanent magnet thin film preparation technology, the composition of the alloy target is fixed, which is prone to problems such as impurity entry and high oxygen content, resulting in low purity. Moreover, the efficiency of magnetron sputtering using alloy targets is low, making it difficult to study multiple groups. Element doping system and complex phase composition.
Using ion beam-assisted multi-target DC magnetron sputtering technology, a multi-component gradient SmCo alloy permanent magnet film is formed by cutting and combining rare earth metal Sm, transition metal Co and other transition metal targets. Magnetron sputtering and In-situ heat treatment is used to obtain films with continuous gradient changes in composition, and samples with excellent properties are obtained through high-throughput screening.
It achieves efficient preparation of SmCo alloy permanent magnet thin films, improves experimental efficiency, can quickly prepare large batches of samples with continuously changing compositions, improves the purity and magnetic properties of the material, simplifies the experimental process, and is suitable for studying multi-component doping systems.
Smart Images

Figure CN115537744B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thin film material preparation, and in particular relates to a method for preparing a SmCo alloy permanent magnetic thin film with a single-substance target at high throughput. Background Art
[0002] As an important functional material, permanent magnetic film has been widely used in important fields such as data storage, microwave communication, aviation industry, microelectronics industry, etc. Among them, SmCo-based permanent magnetic alloy has irreplaceable important applications due to its high magnetocrystalline anisotropy and high Curie temperature.
[0003] SmCo alloy permanent magnetic film has always been a research hotspot due to its high anisotropy, high coercive force and high Curie temperature. At present, SmCo alloy targets with fixed composition are generally used as targets for magnetron sputtering. Once made, the composition is fixed and cannot be adjusted. Moreover, most alloy targets are made by powder metallurgy. Impurities are easily introduced during the production process, and the oxygen content is high. The purity can only reach 99.9X%, which is much lower than the 99.999% of the single target. In addition, the use of alloy targets for magnetron sputtering is essentially based on trial and error. It is necessary to prepare SmCo alloy targets with fixed composition in advance, and then coat them for film performance screening, which greatly reduces the efficiency of the experiment. The use of single targets to prepare SmCo alloy permanent magnetic films can effectively solve the above problems, but the use of only single targets will lead to a decrease in the utilization rate of the magnetron sputtering target head, which is not conducive to the study of multi-component doped systems, the complex phase composition of the SmCo alloy system, and the multi-phase coupling mechanism. This has greatly hindered the development and industrial application of SmCo-based magnetic films.
[0004] The patent application for the method of preparing SmCo5 thin film with a single target discloses a method of preparing SmCo alloy thin film with a single target, and describes the preparation of SmCo alloy thin film by alternating multiple depositions using a single target. Current researchers improve the magnetic properties of samples by doping with different elements, such as doping with Fe elements to improve remanence, doping with Cu elements to improve coercivity, etc. However, traditional experimental preparation techniques are not conducive to the study of multi-component doped SmCo system alloy permanent magnetic films. Alternating deposition of different metals to achieve element-doped SmCo alloy films will greatly increase experimental time and reduce experimental efficiency. The use of high-throughput experiments can quickly prepare a large number of different samples with continuously changing components at one time. Combined with high-throughput characterization methods, the material cost and experimental time can be halved, greatly improving experimental efficiency.
[0005] Therefore, it is urgent to develop a simple, easy-to-control, and experimentally efficient method for preparing SmCo system rare earth permanent magnetic films. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing SmCo alloy permanent magnetic film with a single target at high throughput, specifically a method for preparing multi-component gradient-changing magnetron sputtering SmCo alloy permanent magnetic film by ion beam assisted multi-target DC magnetron sputtering.
[0007] The purpose of the present invention is achieved through the following technical solutions.
[0008] The present invention provides a high-throughput preparation method of a SmCo alloy permanent magnetic film, comprising the following steps:
[0009] (1) respectively cutting the rare earth metal Sm, the transition metal Co and other transition metals except Co into fan-shaped targets to obtain the rare earth metal Sm fan-shaped target, the transition metal Co fan-shaped target and other transition metal fan-shaped targets except Co;
[0010] (2) combining the rare earth metal Sm fan-shaped target and the transition metal Co fan-shaped target cut in step (1) into circular targets at different central angle ratios according to the component ratio required by the experiment, and obtaining a SmCo composite target. The entire Cu circular target is used as a base to prevent magnetron sputtering from passing through the gaps in the fan-shaped targets and bombarding the target head. The transition metal fan-shaped targets other than Co cut in step (1) are combined into circular targets according to the doping ratio required by the experiment, and obtaining a transition metal target other than Co. The entire Cu circular target is used as a base, and the SmCo composite target and the transition metal target other than Co are respectively fixed on the magnetron sputtering target head with adjustable angle and position by using a steel ring.
[0011] (3) Adjust the center of the SmCo composite target head and the target head of other transition metals except Co to align with the center of the sputtering substrate, and adjust the angles between the planes of the SmCo composite target head and the target head of other transition metals except Co and the plane of the substrate, and adjust the distances between the center of the planes of the SmCo composite target head and the target head of other transition metals except Co and the center of the plane of the substrate, so as to adjust the position of Sm in the SmCo composite target head to a position close to the sputtering substrate.
[0012] (4) After magnetron sputtering coating, in-situ heat treatment is performed to obtain a SmCo alloy permanent magnet film doped with other transition metals other than Co on the substrate, wherein the composition changes gradually along the circumference and the diameter of the substrate. High-throughput screening is performed in the area where the composition changes continuously in gradient, thereby obtaining a SmCo alloy permanent magnet film doped with other transition metals other than Co with better performance.
[0013] (5) The element distribution patterns and corresponding atomic ratios of each region on the SmCo alloy permanent magnetic film samples doped with transition metals other than Co were analyzed by scanning electron microscopy-energy spectrum. A concentration gradient diffusion line was established from the highest point of the Sm atomic composition ratio to the highest point of the Co atomic composition ratio. A high-throughput selection area was established along this concentration gradient diffusion line. Points were taken at equal intervals on the concentration gradient diffusion line, and samples were cut with the points as the center of the circle.
[0014] Preferably, in step (1), the other transition metals except Co are one or more of Fe, Cu, Cr, Zr and Ti, and the purity of the rare earth metal Sm, the transition metal Co and the other transition metals except Co are all greater than 99.995%.
[0015] Preferably, in step (2), the transition metal targets other than Co are FeCu composite targets, the central angle ratio of Fe and Cu in the FeCu composite target is 1:1, the central angle of Fe and the central angle of Cu account for 50% of the central angle of each FeCu composite target, and the Fe fan-shaped target material and the Cu fan-shaped target material in the combined FeCu alloy target are reassembled in a cross-splicing manner.
[0016] Preferably, in step (1), the Sm single element circular target and the Co single element circular target are cut into sectors by wire cutting, and the center angles of the rare earth metal Sm sector-shaped target and the transition metal Co sector-shaped target obtained after cutting are 30 to 60°.
[0017] Preferably, the radius of the sector-shaped target in step (1) is 30 mm, the thickness is 3-4 mm, and the central angle is 30°-60°.
[0018] Preferably, the thickness of the sector-shaped target in step (1) is 3 mm, and the central angle of the sector-shaped target is 60°.
[0019] Preferably, in step (2), the central angle of Sm in the SmCo composite target accounts for 8.3% to 25% of the central angle of the SmCo composite target.
[0020] Preferably, in step (2), the central angle ratio of Sm to Co in the SmCo composite target is 1:3, 1:5, or 1:11.
[0021] Preferably, in step (2), the thickness of the Cu circular target base is 1 mm and the radius is 30 mm.
[0022] Preferably, the base in step (3) is composed of a sample stage and a substrate, wherein the sample stage and the substrate can rotate around an axis to ensure the uniformity of the required doping elements, and the substrate is a single crystal Si (100) substrate with a diameter of 4 inches or 6 inches.
[0023] Preferably, the substrate is a single crystal Si (100) substrate with a diameter of 4 inches.
[0024] Preferably, a single crystal Si (100) substrate is ultrasonically cleaned in sequence with a hydrofluoric acid solution, acetone and anhydrous ethanol before use.
[0025] Preferably, in step (3), the concentration gradient of the sputtered element can be controlled by adjusting the rotation speed of the substrate.
[0026] Preferably, in step (3), the distance between the center of the plane of the SmCo combined target head and the center of the substrate plane is adjusted to 10 to 20 cm, the distance between the center of the plane of the target head of other transition metals except Co and the center of the substrate plane is adjusted to 10 to 20 cm, the plane of the SmCo combined target head is adjusted to 45° to 75° with the substrate plane, and the plane of the target head of other transition metals except Co is adjusted to 45° to 75° with the substrate plane.
[0027] Preferably, in step (3), the distance between the center of the SmCo composite target head plane and the center of the substrate plane is adjusted to 15 cm.
[0028] Preferably, in step (3), the planes of the SmCo composite target head and the target heads of other transition metals except Co are adjusted to be 60° with the substrate plane.
[0029] Preferably, the working gas used in magnetron sputtering in step (4) is Ar with a purity of 99.999%.
[0030] Preferably, the background vacuum of the magnetron sputtering in step (4) is ≤1×10 -4 Pa, the sputtering gas pressure of magnetron sputtering is 0.5~1.0Pa.
[0031] Preferably, the sputtering gas pressure of magnetron sputtering in step (4) is 0.5 Pa.
[0032] Preferably, when magnetron sputtering is performed in step (4), the DC sputtering power for the SmCo composite target is 30-130W.
[0033] Preferably, when magnetron sputtering is performed in step (4), the DC sputtering power for the SmCo composite target is 80W.
[0034] Preferably, when magnetron sputtering is performed in step (4), the DC sputtering power for transition metal targets other than Co is 80 W.
[0035] Preferably, the in-situ heat treatment in step (4) is performed under the protection of an Ar gas atmosphere of 0.5 Pa, at a temperature of 550° C., and for a holding time of 20 min to obtain a SmCo alloy permanent magnetic film.
[0036] Preferably, the rotation rate of the substrate during the SmCo composite target magnetron sputtering coating process is 0.
[0037] Preferably, the rotation rate of the substrate during magnetron sputtering coating of transition metal targets other than Co is 3 r / min.
[0038] Preferably, the rotation rate of the substrate during the Cr single target magnetron sputtering coating process is 3 r / min.
[0039] Preferably, Cr plating is used as a protective layer to prevent oxidation of the SmCo alloy permanent magnetic film in the subsequent process. The sputtering power is 80 W and the sputtering time is 2 min.
[0040] Preferably, in step (5), the surface composition change of the substrate is obtained by scanning electron microscopy-energy spectrum analysis, and a concentration gradient diffusion line is established from the highest point of the Sm element ratio to the highest point of the Co element ratio.
[0041] Preferably, in step (5), the radius of the SmCo alloy permanent magnetic film samples sampled equidistantly by high-throughput characterization is 8 to 10 mm.
[0042] Preferably, the composition segregation of two or more components on the substrate is controlled to obtain a corresponding composition ratio at the transition interface.
[0043] Preferably, in this experiment, high-throughput sampling is defined as analyzing the element distribution of transition metal-doped SmCo alloy permanent magnetic film by scanning electron microscopy-energy spectrum, establishing a concentration gradient diffusion line from the highest point of Sm atomic composition ratio to the lowest point of Co atomic composition, establishing a high-throughput selection area along this concentration gradient diffusion line, taking points equidistantly on the concentration gradient diffusion line, and cutting and sampling with the points as the center of the circle.
[0044] Preferably, in step (5), six points are taken at equal intervals by high-throughput sampling.
[0045] Preferably, the radius of the SmCo alloy permanent magnetic film sample sampled by high-throughput sampling in step (5) is 8 to 10 mm.
[0046] The principle of the present invention is to coat the assembled target by magnetron sputtering, and utilize the different bombardment efficiencies of ions on different elements, resulting in a gradient change in the concentration of different elements deposited on the substrate due to differences in position and distance, so that the desired sample can be screened in the area where the composition changes continuously to obtain.
[0047] The beneficial effects of the present invention are as follows: the preparation method of the present invention is simple and easy to control, the ingredients are easy to adjust, the efficiency of sample preparation is improved through a high-throughput experimental method, a large number of samples can be prepared at one time, and samples with required ingredients can be screened out at a continuous gradient diffusion point through high-throughput screening, and the doping system can be quickly analyzed. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a diagram of the metal Sm and Co target materials in Example 1 after cutting and splicing.
[0049] Figure 2 This is a diagram of the metal Sm and Co target materials in Example 2, Example 4 and Example 5 after cutting and splicing.
[0050] Figure 3 This is a diagram of the metal Sm and Co targets in Example 3 after cutting and splicing.
[0051] Figure 4 This is a diagram of the metal Fe and Cu targets in Examples 1-3 after cutting and splicing.
[0052] Figure 5 This is a diagram of the metal Fe and Cu targets in Examples 4 to 5 after cutting and splicing.
[0053] Figure 6 Schematic diagram of the distribution of SmCo combined target head, FeCu combined target head, Cr single target head and substrate.
[0054] Figure 7 Schematic diagram of the gradient change of the SmCo alloy permanent magnetic film sample in Example 1.
[0055] Figure 8 This is a demagnetization curve of the SmCo alloy permanent magnetic film prepared by alternating sputtering of a single target in Comparative Example 1.
[0056] Fig. 9 This is a comparison chart of the demagnetization curves of 6 samples along the gradient change in Example 1.
[0057] Fig.10 This is a comparison chart of the demagnetization curves of 6 samples along the gradient change in Example 2.
[0058] Fig.11 This is a comparison chart of the demagnetization curves of 6 samples along the gradient change in Example 3.
[0059] Fig.12 This is a comparison chart of the demagnetization curves of 6 samples along the gradient change in Example 4.
[0060] Fig.13 This is a comparison chart of the demagnetization curves of 6 samples along the gradient change in Example 5. DETAILED DESCRIPTION
[0061] The present invention will be further explained and illustrated below in conjunction with specific embodiments.
[0062] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0063] Comparative Example 1
[0064] In Comparative Example 1, the film was prepared by pulsed laser deposition, and the magnetic layer was prepared by alternately depositing a single Sm target and a Co target, and the background vacuum was 2×10 -4 Pa, the working pressure is maintained at 0.5Pa, the deposition temperature is 400℃, the laser frequency is 8Hz, and the energy is 190mJ / pulse First, a Cu bottom layer was deposited for 60 minutes, followed by alternating deposition of Sm / Co targets, with Sm deposition time of 6 seconds and Co deposition time of 3 minutes, repeated 10 times, and finally a Cr anti-oxidation layer was plated, with Cr deposition time of 5 minutes. The sample was annealed at 700℃ for 30 minutes, and then cooled to room temperature in the furnace to obtain a SmCo alloy permanent magnetic film.
[0065] The demagnetization curve of the SmCo alloy permanent magnet film obtained by the physical properties comprehensive test system (PPMS) is as follows: Figure 8 As shown, the coercivity H of the SmCo alloy permanent magnet film cj =11.7kOe.
[0066] Example 1
[0067] A method for preparing a gradient-varied magnetron sputtering SmCo alloy permanent magnetic film comprises the following steps:
[0068] 1) Select a 0.5 mm thick 4-inch single crystal Si (100) substrate and use a 5% mass fraction hydrofluoric acid aqueous solution, acetone and anhydrous ethanol to ultrasonically clean it for 10 minutes. After cleaning, dry it in an oven and fix it on the sample table with silver glue after there are no water drops on the surface.
[0069] 2) Use an electric spark wire cutting machine to cut the Sm single target and the Co single target into fan-shaped targets with a radius of 30 mm, a thickness of 3 mm, and a central angle of 90°, respectively, to obtain Sm fan-shaped targets and Co fan-shaped targets, respectively; use an electric spark wire cutting machine to cut the Fe single target and the Cu single target into fan-shaped targets with a radius of 30 mm, a thickness of 3 mm, and a central angle of 60°, respectively, to obtain Fe fan-shaped targets and Cu fan-shaped targets, respectively.
[0070] 3) Assemble and splice the Sm fan-shaped target and the Co fan-shaped target in a ratio of 1:3 to form a SmCo composite target (such as Figure 1As shown), a 1 mm Cu target is used as the base; the Fe sector target and the Cu sector target are alternately spliced and assembled into a FeCu composite target (as shown) with a central angle ratio of 1:1. Figure 4 As shown), a 1 mm Cu target is used as the base, and a SmCo composite target, a FeCu composite target, and a Cr single target are fixed on the target head respectively with a steel ring;
[0071] 4) Adjust the center of the SmCo target head and the FeCu target head to align with the center of the substrate, and adjust the angle between the plane of the SmCo target head and the FeCu target head and the substrate plane to 60°, adjust the distance between the plane center of the SmCo target head and the FeCu target head and the substrate plane center to 15 cm, and the distance between the plane center of the single metal Cr target head and the substrate plane center to 15 cm. The distribution of each target head is as follows: Figure 6 shown.
[0072] 5) Evacuate the system to 5×10 -5 Pa, introduce Ar, adjust the gas pressure to 0.5Pa, and perform ion beam cleaning for 5 minutes. The order and parameters of coating are: SmCo combination target: 80W, 20min, DC magnetron sputtering, non-rotating substrate; FeCu combination target: 80W, 1min, DC magnetron sputtering, rotating substrate at a speed of 3r / min; Cr target: 80W, 30s, DC magnetron sputtering, rotating substrate at a speed of 3r / min. The purpose of Cr coating is to act as a protective layer to prevent the SmCo alloy permanent magnetic film from being oxidized.
[0073] 6) Perform in-situ heat treatment, heat the substrate in-situ to 550°C, keep the temperature for 15 minutes, and then cool it to room temperature under Ar atmosphere protection while maintaining the pressure at 0.5 Pa. A FeCu-doped SmCo alloy permanent magnetic film with a continuous gradient composition can be obtained on the substrate.
[0074] 7) After the in-situ heat treatment, the SmCo alloy permanent magnetic film was divided into 6 points along the diffusion gradient line, and a circle with a radius of 10 mm was cut with each point as the center for high-throughput sampling (such as Figure 7 As shown, one end of the substrate close to the Sm sector target is rich in Sm, and the other end is rich in Co), and the SmCo alloy permanent magnetic film samples 1-1, sample 1-2, sample 1-3, sample 1-4, sample 1-5, and sample 1-6 of Example 1 are obtained.
[0075] 8) Table 1 is a table of the composition of the FeCu-doped SmCo alloy permanent magnetic film measured by scanning electron microscope-energy spectrometer in Example 1. The distribution law of the composition on the sample surface can be obtained from the table. From Table 1, it can be seen that the atomic percentage Sm / at.% of Sm in samples 1-1 to 1-6 gradually decreases from 35.41% to 11.35%, the atomic percentage Co / at.% of Co gradually increases from 59.13% to 82.86%, and the atomic percentages of Cu and Fe are approximately equal and both are close to 2.5%.
[0076] 9) The demagnetization curve of FeCu doped SmCo alloy permanent magnetic film was tested by physical properties comprehensive test system (PPMS). The magnetic properties of the sample are as follows: Fig. 9 As shown, the coercivity of sample 1-3 is the highest. cj =15.8kOe.
[0077] Table 1 Composition of FeCu doped SmCo alloy film in Example 1
[0078]
[0079] Fig. 9 The figure is a comparison of the demagnetization curves of the six samples along the gradient change in Example 1. Fig. 9 It can be seen that the coercive force of the six samples with gradient changes first increases and then decreases, and the coercive force is the highest at samples 1-3. Therefore, when the Cu doping amount of the sample is 2.22% and the Fe doping amount is 2.03%, that is, when the total amount of transition metal FeCu doping other than Co is 4.25%, the optimal SmCo phase ratio can be obtained. The energy spectrum result corresponding to this area is the optimal composition ratio in the SmCo alloy permanent magnet film system when FeCu doping is 4.25%.
[0080] Example 2
[0081] A method for preparing a gradient-varied magnetron sputtering SmCo alloy permanent magnetic film comprises the following steps:
[0082] 1) Select a 0.5 mm thick 4-inch single crystal Si (100) substrate and use a 5% mass fraction hydrofluoric acid aqueous solution, acetone and anhydrous ethanol to ultrasonically clean it for 10 minutes. After cleaning, dry it in an oven and fix it on the sample table with silver glue after there are no water drops on the surface.
[0083] 2) Use an electric spark wire cutting machine to cut the Sm single target and the Co single target into fan-shaped targets with a radius of 30 mm, a thickness of 3 mm, and a central angle of 60°, respectively, to obtain Sm fan-shaped targets and Co fan-shaped targets, respectively; wire cut the Fe single target and the Cu single target into fan-shaped targets with a radius of 30 mm, a thickness of 3 mm, and a central angle of 60°, respectively, to obtain Fe fan-shaped targets and Cu fan-shaped targets.
[0084] 3) Assemble and splice the Sm fan-shaped target and the Co fan-shaped target with a central angle ratio of 1:5 to form a SmCo combined target (such as Figure 2 As shown), a 1 mm Cu target is used as the base; the Fe sector target and the Cu sector target are alternately spliced and assembled into a FeCu composite target (as shown) with a central angle ratio of 1:1. Figure 4 As shown), a 1 mm Cu target was used as the base, and the SmCo composite target, FeCu composite target, and Cr single target were fixed on the target head with steel rings.
[0085] 4) Adjust the center of the SmCo combination target head and the FeCu combination target head to align with the center of the substrate sample stage, and adjust the angle between the plane of the SmCo combination target head and the FeCu combination target head and the substrate plane to 60°, respectively, adjust the distance between the plane center of the SmCo combination target head and the FeCu combination target head and the substrate plane center to 15 cm, and the distance between the plane center of the elemental metal Cr target head and the substrate plane center to 15 cm.
[0086] 5) Evacuate the system to 5×10 -5 Pa, introduce Ar, adjust the gas pressure to 1.0Pa, and perform ion beam cleaning for 5 minutes. The order and parameters of coating are: SmCo combination target: 80W, 20min, DC magnetron sputtering, non-rotating substrate; FeCu combination target: 80W, 2min, DC magnetron sputtering, rotating substrate at a speed of 3r / min; Cr target: 80W, 30s, DC magnetron sputtering, rotating substrate at a speed of 3r / min. The purpose of Cr coating is to act as a protective layer to prevent the SmCo alloy permanent magnetic film from being oxidized.
[0087] 6) Perform in-situ heat treatment, heat the substrate in-situ to 550°C, keep the temperature for 15 minutes, and then cool it to room temperature under Ar atmosphere protection while maintaining the pressure at 0.5 Pa. A FeCu-doped SmCo alloy permanent magnetic film with a continuous gradient composition can be obtained on the substrate.
[0088] 7) The SmCo alloy permanent magnetic film after in-situ heat treatment was divided into 6 equal points along the diffusion gradient line, and a circle with a radius of 10 mm was cut with each point as the center for high-throughput sampling to obtain SmCo alloy permanent magnetic film samples 2-1, sample 2-2, sample 2-3, sample 2-4, sample 2-5, and sample 2-6 of Example 2.
[0089] 8) Table 2 is a table of the composition of the FeCu-doped SmCo alloy permanent magnetic film measured by scanning electron microscope-energy spectrometer in Example 2. The distribution of the composition on the sample surface can be obtained from the table. From Table 2, it can be seen that the atomic percentage Sm / at.% of Sm in sample 2-1 to sample 2-6 gradually decreases from 21.19% to 9.36%, the atomic percentage Co / at.% of Co gradually increases from 67.81% to 78.62%, and the atomic percentages of Cu and Fe are approximately equal and both close to 5%.
[0090] 9) The demagnetization curve of FeCu doped SmCo alloy permanent magnetic film was tested by physical properties comprehensive test system (PPMS). The magnetic properties of the sample are as follows: Fig.10 As shown, the coercivity of sample 2-2 is the highest. cj =25.5kOe.
[0091] Table 2 Composition of FeCu doped SmCo alloy film in Example 2
[0092]
[0093] Fig.10 The figure is a comparison of the demagnetization curves of the six samples along the gradient change in Example 2. Fig.10 It can be seen that the coercive force of the six samples with gradient changes first increases and then decreases, and the coercive force is the highest at sample 2-2. Therefore, when the Cu doping amount of the sample is 5.03% and the Fe doping amount is 4.92%, that is, when the total amount of transition metal FeCu doping other than Co is 9.95%, the optimal SmCo phase ratio can be obtained. The energy spectrum result corresponding to this area is the optimal composition ratio in the SmCo alloy permanent magnet film system when FeCu doping is 9.95%.
[0094] Example 3
[0095] A method for preparing a gradient-varied magnetron sputtering SmCo alloy permanent magnetic film comprises the following steps:
[0096] 1) Select a 0.5 mm thick 4-inch single crystal Si (100) substrate and use a 5% mass fraction hydrofluoric acid aqueous solution, acetone and anhydrous ethanol to ultrasonically clean it for 10 minutes. After cleaning, dry it in an oven and fix it on the sample table with silver glue after there are no water drops on the surface.
[0097] 2) Use an electric spark wire cutting machine to cut the Sm single target and the Co single target into fan-shaped targets with a radius of 30 mm, a thickness of 3 mm, and a central angle of 30°, respectively, to obtain Sm fan-shaped targets and Co fan-shaped targets, respectively; wire cut the Fe single target and the Cu single target into fan-shaped targets with a radius of 30 mm, a thickness of 3 mm, and a central angle of 60°, respectively, to obtain Fe fan-shaped targets and Cu fan-shaped targets.
[0098] 3) Assemble and splice the Sm fan-shaped target and the Co fan-shaped target with a central angle ratio of 1:11 to form a SmCo combined target (such as Figure 3 As shown), a 1 mm Cu target is used as the base; the Fe sector target and the Cu sector target are alternately spliced and assembled into a FeCu composite target (as shown) with a central angle ratio of 1:1. Figure 4 As shown), a 1 mm Cu target was used as the base, and the SmCo composite target, FeCu composite target, and Cr single target were fixed on the target head with steel rings.
[0099] 4) Adjust the center of the SmCo combination target head and the FeCu combination target head to align with the center of the substrate sample stage, and adjust the angle between the plane of the SmCo combination target head and the FeCu combination target head and the substrate plane to 60°, respectively. Adjust the distance between the center of the plane of the SmCo combination target head and the FeCu combination target head and the center of the substrate plane to 15 cm, and the distance between the center of the plane of the single metal Cr target head and the center of the substrate plane to 15 cm.
[0100] 5) Evacuate the system to 5×10 -5 Pa, introduce Ar, adjust the gas pressure to 0.5Pa, and perform ion beam cleaning for 5 minutes. The order and parameters of coating are: SmCo combination target: 80W, 20min, DC magnetron sputtering, non-rotating substrate; FeCu combination target: 80W, 3min, DC magnetron sputtering, rotating substrate at a speed of 3r / min; Cr target: 80W, 30s, DC magnetron sputtering, rotating substrate at a speed of 3r / min. The purpose of Cr coating is to act as a protective layer to prevent the SmCo alloy permanent magnetic film from being oxidized.
[0101] 6) Perform in-situ heat treatment, heat the substrate to 550°C, keep the temperature for 15 minutes, and then cool to room temperature under Ar atmosphere protection while maintaining the pressure at 0.5 Pa. A FeCu-doped SmCo alloy permanent magnetic film with a continuous gradient composition can be obtained on the substrate.
[0102] 7) The SmCo alloy permanent magnetic film after in-situ heat treatment was divided into 6 equal points along the diffusion gradient line, and a circle with a radius of 10 mm was cut with each point as the center for high-throughput sampling to obtain SmCo alloy permanent magnetic film samples 3-1, sample 3-2, sample 3-3, sample 3-4, sample 3-5, and sample 3-6 of Example 3.
[0103] 8) Table 3 is a table of the composition of the FeCu-doped SmCo alloy permanent magnetic film measured by scanning electron microscope-energy spectrometer in Example 3. The distribution law of the composition on the sample surface can be obtained through the table. From Table 3, it can be seen that the atomic percentage Sm / at.% of Sm in samples 3-1 to 3-6 gradually decreases from 16.48% to 7.14%, the atomic percentage Co / at.% of Co gradually increases from 67.40% to 76.40%, and the atomic percentages of Cu and Fe are approximately equal and both close to 7.5%.
[0104] 9) The demagnetization curve of FeCu doped SmCo alloy permanent magnetic film was tested by physical properties comprehensive test system (PPMS). The magnetic properties of the sample are as follows: Fig.11 As shown, the coercivity of sample 3-1 is the highest. cj =12.9kOe.
[0105] Table 3 Composition of FeCu doped SmCo alloy film in Example 3
[0106]
[0107] Fig.11 The demagnetization curves of the six samples along the gradient change in Example 3 are compared. Fig.11 It can be seen that the coercive force of the six samples with gradient changes gradually decreases, and the coercive force is the highest at sample 3-1. Therefore, when the Cu doping amount of the sample is 8.12% and the Fe doping amount is 8.00%, that is, when the total amount of transition metal FeCu doping other than Co is 16.12%, the optimal SmCo phase ratio can be obtained. The energy spectrum result corresponding to this area is the optimal composition ratio in the SmCo alloy permanent magnet film system when FeCu doping is 15.21%.
[0108] Example 4
[0109] A method for preparing a gradient-varied magnetron sputtering SmCo alloy permanent magnetic film comprises the following steps:
[0110] 1) Select a 6-inch single crystal Si (100) substrate with a thickness of 0.5 mm and use a 5% hydrofluoric acid aqueous solution, acetone and anhydrous ethanol to ultrasonically clean it for 10 minutes in sequence. After cleaning, dry it in an oven and fix it on the sample table with silver glue after there are no water drops on the surface.
[0111] 2) Use an electric spark wire cutting machine to cut the Sm single target and the Co single target into fan-shaped targets with a radius of 30 mm, a thickness of 4 mm, and a central angle of 60°, respectively, to obtain Sm fan-shaped targets and Co fan-shaped targets, respectively; wire cut the Fe single target and the Cu single target into fan-shaped targets with a radius of 30 mm, a thickness of 4 mm, and a central angle of 30°, respectively, to obtain Fe fan-shaped targets and Cu fan-shaped targets.
[0112] 3) Assemble and splice the Sm fan-shaped target and the Co fan-shaped target with a central angle ratio of 1:5 to form a SmCo combined target (such as Figure 2 As shown), a 1 mm Cu target is used as the base; the Fe sector target and the Cu sector target are alternately spliced and assembled into a FeCu composite target (as shown) with a central angle ratio of 1:1. Figure 5 As shown), a 1 mm Cu target was used as the base, and the SmCo composite target, FeCu composite target, and Cr single target were fixed on the target head with steel rings.
[0113] 4) Adjust the center of the SmCo combination target head and the FeCu combination target head to align with the center of the substrate sample stage, and adjust the angle between the plane of the SmCo combination target head and the FeCu combination target head and the substrate plane to 75°, respectively, adjust the distance between the plane center of the SmCo combination target head and the FeCu combination target head and the substrate plane center to 10 cm, and the distance between the plane center of the elemental metal Cr target head and the substrate plane center to 10 cm.
[0114] 5) Evacuate the system to 5×10 -5 Pa, introduce Ar, adjust the gas pressure to 0.5Pa, and perform ion beam cleaning for 5 minutes. The order and parameters of coating are: SmCo combination target: 30W, 20min, DC magnetron sputtering, non-rotating substrate; FeCu combination target: 30W, 1min, DC magnetron sputtering, rotating substrate at a speed of 3r / min; Cr target: 80W, 30s, DC magnetron sputtering, rotating substrate at a speed of 3r / min. The purpose of Cr coating is to act as a protective layer to prevent the SmCo alloy permanent magnet film from being oxidized.
[0115] 6) Perform in-situ heat treatment, heat the substrate to 550°C, keep the temperature for 15 minutes, and then cool to room temperature under Ar atmosphere protection while maintaining the pressure at 0.5 Pa. A FeCu-doped SmCo alloy permanent magnetic film with a continuous gradient composition can be obtained on the substrate.
[0116] 7) The SmCo alloy permanent magnetic film after in-situ heat treatment was divided into 6 equal points along the diffusion gradient line, and a circle with a radius of 8 mm was cut with each point as the center for high-throughput sampling to obtain SmCo alloy permanent magnetic film samples 4-1, sample 4-2, sample 4-3, sample 4-4, sample 4-5, and sample 4-6 of Example 4.
[0117] 8) Table 4 is a table of the composition of the FeCu-doped SmCo alloy permanent magnetic film measured by scanning electron microscope-energy spectrometer in Example 4. The distribution of the composition on the sample surface can be obtained from the table. From Table 4, it can be seen that the atomic percentage Sm / at.% of Sm in sample 4-1 to sample 4-6 gradually decreases from 18.14% to 10.44%, the atomic percentage Co / at.% of Co gradually increases from 70.75% to 78.30%, and the atomic percentages of Cu and Fe are approximately equal and both close to 5%.
[0118] 9) The demagnetization curve of FeCu doped SmCo alloy permanent magnetic film was tested by physical properties comprehensive test system (PPMS). The magnetic properties of the sample are as follows: Fig.12 As shown, the coercivity of sample 4-2 is the highest. cj =25.7kOe.
[0119] Table 4 Composition of FeCu doped SmCo alloy film in Example 4
[0120]
[0121] Fig.12 The figure is a comparison of the demagnetization curves of the six samples along the gradient change in Example 4. Fig.12 It can be seen that the coercive force of the six samples with gradient changes first increases and then decreases, and the coercive force is the highest at sample 4-2. Therefore, when the Cu doping amount of the sample is 4.98% and the Fe doping amount is 5.04%, that is, when the total amount of transition metal FeCu doping other than Co is 10.02%, the optimal SmCo phase ratio can be obtained. The energy spectrum result corresponding to this area is the optimal composition ratio in the SmCo alloy permanent magnet film system when FeCu doping is 10.02%.
[0122] Example 5
[0123] A method for preparing a gradient-variable magnetron sputtering SmCo alloy permanent magnetic film comprises the following steps:
[0124] 1) Select a 0.5 mm thick 4-inch single crystal Si (100) substrate and use a 5% mass fraction hydrofluoric acid aqueous solution, acetone and anhydrous ethanol to ultrasonically clean it for 10 minutes. After cleaning, dry it in an oven and fix it on the sample table with silver glue after there are no water drops on the surface.
[0125] 2) Use an electric spark wire cutting machine to cut the Sm single target and the Co single target into fan-shaped targets with a radius of 30 mm, a thickness of 4 mm, and a central angle of 60°, respectively, to obtain Sm fan-shaped targets and Co fan-shaped targets, respectively; wire cut the Fe single target and the Cu single target into fan-shaped targets with a radius of 30 mm, a thickness of 4 mm, and a central angle of 30°, respectively, to obtain Fe fan-shaped targets and Cu fan-shaped targets.
[0126] 3) Assemble and splice the Sm fan-shaped target and the Co fan-shaped target with a central angle ratio of 1:5 to form a SmCo combined target (such as Figure 2 As shown), a 1 mm Cu target is used as the base; the Fe sector target and the Cu sector target are alternately spliced and assembled into a FeCu composite target (as shown) with a central angle ratio of 1:1. Figure 5 As shown), a 1 mm Cu target was used as the base, and the SmCo composite target, FeCu composite target, and Cr single target were fixed on the target head with steel rings.
[0127] 4) Adjust the center of the SmCo combination target head and the FeCu combination target head to align with the center of the substrate sample stage, and adjust the angle between the plane of the SmCo combination target head and the FeCu combination target head and the substrate plane to 45°, respectively, adjust the distance between the plane center of the SmCo combination target head and the FeCu combination target head and the substrate plane center to 20 cm, and the distance between the plane center of the elemental metal Cr target head and the substrate plane center to 20 cm.
[0128] 5) Evacuate the system to 5×10 -5 Pa, introduce Ar, adjust the gas pressure to 0.5Pa, and perform ion beam cleaning for 5 minutes. The order and parameters of coating are: SmCo combination target: 130W, 20min, DC magnetron sputtering, non-rotating substrate; FeCu combination target: 130W, 2min, DC magnetron sputtering, rotating substrate at a speed of 3r / min; Cr target: 80W, 30s, DC magnetron sputtering, rotating substrate at a speed of 3r / min. The purpose of Cr coating is to act as a protective layer to prevent the SmCo alloy permanent magnetic film from being oxidized.
[0129] 6) Perform in-situ heat treatment, heat the substrate in-situ to 550°C, keep the temperature for 15 minutes, and then cool it to room temperature under Ar atmosphere protection while maintaining the pressure at 0.5 Pa. A FeCu-doped SmCo alloy permanent magnetic film with a continuous gradient composition can be obtained on the substrate.
[0130] 7) The SmCo alloy permanent magnetic film after in-situ heat treatment was divided into 6 equal points along the diffusion gradient line, and a circle with a radius of 9 mm was cut with each point as the center for high-throughput sampling to obtain SmCo alloy permanent magnetic film samples 5-1, sample 5-2, sample 5-3, sample 5-4, sample 5-5, and sample 5-6 of Example 5.
[0131] 8) Table 5 is a table of the composition of the FeCu-doped SmCo alloy permanent magnetic film measured by scanning electron microscope-energy spectrometer in Example 5. The distribution of the composition on the sample surface can be obtained from the table. From Table 5, it can be seen that the atomic percentage of Sm Sm / at.% gradually decreases from 26.71% to 10.63% from sample 5-1 to sample 5-6, the atomic percentage of Co Co / at.% gradually increases from 66.78% to 82.91%, and the atomic percentages of Cu and Fe are approximately equal and both close to 2.5%.
[0132] 9) The demagnetization curve of FeCu doped SmCo alloy permanent magnetic film was tested by physical properties comprehensive test system (PPMS). The magnetic properties of the sample are as follows: Fig.13 As shown, the coercivity of sample 5-2 is the highest. cj =25.5kOe.
[0133] Table 5 Composition of FeCu doped SmCo alloy film in Example 5
[0134]
[0135] Fig.13 The figure is a comparison of the demagnetization curves of the six samples along the gradient change in Example 5. Fig.13 It can be seen that the coercive force of the six samples with gradient changes first increases and then decreases, and the coercive force is the highest at sample 5-2. Therefore, when the Cu doping amount of the sample is 2.93% and the Fe doping amount is 2.98%, that is, when the total amount of transition metal FeCu doping other than Co is 5.91%, the optimal SmCo phase ratio can be obtained. The energy spectrum result corresponding to this area is the optimal composition ratio in the SmCo alloy permanent magnet film system when FeCu doping is 5.91%.
[0136] The results show that the high-throughput experiment can be used to prepare and screen the gradient FeCu-doped SmCo alloy permanent magnetic films. By comparing Examples 1 to 5, it can be found that the coercivity and squareness of sample 4-2 in Example 4 are the best, indicating that the formation of a favorable magnetic phase is achieved when the total FeCu doping amount is 10%.
[0137] The existing technology for preparing SmCo alloy permanent magnetic thin films with single-substance targets is to prepare multilayer films by alternately depositing Sm / Co targets. This method of alternating deposition not only reduces the experimental efficiency, but also easily causes insufficient diffusion of SmCo atoms, resulting in poor performance of the formed film. The high-throughput preparation method can not only improve the experimental efficiency, but also solve the problems of low proportion of magnetic phase components and many impurity phases after doping elements. Through high-throughput experiments, hard magnetic phases with specific components can be obtained to improve the magnetic properties of SmCo alloy permanent magnetic films. In addition, by further changing the cutting and combination methods of single-substance targets, the influence of multiple elements on the SmCo system can be further studied, providing a research method for further studying the SmCo doping system.
[0138] The above embodiments are preferred implementation modes of the present invention, but the experimental methods of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing SmCo alloy permanent magnetic film with single target high throughput, characterized in that: In terms of atomic percentage, the composition of the SmCo alloy permanent magnetic film is 16.42% Sm, 73.56% Co, 4.98% Cu, 5.04% Fe, or 16.8% Sm, 73.25% Co, 5.03% Cu, 4.92% Fe; The preparation method comprises the following steps: (1) respectively cutting a rare earth metal Sm, a transition metal Co, and other transition metals other than Co into fan-shaped targets to obtain a rare earth metal Sm fan-shaped target, a transition metal Co fan-shaped target, and other transition metal fan-shaped targets other than Co, wherein the other transition metals other than Co are Cu and Fe; (2) reassembling and splicing the rare earth metal Sm fan-shaped target material and the transition metal Co fan-shaped target material cut in step (1) into a circular target material to obtain a SmCo composite target; reassembling and splicing the transition metal fan-shaped target materials other than Co cut in step (1) into a circular target material to obtain a transition metal target other than Co; and fixing the SmCo composite target and the transition metal target other than Co on a magnetron sputtering target head with adjustable angle and position; the center angle of Sm in the spliced SmCo composite target accounts for 8.3% to 25% of the center angle of the SmCo composite target; (3) adjusting the SmCo composite target head and the target heads of other transition metals except Co to align with the center of the sputtering substrate, adjusting the angles between the planes of the SmCo composite target head and the target heads of other transition metals except Co and the plane of the substrate, and adjusting the distances between the centers of the planes of the SmCo composite target head and the target heads of other transition metals except Co and the center of the plane of the substrate; (4) performing magnetron sputtering and in-situ heat treatment to obtain SmCo alloy permanent magnetic films doped with transition metals other than Co; (5) The element distribution and atomic ratio of SmCo alloy permanent magnetic films doped with transition metals other than Co were analyzed by scanning electron microscopy-energy spectrum. A concentration gradient diffusion line was established from the highest point of Sm atomic composition ratio to the highest point of Co atomic composition ratio. A high-throughput selection area was established along the concentration gradient diffusion line. Points were taken at equal intervals on the concentration gradient diffusion line, and cutting and sampling were performed with the points as the center of the circle.
2. A method for preparing SmCo alloy permanent magnetic thin film with a single target in high throughput according to claim 1, characterized in that: In step (1), the Sm single substance circular target and the Co single substance circular target are cut into sectors by wire cutting, and the center angles of the rare earth metal Sm sector-shaped target and the transition metal Co sector-shaped target obtained after cutting are 30 to 60 degrees.
3. A method for preparing SmCo alloy permanent magnetic thin film with a single target in high throughput according to claim 1, characterized in that: The radius of the sector-shaped target in step (1) is 30 mm and the thickness is 3 to 4 mm.
4. A method for preparing SmCo alloy permanent magnetic thin film with a single target in high throughput according to claim 1, characterized in that: The base in step (3) is composed of a sample stage and a substrate, wherein the sample stage and the substrate can rotate around an axis, and the substrate is a single crystal Si (100) substrate with a diameter of 4 inches or 6 inches.
5. The method for preparing SmCo alloy permanent magnetic film with a single target in high throughput according to claim 1, characterized in that: In step (3), the distance between the center of the plane of the SmCo combined target head and the center of the substrate plane is adjusted to 10 to 20 cm, the distance between the center of the plane of the target head of other transition metals except Co and the center of the substrate plane is adjusted to 10 to 20 cm, the plane of the SmCo combined target head is adjusted to 45° to 75° with the substrate plane, and the plane of the target head of other transition metals except Co is adjusted to 45° to 75° with the substrate plane.
6. A method for preparing SmCo alloy permanent magnetic thin film with a single target in high throughput according to claim 1, characterized in that: The background vacuum of the magnetron sputtering in step (4) is ≤1×10 -4 Pa, the sputtering gas pressure of magnetron sputtering is 0.5~1.0Pa.
7. A method for preparing SmCo alloy permanent magnetic thin film with a single target in high throughput according to claim 1, characterized in that: When magnetron sputtering is performed in step (4), the DC sputtering power for the SmCo composite target is 30-130W.
8. A method for preparing SmCo alloy permanent magnetic thin film with a single target in high throughput according to any one of claims 1 to 7, characterized in that: The radius of the SmCo alloy permanent magnetic film sample sampled by high-throughput equidistant sampling in step (5) is 8 to 10 mm.
Citation Information
Patent Citations
SmCo5-based permanent magnet thin strip magnet and preparation method thereof
CN106710764A