Stress-adjustable corrosion device and corrosion test method for degradable human implant materials

By designing a zinc-based biomedical metal material corrosion device with adjustable stress, the existing technology cannot simulate the inadequacy of material corrosion by the inability to simulate the internal stress and flow rate of human body, achieving more accurate corrosion tests on zinc-based materials, providing a more realistic Human environment simulation.

CN115598049BActive Publication Date: 2024-11-19NANJING INST OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211373671.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-03
Publication Date
2024-11-19
Estimated Expiration
2042-11-03

AI Technical Summary

Technical Problem

The prior art cannot truly simulate the stress corrosion of zinc-based degradable biomedical metal materials in the human body, especially the impact of blood flow rate on the material, resulting in inaccurate corrosion test results.

Method used

A stress adjustable corrosion device including a stirring mechanism, a heating mechanism, a sample fixing mechanism and an intake mechanism is designed. Dynamic stress corrosion test on zinc-based materials is achieved through adjustable spring length, oxygen flow control and agitating paddle, and simulated Complex environment in the human body.

Benefits of technology

The device can more realistically simulate the corrosion conditions of zinc-based materials by stress and flow rates in the human body, providing more accurate corrosion rate data, helping to understand the impact of tensile stress and oxygen flow on corrosion reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115598049B_ABST
    Figure CN115598049B_ABST
Patent Text Reader

Abstract

The present invention discloses a stress-adjustable corrosion device and corrosion test method for degradable human implant materials. The corrosion device includes a stirring mechanism, a heating mechanism, a sample fixing mechanism, an air intake mechanism, a corrosion tank and a water bath; the heating mechanism includes a heating resistor, a sensor and a temperature controller; the sample fixing mechanism includes a spring, a first sample fixing rod, a second sample fixing rod, a screw, a slider, a guide groove, a tensile stress sensor and a digital display. When the present invention performs a corrosion test, the slider is driven to move in the guide groove by the screw, the elongation of the spring is increased, the tensile stress is obtained by the tensile stress sensor and the digital display, the knob is adjusted to the preset stress applied to the sample to be tested, and the sample is immersed in a corrosive medium, and temperature control is performed at the same time, oxygen is delivered and the corrosive medium is stirred, and the corrosive medium is discharged after the test. The present invention realizes dynamic corrosion under different flow rates, different oxygen flow rates and different stresses, and improves the integrity and reliability of the corrosion test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of corrosion of degradable biomedical metal materials, and in particular to a stress-adjustable corrosion device and a corrosion testing method for degradable human body implant materials. Background Art

[0002] Zinc-based biodegradable biomedical metal materials have attracted extensive attention due to their excellent mechanical properties and good biocompatibility, but their corrosion rate does not match the needs of the human body, which seriously restricts their clinical use. In order to gain a deeper understanding of the degradation process of zinc-based alloys as stent materials in the human body, a variety of in vitro dynamic degradation devices that simulate the human blood environment have been published.

[0003] The prior art discloses an in vitro dynamic corrosion simulation device for biomedical materials in the field of biomedical material technology with application number: 200720075388.7 and an in vitro dynamic corrosion simulation device for biomedical materials with authorization announcement number: CN207133170U. These two devices can only detect the corrosion process of the fluid on the sample, but fail to take into account the stress corrosion of the blood vessel wall to which the biological implant material is subjected, and cannot more realistically simulate the actual corrosion situation of the implant material.

[0004] The dynamic stress corrosion device for biodegradable vascular stent materials with the authorization announcement number CN210626288U has a stress mechanism outside the sample tube for providing stress to the sample inside the sample tube, and the liquid supply device, joint and connecting pipe are all located in a constant temperature water bath. This technology provides an in vitro corrosion simulation device for biodegradable materials that is more in line with the human vascular environment, and realizes the test of stress-added dynamic corrosion. However, the device can only detect the corrosion process of the sample by fluid and compressive stress, and fails to reflect the stress corrosion of the implant material by blood flow rate, and still cannot better simulate the real environment of the implant in the body. Summary of the invention

[0005] Purpose of the invention: In order to overcome the defects of the prior art, the present invention provides a stress-adjustable corrosion device and a corrosion testing method for degradable human implant materials, that is, by applying different stress levels to the sample and calculating its different corrosion rates, it is possible to more clearly understand the effect of tensile stress and oxygen flow on the entire corrosion reaction process.

[0006] Technical solution: The stress-adjustable corrosion device for degradable human implant materials of the present invention comprises a stirring mechanism, a heating mechanism, a sample fixing mechanism, an air intake mechanism, a corrosion tank and a water bath;

[0007] The heating mechanism includes a heating resistor, a sensor and a temperature controller; the sample fixing mechanism includes a spring, a first sample fixing rod, a second sample fixing rod, a screw rod, a slider, a guide groove, a tensile stress sensor and a digital display;

[0008] One end of the spring is connected to the tensile stress sensor, and the other end is connected to the first sample fixing rod, and the first sample fixing rod and the second sample fixing rod are immersed in the corrosive medium;

[0009] The stirring mechanism, heating mechanism and sample fixing mechanism are all placed in the corrosion tank, and the corrosion tank is placed in the water bath.

[0010] The air intake mechanism includes a pressure reducing valve, a flow meter, an air intake pipe, an exhaust plate and an oxygen cylinder. A plurality of air outlet branches are distributed on the surface of the exhaust plate, and the exhaust plate is placed at the bottom of the corrosion tank.

[0011] The exhaust plate comprises an exhaust port and a branch exhaust pipe, and a hole is opened on the branch exhaust pipe.

[0012] One end of the sensor is connected with a slider, the slider is in a guide slide groove, the guide slide groove is connected with a first sample fixing rod, and the screw rod is in the guide slide groove and connected with the slider.

[0013] The heating mechanism comprises a heating resistor, a sensor and a temperature controller, and the heating resistor and the sensor are arranged at the bottom of the corrosion tank.

[0014] The stirring mechanism includes a motor and a stirring paddle.

[0015] The stress-adjustable corrosion testing method for degradable human implant materials of the present invention comprises the following steps:

[0016] (1) Fix the sample, rotate the screw knob, move the slider in the guide groove through the screw, adjust the elongation of the spring to the minimum, cover the small holes at both ends of the sample to be tested on the first sample fixing rod and the second sample fixing rod pin 713 respectively, and then rotate the knob to drive the slider to move in the guide groove through the screw to increase the elongation of the spring, obtain the tensile stress through the tensile stress sensor and the digital display, adjust the knob to the preset stress applied to the sample to be tested, and then insert the sample fixing mechanism into the groove in the water bath tank cover, cover the water bath tank cover, and before covering the water bath tank cover, cover the corrosion tank cover first, and immerse the sample to be tested in the corrosive medium through the hole opened in the corrosion tank cover;

[0017] (2) Temperature control: according to the test conditions, the temperature controller sets the heating temperature, turns on the power, heats the corrosive medium through the resistance wire, and controls the temperature with the thermocouple;

[0018] (3) Supply oxygen. Open the pressure reducing valve on the oxygen cylinder to adjust the oxygen pressure. Then adjust the flow meter to control the amount of oxygen input. The oxygen is transported to the exhaust plate at the bottom of the corrosion tank through the air inlet pipe. The oxygen enters the branch exhaust pipe through the exhaust port and enters the corrosive medium through the hole.

[0019] (4) Stir the corrosive medium. According to the required flow rate, start the agitator and stir the corrosive medium with the stirring paddle. The dynamic stress corrosion test begins. Complete according to the requirements of the experiment. After the test, discharge the corrosive medium through the drainage port of the corrosion tank and collect the waste liquid.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following advantages: The present invention utilizes an adjustable spring length to introduce oxygen into the flowing corrosive medium, thereby solving the deficiency of single stress corrosion on the corrosion of human implants. The stress and flow rate are adjustable, and the gas flow rate is controllable. It is a more complete test of the corrosion of human implant materials under real conditions, and is a technical innovation in this field. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic structural diagram of the stress-adjustable corrosion device for degradable human implant materials of the present invention;

[0022] Figure 2 It is a schematic diagram of the structure of the sample fixing mechanism of the present invention;

[0023] Figure 3 This is a schematic diagram of the guide chute of the present invention;

[0024] Figure 4 It is a schematic diagram of the screw rod of the present invention;

[0025] Figure 5 It is a schematic diagram of a slider of the present invention;

[0026] Figure 6 This is a schematic diagram of a first sample clamping rod of the present invention;

[0027] Figure 7 This is a schematic diagram of a second sample clamping rod of the present invention;

[0028] Figure 8 It is a schematic diagram of the exhaust disk;

[0029] Fig. 9 Schematic diagram of the water bath lid. DETAILED DESCRIPTION

[0030] like Figure 1 As shown, the stress-adjustable corrosion device for degradable human implant material of the present invention comprises a stirring mechanism, a heating mechanism, a sample fixing mechanism and an air intake mechanism, wherein the stirring mechanism comprises a motor 6 and a stirring paddle 5; the heating mechanism comprises a heating resistor 14, a thermocouple 17 and a temperature controller 18. The sample fixing mechanism comprises a spring 705, a first sample fixing rod 712, a second sample fixing rod 701, a screw rod 709, a slider 708, a guide groove 711, a tensile stress sensor 706 and a digital display 707, wherein the first sample fixing rod 712 and the second sample fixing rod 701 in the sample fixing mechanism are immersed in the corrosive medium.

[0031] One end of the spring 705 in the sample fixing mechanism is connected to the tensile stress sensor 706, and the other end is connected to the second sample fixing rod 701 through the crossbeam 702; and the other end of the tensile stress sensor (706) is connected to the slider 708, the slider 708 is in the guide slot 711, the guide slot 711 and the crossbeam connected to the second sample fixing rod (701) are connected by a pin, the screw rod 709 is in the guide slot 711 and threadedly cooperates with the slider 708, and the guide slot 711 is fixedly connected to the first sample fixing rod (712). By rotating the knob on the screw rod 709, the slider 708 is driven to move in the guide slot 711, and the elongation of the spring 705 is adjusted, thereby changing the magnitude of the tension.

[0032] The air intake mechanism includes a pressure reducing valve 2, a flow meter 3, an air intake pipe 4, an exhaust disk 13 and an oxygen cylinder 1. The oxygen cylinder 1 adjusts the oxygen pressure, and the air intake pipe 4 transports oxygen to the exhaust disk 13 at the bottom of the corrosion tank 9.

[0033] The stirring mechanism, the heating mechanism, and the sample fixing mechanism are all placed in the corrosion tank 9, and the corrosion tank 9 is placed in the water bath 11.

[0034] The present invention is applicable to the adjustable stress dynamic corrosion of metal materials, and only requires replacing the sample 12 with other metal materials.

[0035] The stress-adjustable corrosion testing method for degradable human implant materials of the present invention comprises the following steps:

[0036] (1) Fix the sample 12, rotate the screw knob 710, move the slider 708 in the guide groove 711 through the screw 709, adjust the elongation of the spring 705 to the minimum, and respectively cover the small holes at both ends of the sample 12 to be tested on the pins 703 of the first sample fixing rod 712 and the second sample fixing rod 701, and then rotate the knob 710 to drive the slider 708 to move in the guide groove through the screw 709, increase the elongation of the spring, obtain the tensile stress through the tensile stress sensor 706 and the digital display 707, adjust the knob 710 to the preset stress applied to the sample 12 to be tested, and then insert the sample fixing mechanism 7 into the groove 102 in the water bath cover 10, and cover the water bath cover 10, where 101 is the cover opening. Before covering the water bath cover 10, first cover the cover 8 of the corrosion tank 9, and immerse the sample to be tested in the corrosive medium through the hole opened in the cover 8 of the corrosion tank 9;

[0037] (2) Temperature control: according to the test conditions, the temperature controller 18 sets the heating temperature, turns on the power, heats the corrosive medium through the resistance wire 14, and the thermocouple 17 controls the heating temperature;

[0038] (3) Supply oxygen. Open the pressure reducing valve 2 on the oxygen cylinder 1 to adjust the oxygen pressure. Then adjust the flow meter 3 to control the amount of oxygen input. The oxygen is delivered to the exhaust plate 13 at the bottom of the corrosion tank 9 through the air inlet pipe 4. The oxygen enters the branch exhaust pipe 1302 through the exhaust port 1301 and enters the corrosion medium through the small hole 1303.

[0039] (4) Stirring the corrosive medium. According to the required flow rate, start the stirrer 6, and stir the corrosive medium with the stirring paddle 5, and the dynamic stress corrosion test begins. Complete the test according to the experimental requirements. After the test, discharge the corrosive medium through the corrosion tank drain port 16 and collect the waste liquid.

Claims

1. A stress-adjustable corrosion device for degradable human implant materials, characterized in that: It comprises a stirring mechanism, a heating mechanism, a sample fixing mechanism, an air intake mechanism, a corrosion tank (9) and a water bath tank (11); The heating mechanism comprises a heating resistor (14), a sensor and a temperature controller (18); the sample fixing mechanism comprises a spring (705), a first sample fixing rod (712), a second sample fixing rod (701), a screw rod (709), a slider (708), a guide groove (711), a tensile stress sensor (706) and a digital display (707); The first sample fixing rod (712) and the second sample fixing rod (701) are immersed in a corrosive medium; One end of the spring (705) in the sample fixing mechanism is connected to the tensile stress sensor (706), and the other end is connected to the second sample fixing rod 701 through the crossbeam (702); the other end of the tensile stress sensor (706) is connected to the slider (708), the slider (708) is in the guide slot (711), the guide slot (711) and the crossbeam connected to the second sample fixing rod (701) are connected by a pin, the screw rod (709) is in the guide slot (711) and is threadedly matched with the slider (708), and the guide slot (711) is fixedly connected to the first sample fixing rod (712); by rotating the knob on the screw rod (709), the slider (708) is driven to move in the guide slot (711), and the elongation of the spring (705) is adjusted, thereby changing the magnitude of the tensile force; The stirring mechanism, heating mechanism and sample fixing mechanism are all placed in a corrosion tank (9), and the corrosion tank (9) is placed in a water bath tank (11).

2. The stress-adjustable corrosion device for degradable human implant material according to claim 1, characterized in that: The air intake mechanism comprises a pressure reducing valve (2), a flow meter (3), an air intake pipe (4), an exhaust plate (13) and an oxygen cylinder (1); a plurality of exhaust branch pipes are distributed on the surface of the exhaust plate (13); and the exhaust plate (13) is placed at the bottom of the corrosion tank (9).

3. The stress-adjustable corrosion device for degradable human implant material according to claim 2, characterized in that: The exhaust plate (13) comprises an exhaust port (1301) and a branch exhaust pipe (1302), and a hole (1303) is provided on the branch exhaust pipe (1302).

4. The stress-adjustable corrosion device for degradable human implant material according to claim 1, characterized in that: The heating mechanism comprises a heating resistor (14), a sensor and a temperature controller (18), and the heating resistor (14) and the sensor are placed at the bottom of the corrosion tank (9).

5. The stress-adjustable corrosion device for degradable human implant material according to claim 1, characterized in that: The stirring mechanism comprises a motor (6) and a stirring paddle (5).

6. A stress-adjustable corrosion test method for degradable human implant materials, implemented by the stress-adjustable corrosion test device for degradable human implant materials according to claim 1, characterized in that: The method comprises the following steps: (1) Fix the sample (12), rotate the screw knob (710), move the slider (708) in the guide groove (711) through the screw (709), adjust the elongation of the spring to the minimum, put the two ends of the sample to be tested on the first sample rod and the second sample rod, and then rotate the knob (710) to drive the slider to move in the guide groove through the screw (709), increase the elongation of the spring, obtain the tensile stress through the tensile stress sensor, adjust the knob to the preset applied stress, and then insert the sample fixing mechanism into the water bath tank cover, cover the corrosion tank cover, immerse the sample in the corrosive medium through the corrosion tank cover, and then cover the water bath tank cover; (2) temperature control, the temperature controller (18) sets the heating temperature, the corrosive medium is heated by the heating resistor (14), and the temperature is controlled by the sensor; (3) supplying oxygen, opening the oxygen cylinder (1), adjusting the oxygen pressure, and then adjusting the amount of oxygen input by the flow meter (3), and delivering the oxygen to the exhaust plate (13) at the bottom of the corrosion tank (9) through the air inlet pipe, and the oxygen enters the branch exhaust pipe (1302), and enters the corrosion medium through the small hole (1303); (4) Start the agitator to stir the corrosive medium and start the dynamic stress corrosion test. After the test, discharge the corrosive medium through the corrosion tank drain port and collect the waste liquid.