A cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature and a preparation method thereof
By combining carbon nitride-doped cobalt with a carrier, a cobalt-nitrogen-carbon non-noble metal catalyst is prepared, which solves the problem of low formaldehyde removal rate at room temperature and achieves high-efficiency, low-cost and long-life catalytic effects.
Patent Information
- Application Number
- CN202211421527.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-14
AI Technical Summary
The existing technology has a low formaldehyde removal rate at room temperature, and the noble metal catalyst has high cost and poor stability, making it difficult to achieve low-cost and efficient catalytic oxidation effects.
A cobalt-nitrogen-carbon non-precious metal catalyst composed of carbon nitride doped with cobalt element and a carrier (such as activated carbon or carbon black) is used to prepare a catalyst with a high specific surface area through a combined preparation method of cobalt acetate, nitrogen-containing ligands and carbon carriers. , and calcined and pyrolyzed in a nitrogen atmosphere to obtain the catalyst.
The catalytic efficiency of formaldehyde removal at room temperature reaches 95%, with low cost and a service life of up to 1,000 hours, overcoming the harsh conditions of traditional transition metal oxides.
Smart Images

Figure CN115591569B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst, specifically, to a cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature. The present invention also relates to a preparation method of the cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature, belonging to the technical field of non-precious metal catalyst preparation methods. Background Art
[0002] Indoor formaldehyde mainly comes from artificial boards and other decoration materials. Long-term exposure to formaldehyde above a safe concentration of 0.08 mg / m3 may cause malformation and cancer. At present, catalytic oxidation is one of the more feasible methods to remove indoor formaldehyde pollutants. This method uses room temperature catalytic oxidation to oxidize formaldehyde into CO2 and H2O to achieve the purpose of removing formaldehyde pollutants.
[0003] However, the difficulty in the practical application of catalytic oxidation technology is mainly to prepare catalysts with low temperature, high efficiency, low cost and good stability. At room temperature, the catalysts for efficient catalytic oxidation of formaldehyde are mainly precious metal-loaded catalysts. Common carriers include TiO2, SiO2, metal oxides, etc. However, the precious metals used in these catalysts result in high raw material costs and poor stability, which is not conducive to practical applications. Although transition metal oxides, which are abundant in resources and relatively cheap, show good stability, their formaldehyde removal rates at room temperature are generally low, and there is still a gap from practical applications. How to obtain efficient, stable and low-cost formaldehyde removal catalysts at room temperature is a hot spot and challenge in current technological development. Summary of the invention
[0004] In view of the above-mentioned shortcomings, the purpose of the present invention is to provide a non-precious metal catalyst for removing formaldehyde at room temperature, which solves the problem that the formaldehyde removal rate of existing transition metal oxides is low under room temperature conditions.
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature.
[0006] To this end, the first technical solution of the present invention is as follows:
[0007] A cobalt-nitrogen-carbon non-noble metal catalyst for removing formaldehyde at room temperature is composed of a carbon nitride-doped cobalt single substance and a carrier.
[0008] Furthermore, in the above-mentioned cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature, the mass ratio of the carbon nitride-doped cobalt single substance to the carrier is 1:7-10.
[0009] Furthermore, in the above-mentioned cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature, the nitrogen-containing ligands are o-phenylenediamine and 1,10-phenanthroline.
[0010] Furthermore, in the above-mentioned cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature, the carrier is activated carbon or carbon black.
[0011] The second technical solution provided by the present invention is as follows:
[0012] A method for preparing a cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature comprises the following steps in sequence:
[0013] 1) Preparation of catalyst precursor
[0014] Cobalt acetate, nitrogen-containing ligand and carbon carrier are weighed in a mass ratio of 1:2-4:2.5-3.5, and the weighed cobalt acetate and nitrogen-containing ligand are added to anhydrous ethanol in sequence, and stirred in a constant temperature magnetic stirring instrument for 0.2-1h until fully dissolved to obtain a raw material solution; then the weighed carbon carrier is introduced into the solution, heated and fully stirred for 0.05-0.15h, and vacuum evaporated to dryness for 0.5-1.5h to obtain a catalyst precursor;
[0015] 2) Calcination
[0016] The catalyst precursor prepared in step 1) is calcined and pyrolyzed in a nitrogen atmosphere to obtain a cobalt-nitrogen-carbon non-precious metal catalyst.
[0017] Furthermore, in the above-mentioned method for preparing a cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature, the vacuum evaporation operation steps described in step 1) are specifically as follows: placing the conical beaker containing the solution in a constant temperature water bath, maintaining the water temperature at 50°C, connecting a vacuum circulation pump with a T-type three-way connector, evaporating anhydrous ethanol under stirring, and then vacuum drying to obtain a solid powder; pouring the remaining solid material into an agate mortar and grinding it thoroughly to obtain a catalyst precursor.
[0018] Furthermore, in the above-mentioned method for preparing a cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature, the calcination and pyrolysis conditions in step 2) are under nitrogen protection, the tubular furnace heating rate is 5° / min, the calcination temperature is 300-900°C, the calcination time is 1h, and the nitrogen flow rate is 20mL / min.
[0019] Compared with the prior art, the technical solution provided by the present invention has the following technical advantages:
[0020] 1. The cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature provided by the present invention uses cobalt acetate, nitrogen-containing ligands and carbon carriers as raw materials to prepare the catalyst, which has the following advantages: cobalt acetate is a transition metal salt, which is low in cost and easy to obtain; the preparation process is simple, the preparation process of CoNC precursor has few steps, short time consumption and easy operation; the preparation conditions are mild and the preparation process is easy to control;
[0021] 2. The cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature provided by the present invention changes its surface properties, forms more accumulation pores and crack pores on the surface, promotes the increase of specific surface area, and strengthens the catalyst's ability to adsorb formaldehyde in the air; but does not affect the internal inherent structure of the catalyst;
[0022] 3. The cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature provided by the present invention has good catalytic purification ability, overcoming the harsh conditions required for the traditional transition metal oxides to catalytically oxidize formaldehyde, such as very high catalytic temperature. The non-precious metal catalyst of the present invention has the characteristics of simple preparation, economy and environmental protection, catalytic efficiency of up to 95% at room temperature, and service life of up to 1000 hours. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is the XRD pattern of the cobalt-nitrogen-carbon non-noble metal catalyst provided in Examples 2 to 5;
[0024] Figure 2 is the FTIR graph of the cobalt-nitrogen-carbon non-noble metal catalyst provided in Examples 2 to 5;
[0025] Figure 3 is the nitrogen adsorption-desorption isotherm of the cobalt-nitrogen-carbon non-precious metal catalyst provided in Examples 2 to 5;
[0026] Figure 4 It is the pore size distribution diagram of the cobalt-nitrogen-carbon non-precious metal catalyst provided in Examples 2 to 5. DETAILED DESCRIPTION
[0027] The following is a further description of the cobalt nitrogen carbon / carbon carrier catalyst for removing formaldehyde at room temperature and its preparation method according to the present invention in combination with some specific embodiments. The specific examples are for further illustrating the present invention in detail, but do not limit the scope of protection of the present invention. Unless otherwise specified, the methods and raw materials used in the embodiments of the present invention are conventionally selected in the art.
[0028] Example 1
[0029] 1) Weigh 2.30g of cobalt acetate, 4.60g of phenanthroline and 6.90g of carbon black, add the weighed cobalt acetate and phenanthroline to 100ml of anhydrous ethanol in turn, place in a constant temperature magnetic stirring instrument and stir for 0.5h until fully dissolved to obtain a raw material solution; then introduce the weighed carbon black into the solution, heat and stir fully for 0.12h, move the solution into a conical beaker and put it into a constant temperature water bath, keep the water temperature at 50°C, connect a vacuum circulation pump with a T-type three-way connector, evaporate the anhydrous ethanol for 0.5h under stirring, and then dry under -0.1MPa, 60°C vacuum conditions for 12h to obtain a solid powder; pour the remaining solid matter into an agate mortar and grind it fully to obtain a catalyst precursor;
[0030] 2) The catalyst precursor prepared in step 1) was calcined and pyrolyzed in a nitrogen atmosphere with a flow rate of 20 mL / min, a heating rate of 5° / min, a temperature of 700°C, and calcined for 1 h to obtain a cobalt-nitrogen-carbon non-precious metal catalyst.
[0031] Example 2
[0032] 1) Weigh 1.84 g of cobalt acetate, 5.52 g of o-phenylenediamine and 6.44 g of activated carbon, add the weighed cobalt acetate and the nitrogen-containing ligand to 100 ml of anhydrous ethanol in sequence, place in a constant temperature magnetic stirring instrument and stir for 1 hour until fully dissolved to obtain a raw material solution; then introduce the weighed activated carbon into the solution, heat and stir for 0.15 hours, transfer the solution to a conical beaker and place it in a constant temperature water bath, maintain the water temperature at 50°C, connect a vacuum circulation pump with a T-type three-way connector, evaporate the anhydrous ethanol for 1.2 hours under stirring, and then dry under -0.1 MPa, 60°C vacuum conditions for 12 hours to obtain a solid powder; pour the remaining solid matter into an agate mortar and grind it thoroughly to obtain a catalyst precursor;
[0033] 2) The catalyst precursor prepared in step 1) was calcined and pyrolyzed in a nitrogen atmosphere with a flow rate of 20 mL / min, a heating rate of 5° / min, a temperature of 500°C, and calcined for 1 h to obtain a cobalt-nitrogen-carbon non-precious metal catalyst.
[0034] Example 3
[0035] 1) Weigh 1.84 g of cobalt acetate, 7.36 g of o-phenylenediamine and 4.60 g of activated carbon, add the weighed cobalt acetate and the nitrogen-containing ligand to 100 ml of anhydrous ethanol in sequence, place in a constant temperature magnetic stirring instrument and stir for 0.2 h until fully dissolved to obtain a raw material solution; then introduce the weighed activated carbon into the solution, heat and stir for 0.05 h, transfer the solution to a conical beaker and place in a constant temperature water bath, maintain the water temperature at 50° C., connect a vacuum circulation pump with a T-type three-way connector, evaporate the anhydrous ethanol for 1.5 h under stirring, and then dry under -0.1 MPa, 60° C. vacuum conditions for 12 h to obtain a solid powder; pour the remaining solid matter into an agate mortar and grind it thoroughly to obtain a catalyst precursor;
[0036] 2) The catalyst precursor prepared in step 1) was calcined and pyrolyzed in a nitrogen atmosphere with a flow rate of 20 mL / min, a heating rate of 5° / min, a temperature of 300°C, and calcined for 1 h to obtain a cobalt-nitrogen-carbon non-precious metal catalyst.
[0037] Example 4
[0038] 1) Weigh 2.51 g of cobalt acetate, 5.02 g of o-phenylenediamine and 6.27 g of activated carbon, add the weighed cobalt acetate and the nitrogen-containing ligand to 100 ml of anhydrous ethanol in sequence, place in a constant temperature magnetic stirring instrument and stir for 0.6 h until fully dissolved to obtain a raw material solution; then introduce the weighed activated carbon into the solution, heat and stir for 0.1 h, transfer the solution to a conical beaker and place in a constant temperature water bath, maintain the water temperature at 50°C, connect a vacuum circulation pump with a T-type three-way connector, evaporate the anhydrous ethanol for 0.8 h under stirring, and then dry under -0.1 MPa, 60°C vacuum conditions for 12 h to obtain a solid powder; pour the remaining solid matter into an agate mortar and grind it thoroughly to obtain a catalyst precursor;
[0039] 2) The catalyst precursor prepared in step 1) was calcined and pyrolyzed in a nitrogen atmosphere with a flow rate of 20 mL / min, a heating rate of 5° / min, a temperature of 700°C, and calcined for 1 h to obtain a cobalt-nitrogen-carbon non-precious metal catalyst.
[0040] Example 5 Preparation of Cobalt Nitrogen Carbon Non-Noble Metal Catalyst
[0041] 1) Weigh 2.30 g of cobalt acetate, 5.75 g of o-phenylenediamine and 5.75 g of activated carbon, add the weighed cobalt acetate and the nitrogen-containing ligand to 100 ml of anhydrous ethanol in sequence, place in a constant temperature magnetic stirring instrument and stir for 0.8 h until fully dissolved to obtain a raw material solution; then introduce the weighed activated carbon into the solution, heat and stir for 0.1 h, transfer the solution to a conical beaker and place it in a constant temperature water bath, maintain the water temperature at 50°C, connect a vacuum circulation pump with a T-type three-way connector, evaporate the anhydrous ethanol for 1.2 h under stirring, and then dry under -0.1 MPa, 60°C vacuum conditions for 12 h to obtain a solid powder; pour the remaining solid matter into an agate mortar and grind it thoroughly to obtain a catalyst precursor;
[0042] 2) The catalyst precursor prepared in step 1) was calcined and pyrolyzed in a nitrogen atmosphere with a flow rate of 20 mL / min, a heating rate of 5° / min, a temperature of 900°C, and calcined for 1 h to obtain a cobalt-nitrogen-carbon non-precious metal catalyst.
[0043] In order to prove the technical solution provided by the present application, the activity evaluation experiment and data of the cobalt-nitrogen-carbon non-precious metal catalyst provided by the present application are given below.
[0044] 100 mg of the catalyst prepared in Examples 1-5 above were taken respectively and placed in a micro fixed bed reactor for experiment. The experimental conditions were as follows: room temperature (20°C), 20% oxygen, 80% nitrogen, formaldehyde gas was bubbled into the reaction system by nitrogen, the reactor inlet formaldehyde concentration was controlled to be 50 ppm, and the reaction space velocity (GHSV) was 60000 ml / (g·h)SV. The activity of each catalytic sample after 12 hours of stable catalysis was as follows:
[0045] Table 1 BET specific surface area of cobalt-carbon non-precious metal catalysts
[0046]
[0047] Table 2 Activity evaluation results of cobalt-carbon non-precious metal catalysts.
[0048] sample Room temperature formaldehyde conversion rate (%) Example 1 Sample 36.5 Example 2 Sample 71.6 Example 3 Sample 67.8 Example 4 Sample 94.6 Example 5 Sample 93.3
Claims
1. A cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature, characterized in that: The cobalt-nitrogen-carbon non-noble metal catalyst for removing formaldehyde at room temperature is composed of carbon nitride doped with cobalt and a carbon carrier; It is prepared by the following method: 1) Preparation of catalyst precursor Cobalt acetate, nitrogen-containing ligand and carbon carrier are weighed in a mass ratio of 1:2-4:2.5-3.5, and the weighed cobalt acetate and nitrogen-containing ligand are added to anhydrous ethanol in sequence, and placed in a constant temperature magnetic stirring instrument and stirred at room temperature for 0.2-1h until fully dissolved to obtain a raw material solution; then the weighed carbon carrier is introduced into the solution, heated to 50°C and fully stirred for 0.05-0.15h, and vacuum evaporated to dryness for 0.5-1.5h to obtain a catalyst precursor; 2) Calcination calcining and pyrolyzing the catalyst precursor prepared in step 1) under a nitrogen atmosphere to obtain a cobalt-nitrogen-carbon non-noble metal catalyst; The nitrogen-containing ligand is o-phenylenediamine.
2. The cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature according to claim 1, characterized in that: The mass ratio of the carbon nitride doped with cobalt element to the carbon carrier is 1:7-10.
3. The cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature according to claim 1, characterized in that: The carrier is activated carbon or carbon black.
4. The method for preparing a cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature according to claim 1, characterized in that: The steps are as follows: 1) Preparation of catalyst precursor Cobalt acetate, nitrogen-containing ligand and carbon carrier are weighed in a mass ratio of 1:2-4:2.5-3.5, and the weighed cobalt acetate and nitrogen-containing ligand are added to anhydrous ethanol in sequence, and placed in a constant temperature magnetic stirring instrument and stirred at room temperature for 0.2-1h until fully dissolved to obtain a raw material solution; then the weighed carbon carrier is introduced into the solution, heated to 50°C and fully stirred for 0.05-0.15h, and vacuum evaporated to dryness for 0.5-1.5h to obtain a catalyst precursor; 2) Calcination The catalyst precursor prepared in step 1) is calcined and pyrolyzed in a nitrogen atmosphere to obtain a cobalt-nitrogen-carbon non-precious metal catalyst.
5. The method for preparing a cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature according to claim 4, characterized in that: The vacuum evaporation operation steps described in step 1) are specifically as follows: placing the conical beaker containing the solution in a constant temperature water bath, maintaining the water temperature at 50°C, connecting a vacuum circulation pump using a T-type three-way connector, evaporating anhydrous ethanol under stirring, and then vacuum drying to obtain a solid powder; pouring the remaining solid material into an agate mortar and grinding it thoroughly to obtain a catalyst precursor.
6. The method for preparing a cobalt-nitrogen-carbon non-precious metal catalyst for removing formaldehyde at room temperature according to claim 4, characterized in that: In step 2), the calcination and pyrolysis conditions are under nitrogen protection, with a tubular furnace heating rate of 5°C / min, a calcination temperature of 300-900°C, a calcination time of 1h, and a nitrogen flow rate of 20mL / min.