Anionic PGM carboxylates-assisted synthesis of PGM nanoparticles for exhaust gas treatment applications
By combining anionic complexes of PGM and carboxylate ions with the support material, electrostatic interactions are used to solve the fixation problem of PGM on the support material, improving catalytic activity and stability, simplifying the manufacturing process and reducing by-product release .
Patent Information
- Application Number
- CN202210810487.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-07-21
- Filing Date
- 2022-07-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-07-11
AI Technical Summary
The prior art is difficult to firmly place platinum group metals (PGMs) on the carrier material, resulting in migration and wicking, and conventional methods release harmful NOx by-products during calcination, increasing manufacturing costs and steps.
Anionic complexes containing PGM and carboxylate ions are combined with the carrier material to form stronger fixation through electrostatic interactions, reducing steps and reducing by-product release, and enhancing electrostatic attraction using a low pH environment.
This achieves a firmer fixation of PGM on the support material, reduces the passage or mixing of the support coating, improves catalytic activity and stability, while reducing the release of harmful by-products, and simplifies the manufacturing process.
Smart Images

Figure CN115608356B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a catalyst product, a catalyst product obtainable by the method, an emission treatment system, and a method for treating exhaust gases. Background Art
[0002] Platinum group metals (PGMs) are important components in exhaust gas catalysts such as three-way catalysts (TWCs), diesel oxidation catalysts (DOCs) and NO x The key component in the trap catalyst. To maximize efficiency, it is desirable to selectively and / or reliably place the PGM on the target support material. Conventional catalyst preparation methods use PGM simple salts as PGM sources, usually PGM nitrates. However, using such conventional methods, it is difficult to place PGM on certain support materials. This is because when preparing the carrier coating (washcoat), the interaction between the support material and the PGM is weak. In order to overcome this problem, the method that has been considered includes pre-fixing the PGM to the target support material by impregnation followed by calcination, spray drying and reduction-deposition. However, all of these schemes require multiple / additional processing steps. In addition, during calcination to fix the PGM to the support material, the decomposition of nitrates can cause harmful NO x Release of by-products.
[0003] When using PGM nitrate precursors, due to the lack of strong interaction between the PGM and the support material, metal migration may occur, which means that the specific different layer arrangements within the catalyst article may mix, which may cause deactivation of the layers when these layers are included for, e.g., specific different purposes. In addition, such catalyst articles may be prone to excessive wicking of the supported PGM catalyst through the substrate when exposed to further wet-applied washcoat, especially when palladium is used.
[0004] Therefore, there is a need to provide an improved method for manufacturing catalyst products comprising PGMs supported on support materials, particularly such catalyst products in which the PGMs can be more firmly bound to the support material to avoid migration and / or wicking, release fewer harmful by-products during the manufacturing process, and which require fewer steps for simple manufacturing and reduced manufacturing costs.
[0005] WO 96 / 31275 relates to PGM carboxylates, in particular PGM lactates, which are useful as precursors for the manufacture of catalyst products. However, anionic PGM complexes are not described.
[0006] "Free rhodium(II)citrate and rhodium(II)citrate magnetic carriers as potential strategies for breast cancer therapy", Carneiro et al., Journal of Nanobiotechnology, 2011, 9: 11; "Carboxylates of Palladium, Platinum, and Rhodium, and their Adducts", Stephenson et al., Journal of the Chemical Society, 1965, 667, 3632-3640; and "Preparation and Properties of Anhydrous Rhodium(II)acetate and Some Adducts Thereof", Johnson et al., Inorganic Chemistry, 1963, 2, 5, 960-962, each describes a PGM carboxylate complex. However, none of these publications are in the field of preparing catalyst preparations for applications such as treating exhaust gases. Summary of the invention
[0007] One aspect of the present invention relates to a method for manufacturing a catalyst product, which includes: providing an anion complex comprising PGM and carboxylate ions; providing a support material; applying the anion complex to the support material to form a supported support material; placing the supported support material on a substrate; and heating the supported support material to form PGM nanoparticles on the support material.
[0008] Another aspect of the present invention relates to a catalyst product obtained by the method of the first aspect.
[0009] The invention also includes an exhaust system for an internal combustion engine comprising the catalyst article of the second aspect.
[0010] The present invention also includes a method of treating an exhaust gas, the method comprising: providing the catalyst article of the second aspect; and contacting the catalyst article with the exhaust gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 The palladium distribution on the palladium citrate coated core by EPMA method is shown (Example 6).
[0012] Figure 2 The palladium distribution on the palladium nitrate coated core by EPMA method is shown (Example 6). DETAILED DESCRIPTION
[0013] The present invention seeks to address at least some of the problems associated with the prior art, or at least provide a commercially acceptable alternative solution to these problems.
[0014] In a first aspect, the present invention provides a method of making a catalyst article, the method comprising:
[0015] providing an anionic complex comprising a PGM and a carboxylate ion;
[0016] providing carrier materials;
[0017] applying the anionic complex to a support material to form a supported support material;
[0018] placing the supported carrier material on a substrate; and
[0019] The supported support material is heated to form PGM nanoparticles on the support material.
[0020] Each aspect or embodiment defined herein may be combined with any other aspect or embodiment unless explicitly indicated to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature indicated as being preferred or advantageous.
[0021] Surprisingly, when used in an emission treatment system, the catalyst article manufactured by the method of the present invention can show significantly reduced wicking of the carrier coating through or into the substrate and / or mixing of the carrier coating compared to the catalyst article prepared by the conventional method. In other words, the catalyst article manufactured by the method of the present invention can show a stronger / more reliable fixation of the PGM to the carrier material compared to the catalyst article manufactured by the conventional method. And as an aesthetic improvement in such a catalyst article, the catalyst article manufactured by the method of the present invention can therefore show improved catalytic activity. This is at least because the mixing of catalytically active PGMs between any different carrier coatings in the catalyst article can be reduced, which can thereby reduce the possibility of any carrier coating deactivation. When the catalyst article is fresh, and after aging, this can help keep the catalytic activity of the entire catalyst article as high as expected. Keeping the PGMs of any different carrier coatings in their respective target layers is important for maintaining their target catalytic purposes, whether for example for oxidation or reduction. For example, it is known that the direct interaction between Pd and Rh can reduce the catalytic activity of a single component, particularly the catalytic function of the Rh component.
[0022] Without wishing to be bound by theory, it is believed that these surprising and advantageous properties exhibited by the catalyst article manufactured by the method of the present invention can be achieved because of the strong electrostatic interaction between the support material and the anionic complex. When the method is carried out at a low pH, for example, at a pH of 8 or lower, the interaction will be particularly strong. The anionic complex of the present invention can be electrostatically attracted to the support material, which usually has a (weak) positive charge in the solution. Therefore, due to such electrostatic interactions, the anionic complex is unlikely to be separated from the supported support material. In addition, when preparing a support coating (washcoat) solution, the anionic complex will be attracted to the support material, thereby actively gathering in the solution to form a supported support material. This will therefore cause a higher proportion of PGM to actually be loaded (i.e., "fixed" or "loaded") on the support material. This is in contrast to the traditional support coating (washcoating) method using a PGM nitrate precursor, in which, for example, neutral PGM nitrates and / or PGM cations will be "loose" in the solution, i.e., there is no obvious electrostatic attraction to the support material. It is also believed that due to such stronger interactions between the anionic complex and the support material, a more uniform dispersion of the PGM supported on the support material throughout the catalyst preparation can be achieved.
[0023] Advantageously, when the supported support material is heated and / or calcined to form PGM nanoparticles on the support material, due to the composition of the anion complex, i.e., the carboxylate ion ligand, less harmful byproducts such as NO are released compared to conventional methods using PGM nitrate precursors. x Without wishing to be bound by theory, it is believed that this is because nitrates decompose into NO when heated. x , while the carboxylate ion ligands of the present invention decompose into less harmful or "cleaner" byproducts, such as only carbon dioxide and water. In other words, upon heating, the anionic complexes of the present invention are believed to decompose / reduce only to PGM metal (or metal oxide / hydroxide), CO2 and H2O. In addition, it has been found that the anionic complexes of the present invention automatically reduce the PGM centers when heated. In other words, upon heating, the ligands can decompose and reduce PGM to PGM metal without any additional process steps such as chemical reduction or gas phase reduction to produce the catalyst in active form, i.e., with supported PGM metal (nanoparticles).
[0024] Advantageously, the anionic complexes of the present invention may also have a high solubility in water. This is advantageous because it allows conventional aqueous carrier coating techniques to be used without having to substantially change the technique due to a change in precursors.
[0025] Compared to, for example, WO96 / 31275, in which the PGM precursor is not an anionic complex, the catalyst article produced by the process of the present invention will therefore exhibit the above-mentioned advantageous properties, at least in part due to increased electrostatic attraction between the PGM precursor and the support material.
[0026] The term "catalyst article" as used herein may include an article on which or in which a catalyst is supported. The article may take the form of, for example, a honeycomb monolith or a filter such as a wall flow filter or a flow-through filter. The catalyst article may be used in an emission treatment system, in particular for an emission treatment system of a gasoline engine, preferably a stoichiometric gasoline engine. The catalyst article may be used for three-way catalysis, i.e. as a three-way catalyst (TWC). Alternatively, the catalyst article may be used in an emission treatment system for a diesel engine. The catalyst article may be used for diesel oxidation catalysis, i.e. as a diesel oxidation catalyst (DOC). The catalyst article may also be used for NO x Sink catalysis, that is, used as NO x Trap catalyst.
[0027] Providing an anionic complex comprising a PGM and a carboxylate ion generally comprises providing a solution of the anionic complex, such as an aqueous solution or an alcoholic solution, preferably an aqueous solution.
[0028] As used herein, the term "anionic complex" includes any complex comprising at least one metal center and at least one ligand, wherein the overall charge of the at least one metal center and the at least one ligand is less than zero. Thus, anionic complexes are typically associated with a positive counterion. Possible positive counterions are further described below.
[0029] As used herein, the term "PGM" means "platinum group metals" and may include, for example, one or more of platinum, palladium, rhodium, ruthenium, osmium and iridium. Preferably, the PGM includes one or more of platinum, palladium and rhodium, depending on the target application, such as use as a TWC, DOC or NO x The anionic complex may contain one or more PGM metal centers. For example, the anionic complex may contain two or more metal centers, such as two or three metal centers.
[0030] As used herein, the term "carboxylate ion" has its ordinary meaning in the art, i.e., a carboxylate ion of the general formula RCOO - Where R is any group, usually any organic group. Therefore, usually the carboxylate ion is connected via -COO - However, the carboxylate ion may alternatively and / or additionally coordinate to the PGM metal via another functional group such as another -COO -The anionic complex may be coordinated by a group or a different functional group such as an -OH group. The anionic complex may contain one or more carboxylate ions, depending on the size and / or number of the functional groups of the carboxylate ions, for example. R preferably consists of C, H and O. Advantageously, this will cause the anionic complex to decompose only into PGM metals (or metal oxides / hydroxides), CO2 and H2O. Preferred carboxylate ions for use in the present invention are discussed further below.
[0031] The support material can be any material capable of loading the anionic complex and the nanoparticles thereon or therein. The support material can take any form, but is typically in powder form, more typically a high surface area powder. When the method of the present invention is used to prepare a catalytic filter such as a wall flow filter or a flow-through filter, the support material will typically be in powder form having a D50 of, for example, 0.1-25 μm, more typically 0.5-5 μm, measured using TEM. Such a particle size will facilitate the desirable rheology of the slurry used to coat the filter. The support material can act as a washcoat. The support material can be a washcoat or can be part of a washcoat.
[0032] The support material may also act as an oxygen storage material, which stores and releases oxygen under fuel-lean and fuel-rich conditions, respectively, for promoting three-way catalytic conversion or other catalytic applications.
[0033] Applying the anionic complex to the support material typically comprises contacting the anionic complex and the support material in the presence of a solvent (typically water) to produce a slurry. As used herein, the term "slurry" may include a liquid containing insoluble materials, such as insoluble particles. The slurry may contain (1) a solvent; (2) soluble contents, such as "free", uncomplexed carboxylate ions or carboxylic acid molecules, inorganic PGMs and promoter precursors, and anionic complexes (outside the support, i.e., unloaded anionic complexes); and (3) insoluble contents, such as support particles that have and do not interact with the anionic complex and the metal precursor. Preferably, the slurry comprises primarily (1) and (3), such as 70 wt% or more of (1) and (3), based on the total weight of (1), (2) and (3), such as 80 wt% or more of (1) and (3) or even 90 wt% or more of (1) and (3). The slurry is typically stirred, more typically for at least 10 minutes, more typically for at least 30 minutes, and even more typically for at least 1 hour. In addition to theoretically possible electrostatic interactions, increasing the contact and / or stirring time may also increase the amount of anionic complex supported on the support material.
[0034] As used herein, the term "supported support material" may include a support material on which an anionic complex is supported (e.g., on the surface of a high surface area metal oxide support material) and / or in which (e.g., in the pores of a zeolite support material). The anionic complex is typically fixed to the support, for example, by electrostatic forces, hydrogen bonds, coordination bonds, covalent bonds, and / or ionic bonds. For example, in the case of an oxide that has a positive charge, there may be strong electrostatic forces between the anionic complex and the support material. However, there may also be other interactions due to the functional groups of the (carboxylate ion) ligands, such as electrostatic forces or hydrogen bonds formed due to the interaction of carboxylate functional groups and / or other functional groups such as hydroxyl groups with hydroxyl groups on the support.
[0035] As used herein, the term "substrate" may include, for example, a ceramic or metal honeycomb, or a filter block, such as a wall flow filter or a flow-through filter. The substrate may include a ceramic monolith substrate. The material composition, size and configuration, pore shape and density, and wall thickness of the substrate may vary. Suitable substrates are known in the art.
[0036] Placing the carried support material on the substrate can be performed using techniques known in the art. Typically, a slurry of the carried support material is poured into the inlet of the substrate in a predetermined amount using a specialized molding tool to place the carried support material on the substrate. As discussed in more detail below, subsequent vacuum and drying steps can be used in the placing step. When the support is a filter block, the carried support material can be placed on the filter wall, in the filter wall (if porous), or both.
[0037] The supported support material is usually heated in an oven or furnace, more usually a belt or static oven or furnace, usually in hot air at a specific flow rate from one direction. Heating can include calcining. Heating can also include drying. The drying and calcining steps can be continuous or sequential. For example, after the substrate has been coated with a support, another support coating can be applied and dried together with the previous support coating. If the coating is completed, the support-coated substrate can also be dried and calcined using a continuous heating program. During the heating process, the anionic complex can be at least partially, substantially or completely decomposed. In other words, the ligand of the complex, i.e., the carboxylate ion, is at least partially, substantially or completely removed or separated from the PGM and removed from the final catalyst product. The particles of such separated PGM can then begin to form metal-metal and metal-oxide bonds. As a result of heating (calcining), the substrate is generally substantially free of carboxylate ions, more generally completely free of carboxylate ions.
[0038] As used herein, the term "nanoparticle" may include particles having a diameter of 0.01 nm to 100 nm as measured by TEM. The nanoparticle may be in any shape, such as spherical, plate-like, cubic, cylindrical, hexagonal or rod-like, but is typically spherical. The maximum size of the nanoparticle (i.e., if the nanoparticle is spherical, its diameter) will typically be 0.5 to 10 nm, more typically 1 to 5 nm, as measured by TEM.
[0039] After the heating step, the substrate is typically cooled, more typically to room temperature. Cooling is typically performed in air, with or without a coolant / medium, typically without a coolant.
[0040] The carboxylate ion preferably comprises two or more carboxyl functional groups, for example 2-4 carboxyl functional groups. In some preferred embodiments, the carboxylate ion comprises 2 carboxyl functional groups. In other preferred embodiments, the carboxylate ion comprises 3 carboxyl functional groups. When the carboxylate ion comprises 2 or more carboxyl functional groups, for example at least one carboxyl functional group can coordinate to one or more metal centers of the anionic complex. For example, without wishing to be limited by theory, in some embodiments, 2 or more carboxyl functional groups can coordinate to one or more metal centers of the anionic complex, for example to form a chelating ligand or a bridging ligand. For example, in other embodiments, without wishing to be limited by theory, it is believed that one or more of the carboxyl functional groups can interact with the support material, for example to form electrostatic interactions and / or hydrogen bonds with any exposed hydroxyl groups on the (oxide) support material. These interactions can be present in addition to the coordination of one or more of the carboxyl functional groups to one or more metal centers of the anionic complex. Without wishing to be bound by theory, it is believed that in this case these further interactions (i.e. in addition to any electrostatic interactions caused by the anionic complex as described above) may also contribute to the above-mentioned advantageous properties of the anionic complexes of the invention, for example providing even stronger interactions or "bonding" to the support material.
[0041] In a preferred embodiment, the carboxylate ion comprises 2-6 carbon atoms, such as 2,3,4,5 or 6 carbon atoms. In order to realize the present invention, the number of carbon atoms in the carboxylate ion may not be particularly limited. However, it is not desired to be limited by theory, it is believed that the higher the number of carbon atoms of the carboxylate ion, the lower the solubility of the anion complex formed in water. It is desirable that the anion complex can have a high solubility in water. Therefore, it is believed that it is desirable that the number of carbon atoms in the carboxylate ion may be, for example, no more than 6. It is desirable that the anion complex can have a high solubility in water, at least because conventional carrier coating techniques are carried out in aqueous solution. Therefore, in order to make the PGM precursor of the present invention, i.e., the anion complex, be used for conventional carrier coating techniques, even if conventional techniques can be made without significant adjustments, it is desirable that the anion complex has a high solubility in water. Furthermore, it is therefore desirable that the carboxylate ions in the anionic complexes used in the present invention have a good balance between higher water solubility (e.g., by having fewer carbon atoms) and having stronger interactions or "bonding" with the support material (e.g., by a greater negative charge on the anionic complex and / or by greater interactions such as electrostatic or hydrogen bonding with the support material, for example due to carboxylate ions having more functional groups such as carboxyl or hydroxyl functional groups).
[0042] Therefore, in some preferred embodiments, the carboxylate ion comprises a hydroxyl, preferably an alpha-hydroxy acid functional group. Without wishing to be bound by theory, it is believed that such functional groups can increase the number and / or strength of attractions or interactions between the anionic complex and the support material.
[0043] Preferably, the carboxylate ions include one or more of citrate, malate, malonate, succinate, tartrate, glutarate, succinolate, oxalate, lactate and glycolate, more preferably one or more of citrate, malate, malonate, succinate, tartrate, glutarate, succinolate and oxalate, even more preferably the carboxylate ions include citrate and / or malonate. It has been surprisingly found that such carboxylate ions, when used in the anionic complex of the present invention, show strong interactions with the support material, so the advantageous effects described herein are particularly fully exhibited.
[0044] Preferably, the PGM is selected from one or more of rhodium, palladium, platinum and ruthenium. More preferably, the PGM comprises, consists essentially of or consists of rhodium, palladium, platinum or a combination thereof, preferably rhodium and / or palladium. In some preferred embodiments, the PGM comprises, consists essentially of or consists of rhodium. In some preferred embodiments, the PGM comprises, consists essentially of or consists of platinum. In some preferred embodiments, the PGM comprises, consists essentially of or consists of palladium. The selection of platinum, palladium and / or rhodium each for use in the present invention may depend on the specific purpose of the catalyst article, i.e., whether for reduction or oxidation, for example, for TWC or DOC applications. The different applications of each of platinum, palladium and / or rhodium are known to those skilled in the art.
[0045] Particularly preferred anionic complexes comprise one or more of the following: Pt(IV) malonate, Pt(IV) succinate, Pt(II, IV) oxalate, Pd(II) citrate, Pd(II) lactate, Pd(II) oxalate, Pd(II) glycolate, Pd(II) malate, Rh(II) citrate, Rh(III) citrate, Rh(II) lactate, Rh(III) lactate and Ru(III) oxalate, more preferably one or more of the following: Pt(IV) malonate, Pd(II) citrate, Rh(II) citrate and Rh(III) citrate.
[0046] In a preferred embodiment, the anionic complex is provided in the form of an aqueous solution comprising the anionic complex, preferably wherein the pH of the aqueous solution is 8 or less, more preferably 7 or less. The use of an aqueous solution can provide a simple, low-cost method consistent with a more conventional carrier coating method, so that, for example, when using the PGM precursor of the present invention, i.e., the anionic complex, known techniques and additives may not need to be substantially adjusted. This can therefore be easily converted from using a traditional method for making a catalyst product to an improved method of the present invention. As a result of the method for providing anionic complexes for use in the method of the present invention, such an aqueous solution may contain other components, such as "loose" or uncoordinated ligands, such as carboxylate ions or carboxylic acids. For example, due to the method for providing anionic complexes, the aqueous solution may also contain additional acetic acid and / or acetate ions.
[0047] Preferably, at least 70 wt% of the PGM present in the aqueous solution is in the form of anionic complexes as described herein, more preferably at least 80 wt% of the PGM present in the aqueous solution, even more preferably at least 90 wt%, most preferably substantially all or even all of the anionic complexes as described herein. In other words, preferably, other PGM complexes are not present in the aqueous solution, and there are no uncomplexed PGM particles, atoms and / or ions.
[0048] It is desirable that the pH of the aqueous solution is 8 or less, preferably 7 or less, more preferably 6 or less. Without wishing to be bound by theory, it is believed that such a low pH helps to increase the electrostatic attraction between the anionic complex and the support material. This may be because of the presence of H bound in the aqueous solution, for example. + Ions, the carrier material obtains and maintains more positive charge at such pH. This will be particularly evident when the carrier material comprises, for example, oxides. However, when using any suitable carrier material, this effect due to the pH of the aqueous solution can be observed. Using an aqueous solution with such a low pH can therefore help produce the electrostatic attraction that increases between the above-mentioned anionic complex and the carrier material, which can help achieve the above-mentioned favorable effects related to the attraction that increases between the anionic complex and the carrier material. In other words, a lower pH such as 8 or less pH can help produce an even further increased attraction between the anionic complex and the carrier material, thus increasing the surprising effect that the method of the present invention achieves. In addition, such a low pH can help provide anionic complexes, in which the counter ion is a proton or a hydronium ion.
[0049] Preferably, the aqueous solution does not contain PGM nitrates. This can be attributed at least to the properties that the present invention seeks to improve as described above in relation to PGM nitrates, such as greater specificity of PGM placement on the support material, greater fixation of the PGM to the support material, and the production of "less harmful" by-products upon decomposition of the PGM precursor. In other words, the present invention seeks to improve upon conventional methods of making catalyst articles using PGM nitrate precursors, so the methods of the present invention preferably do not include the use of PGM nitrates.
[0050] When the anionic complex is provided in the form of an aqueous solution containing the anionic complex, the anionic complex preferably has a counterion, which preferably includes H + , H3O + and NH4 + One or more of, preferably H + and / or H3O + composition. Preferably, the aqueous solution does not contain elemental inorganic cations. For example, the counterion preferably does not contain elemental inorganic cations. This allows the catalyst product to be formed without contamination by, for example, such inorganic elements. Such an aqueous solution can also help achieve the desired "clean" decomposition of the anion complex during the heating step. Such elemental inorganic cations can include, for example, cations of one or more of sodium, potassium, magnesium and / or calcium (non-exhaustive).
[0051] The anionic complex may comprise one or more additional ligands selected, for example, from water, OH - , acetate ions and bridging O atoms. Preferably, the ligands of the anionic complex comprise carboxylate ions, water, OH- and bridging O atoms, or consisting essentially of or consisting of, depending on the specific carboxylate ion used. Preferably, the anionic complex does not contain phosphorus-containing and / or nitrogen-containing ligands. Thus, such anionic complexes can help achieve a desired "green" decomposition upon heating, such as forming only PGM nanoparticles and releasing CO2 and water upon heating. This is in contrast to conventional methods using, for example, PGM nitrate precursors.
[0052] In some embodiments, the anionic complex comprises more than one PGM center, such as 2 or 3 PGM centers. Thus, such anionic complexes may comprise bridging ligands, such as bridging O atoms and / or bridging carboxylate ions, which may have two or more functional groups, such as two or more carboxyl functional groups and / or additional hydroxyl groups.
[0053] The support material preferably comprises an oxide, preferably one or more of Al2O3, SiO2, TiO2, CeO2, ZrO2, CeO2-ZrO2, V2O5, La2O3 and zeolite. The oxide is preferably a metal oxide. The support material more preferably comprises alumina, even more preferably gamma-alumina. The support material preferably comprises ceria-zirconia. The support material preferably comprises alumina and ceria-zirconia. Alumina and / or ceria-zirconia are preferably doped, more preferably with an oxide of one or more of lanthanum, neodymium, yttrium, niobium, praseodymium, hafnium, molybdenum, titanium, vanadium, zinc, cadmium, manganese, iron, copper, calcium, barium, strontium, cesium, magnesium, potassium or sodium; even more preferably with an oxide of lanthanum, neodymium, praseodymium or yttrium. Such doped oxides are particularly effective as support materials. Preferably, the dopant is present in the alumina and / or ceria-zirconia in an amount of 0.001 wt% to 20 wt%, more preferably 0.5 wt% to 10 wt%. When the anion complex is provided in the form of an aqueous solution containing the anion complex, such a support material may be particularly suitable for the method of the present invention in a preferred embodiment, preferably wherein the pH of the aqueous solution is 8 or less, more preferably 7 or less. This may be because such a support material as described above can ideally obtain a positive charge under such conditions, which produces a strong electrostatic attraction between the support material and the anion complex.
[0054] In certain preferred embodiments, the support material comprises a molecular sieve such as a zeolite. Zeolite support materials, for example, due to a porous structure, tend to be more inclined to the migration of PGM atoms / cations, particularly palladium. Migration can be, for example, from the substrate surface to the substrate, which can lead to the deactivation of the catalyst product. Therefore, it is beneficial to reduce the possibility of migration, because this means that a higher concentration of PGM can be retained on the substrate surface or close to the substrate surface after aging, thereby maintaining the desired catalytic activity level for a longer time. Therefore, the method of the present invention can also be particularly beneficial to zeolite support materials. This is because, in part, due to the increased electrostatic attraction between the anion complex and the support material, the method of the present invention can reduce the possibility of the above-mentioned PGM migration. In an aqueous solution of low pH, for example, a zeolite support material can also obtain a positive charge, and any functional group such as a carboxyl and / or hydroxyl functional group can also interact with the zeolite framework, which can then reduce the possibility of PGM migration.
[0055] The support material is preferably in the form of a powder having a D90 of from 0.1 to 25 μm, preferably from 0.5 to 20 μm, more preferably from 1 to 15 μm, as measured, for example, by TEM.
[0056] Providing the anionic complex preferably comprises: providing a PGM hydroxide and / or a water-insoluble PGM salt, preferably a PGM acetate; contacting the PGM hydroxide and / or the water-insoluble PGM salt with an aqueous solution of carboxylic acid; and optionally recovering the anionic complex in the form of an aqueous solution containing the anionic complex. In other words, the anionic complex can be provided in situ in the method of the present invention, or alternatively the anionic complex can be manufactured at another time and stored before being used in the present invention, for example as a preformed precursor. As used herein, the term "water-insoluble PGM salt" includes PGM salts that are substantially non-dissociated in water, for example, less than 5wt%, 3wt% or 1wt% of the PGM salt is dissociated in water, and / or PGM salts with very low solubility in water, for example less than 10mg / L. When using, for example, PGM acetate, any remaining acetic acid or acetate ions can remain in solution. Without wishing to be bound by theory, it is believed that such substances retained in solution have no adverse effect on the effect of the method of the present invention. Preferably, the pH of the aqueous solution containing the anionic complex is 8 or less, more preferably 7 or less. Preferably, the counter ion of the anionic complex is H + and / or H3O + Preferably, the PGM of the PGM hydroxide is rhodium and / or platinum, and / or the PGM of the water-insoluble PGM salt, preferably the PGM acetate, is palladium. Such combinations have been found to be particularly suitable for use in the present invention.
[0057] Applying the anionic complex to the support material preferably comprises contacting the support material with an aqueous solution comprising the anionic complex, preferably wherein contacting the support material with the aqueous solution is performed at a pH of 8 or less, more preferably 7 or less.
[0058] The supported support material is preferably placed on the substrate in the form of a slurry, preferably wherein the pH of the slurry is 8 or less, more preferably 7 or less. The slurry is particularly effective for placing the material on the substrate, especially for maximizing gas diffusion and minimizing pressure drop during catalytic conversion. The slurry is preferably prepared by a method comprising: applying the anion complex to the support material according to the above method; and optionally adding one or more of the following to the aqueous solution: an oxygen storage material, preferably ceria-zirconia; a promoter salt; a binder; an acid or base; a thickener; and a reducing agent.
[0059] Such a "one-pot" preparation method would be simplified and low-cost compared to conventional methods. It can also maximize the utilization of the anionic complex.
[0060] In other words, the steps of providing an anionic complex comprising a PGM and a carboxylate ion; providing a support material; applying the anionic complex to the support material to form a supported support material; and placing the supported support material on a substrate may include:
[0061] providing a PGM hydroxide and / or a water-insoluble PGM salt, preferably a PGM acetate;
[0062] contacting a PGM hydroxide and / or a water-insoluble PGM salt with an aqueous carboxylic acid solution; and
[0063] optionally recovering the anionic complex as an aqueous solution comprising the anionic complex;
[0064] contacting the support material with an aqueous solution comprising an anionic complex to form a slurry, preferably wherein contacting the support material with the aqueous solution is performed at a pH of 8 or less, more preferably 7 or less;
[0065] optionally adding to the aqueous solution one or more of: an oxygen storage material, preferably ceria-zirconia; a promoter salt; a binder; an acid or base; a thickener; and a reducing agent; and
[0066] The slurry is placed on a substrate.
[0067] Supporting may include washcoating. Conventional washcoating techniques are known in the art.
[0068] Preferably, each step of applying the anionic complex to the support material, placing the supported support material on a substrate, and heating the supported support material is carried out at a pH of 8 or less, preferably 7 or less. For the avoidance of doubt, for all process steps in which the anionic complex has not yet decomposed, it is preferred that the process steps be carried out at a pH of 8 or less, preferably 7 or less for the reasons described herein.
[0069] The slurry preferably has a solids content of 10 to 40%, preferably 15 to 35%. Such a solids content will give the slurry a rheological property suitable for placing a supported support material on a substrate. For example, if the substrate is a honeycomb monolith, such a solids content will cause a thin washcoat to be deposited onto the interior walls of the substrate. If the substrate is a wall flow filter, such a solids content will cause the slurry to enter the channels of the wall flow filter and will cause the slurry to enter the walls of the wall flow filter.
[0070] Preferably, the slurry further comprises one or more of the following:
[0071] Oxygen storage material, preferably ceria-zirconia;
[0072] Accelerator salts;
[0073] Binder;
[0074] Acid or base;
[0075] Thickeners; and
[0076] reducing agent.
[0077] The promoter may include, for example, non-PGM transition metal elements, rare earth elements, alkali metal group elements, and / or a combination of two or more of the above elements in the same or different groups of the periodic table. The promoter salt may be a salt of these elements.
[0078] The binder may comprise, for example, an oxide material having a small particle size to bind together the individual insoluble particles in the washcoat slurry. The use of binders in washcoats is well known in the art.
[0079] Thickeners can include, for example, natural polymers with hydroxyl functional groups that interact with insoluble particles in the carrier coating slurry. Its role is to thicken the carrier coating slurry for improving the coating profile during the carrier coating application on the substrate. It is usually burned off during the carrier coating calcination process. Examples of specific thickeners / rheology modifiers for carrier coatings include galactomannan gum, guar gum, xanthan gum, curdlanschizophyllan, scleroglucan, diutan gum, Whelan gum, hydroxymethylcellulose, carboxymethylcellulose, hydroxyethylcellulose, methylcellulose, methylhydroxyethylcellulose, methylhydroxypropylcellulose and ethylhydroxycellulose.
[0080] As used herein, the term "reducing agent" may include a compound capable of reducing a PGM cation to its metallic state in situ during the washcoat preparation process.
[0081] Additional organic acids may be added which act as a reducing agent for the PGM and / or create a reducing environment during the subsequent heating / calcining step. However, as described above, it is preferred that additional organic acids are not added, as this may be unnecessary due to the auto-reducing properties of the anionic complex. Examples of suitable organic acids may include citric acid, succinic acid, oxalic acid, ascorbic acid, acetic acid, formic acid, tannic acid, and combinations thereof.
[0082] The method preferably further comprises placing an additional slurry on the substrate, the additional slurry comprising one or more of the following: an additional support material; an oxygen storage material; a promoter salt; a binder; an acid or a base; a thickener; and a reducing agent, wherein placing the additional slurry on the substrate is performed before placing the supported support material on the substrate and / or after heating the supported support material to form PGM nanoparticles on the support material. In other words, the additional slurry can form an additional catalyst layer or catalytic zone on the substrate, thereby forming a catalyst product having multiple layers and / or zones of a support coating, for example. Due to the advantageous properties of the anionic complexes described herein, during such a method, the supported PGMs will be more likely to remain in their target layers and / or zones.
[0083] Optionally, the method preferably further comprises placing an additional slurry on the substrate, the additional slurry comprising one or more of the following: an additional anion complex comprising PGM and carboxylate ions; an additional support material; an oxygen storage material; a promoter salt; a binder; an acid or a base; a thickener; and a reducing agent, wherein placing the additional slurry on the substrate is performed after placing the supported support material on the substrate and before heating the supported support material to form PGM nanoparticles on the support material. In other words, in the method of the present invention, the need for an additional calcination step between applying each support coating layer can be eliminated.
[0084] Placing the supported support material on the substrate preferably comprises contacting the slurry with the substrate (e.g., pouring the slurry into an inlet of the substrate) and optionally:
[0085] applying a vacuum to the substrate, and / or
[0086] The slurry on the substrate is dried.
[0087] This results in an advantageous distribution of the supported support material on the substrate.
[0088] Drying preferably occurs under the following conditions:
[0089] A temperature of 60°C to 200°C, more preferably 70°C to 130°C; and / or
[0090] The process is performed for 10-360 minutes, preferably 15-60 minutes.
[0091] The substrate may be "blank", i.e., a substrate that is not washcoated. Alternatively, the substrate may have one or more washcoats already supported. In such a case, the final catalyst article may contain multiple layers of different washcoats.
[0092] The substrate preferably comprises cordierite.Cordierite substrates are particularly suitable for use in catalyst articles.
[0093] The substrate is preferably in the form of a honeycomb monolith, a wall flow filter or a flow-through filter.
[0094] Heating is preferably carried out under the following conditions:
[0095] 400°C-700°C, preferably 400°C-600°C, more preferably 450°C-600°C; and / or
[0096] The process is carried out for 10-360 minutes, preferably 35-120 minutes.
[0097] Lower temperatures and / or shorter heating times may result in insufficient decomposition of the anion complex and / or may result in a high level of carboxylate ion ligands remaining in the matrix. Higher temperatures and / or longer heating times may result in PGM particles having an undesirably large particle size, presumably due to sintering. Higher temperatures and longer heating times may also result in damage to the catalyst article.
[0098] The heating preferably comprises calcining. As used herein, the term "calcining" may include a heat treatment process in the absence or limited supply of air or oxygen to cause thermal decomposition.
[0099] The nanoparticles preferably have a D50 of 0.1 nm to 25 nm, preferably 0.2 to 10 nm, more preferably 0.2 to 5 nm. The D50 can be measured by TEM. Such a particle size will result in a favorable level of catalytic activity and will be less prone to agglomeration and sintering after aging, i.e. after use in an exhaust system.
[0100] In another aspect, the present invention provides a catalyst article that can be obtained by the method described herein, which is used in an emission treatment system. Compared with conventional catalyst articles, for example, PGMs are less likely to experience migration between any catalyst layers and / or zones, which is believed to be at least partially due to the stronger and more reliable fixation of PGMs to the support material. Therefore, each layer and / or zone of the catalyst article can be maintained at a desired activity level for a longer period of time. Obvious wicking will also be less likely.
[0101] The catalyst product is preferably used for three-way catalysis.
[0102] The catalyst article is preferably used for diesel oxidation catalysis.
[0103] The catalyst preparation is preferably used for NO x Trap catalysis.
[0104] The catalyst article may have a washcoat loading of 0.5 g / in 3 Up to 8g / in 3 , or 1g / in 3 Up to 3g / in 3 Such catalyst preparations can exhibit similar or higher catalytic activity than conventional catalyst preparations, but can reduce costs due to the lower amount of PGM used.
[0105] The substrate preferably comprises a wall flow filter substrate or a flow-through substrate.
[0106] In a preferred embodiment, the catalyst article comprises a first catalytic region comprising a first PGM component, and optionally further comprises a second catalytic region comprising a second PGM component. Preferably, the first catalytic region is directly loaded / deposited on the substrate. Preferably, the second catalytic region is directly loaded / deposited on the substrate. Preferably, the first and / or second PGM components are selected from platinum, palladium, rhodium and mixtures of two or more thereof. Preferably, the first PGM component and the second PGM component are different. Preferably, for example, the first PGM component is palladium, and the second PGM component is rhodium.
[0107] The catalyst preparation preferably contains 0.1 g / ft 3 Up to 50g / ft 3 Rhodium, more preferably 0.5 g / ft 3 Up to 25g / ft 3 of rhodium, even more preferably 1 g / ft 3 Up to 20g / ft 3 of rhodium, for example 2g / ft 3 Up to 15g / ft 3 of rhodium.
[0108] The catalyst article preferably comprises 1 g / ft 3 Up to 300g / ft 3 of platinum, more preferably 2 g / ft 3 Up to 200g / ft 3 of platinum, even more preferably 5 g / ft 3 Up to 150g / ft 3 of platinum, for example 10 g / ft 3 Up to 100g / ft 3 of platinum.
[0109] The catalyst product preferably contains 1 g / ft 3 Up to 300g / ft 3 of palladium, more preferably 2 g / ft 3 Up to 200g / ft 3 of palladium, even more preferably 5 g / ft 3 Up to 150g / ft 3 of palladium, for example 10 g / ft 3 Up to 100g / ft 3 of palladium.
[0110] In another aspect, the present invention provides an emission treatment system comprising the catalyst article described herein.
[0111] In some embodiments, the emission treatment system can be used in an internal combustion engine. The emission treatment system is preferably used in a gasoline engine.
[0112] Gasoline engines are preferably operated under stoichiometric conditions.
[0113] In another aspect, the present invention provides a method for treating exhaust gas, the method comprising:
[0114] providing a catalyst article as described herein; and
[0115] The catalyst article is contacted with the exhaust gas.
[0116] In some embodiments, the emission treatment system can be used for an internal combustion engine. The exhaust gas is preferably the exhaust gas from a gasoline engine. The catalyst article is particularly suitable for treating such exhaust gas. The gasoline engine is preferably operated under stoichiometric conditions.
[0117] definition
[0118] As used herein, the term "region" refers to an area on a substrate that is typically obtained from drying and / or calcining of a washcoat. A "region" may be located or supported on a substrate, for example, as a "layer" or "zone". The area or arrangement on the substrate is usually controlled during the process of applying the washcoat to the substrate. A "region" typically has a clear boundary or edge (i.e., one region can be distinguished from another region using conventional analytical techniques).
[0119] Typically, a "region" has a substantially uniform length. In the present context, reference to a "substantially uniform length" refers to a length that deviates from its average value (e.g., the difference between the maximum length and the minimum length) by no more than 10%, preferably by no more than 5%, and more preferably by no more than 1%.
[0120] It is preferred that each "region" has a substantially uniform composition (i.e., there is no significant difference in the composition of the washcoat when one portion of the region is compared to another portion of the region). In this context, substantially uniform composition refers to a material (e.g., a region) wherein the difference in composition when one portion of the region is compared to another portion of the region is 5% or less, typically 2.5% or less, and most typically 1% or less.
[0121] The term "washcoat" is art-recognized and refers to an adherent coating that is typically applied to a substrate during the catalyst production process.
[0122] As used herein, the term "mixed oxide" generally refers to a mixture of oxides of a single phase, as known in the art. As used herein, the term "composite oxide" generally refers to a composition of oxides having more than one phase, as known in the art.
[0123] As used herein, the expression "consisting essentially of defines the scope of a feature to include the specified materials or steps, and any other materials or steps that do not materially affect the basic characteristics of the feature, such as minor impurities. The expression "consisting essentially of" encompasses the expression "consisting of."
[0124] "Slurry" means a liquid containing insoluble matter, such as insoluble particles.
[0125] As used herein, any reference to the amount of dopant, particularly the total amount (expressed as wt %), refers to the weight of the support material or refractory metal oxide thereof.
[0126] As used herein, the term "loading" refers to the weight of the metal in g / ft. 3 The measured value.
[0127] When the specification refers to "a" or "an", this includes both the singular and the plural.
[0128] The invention will now be described with reference to the following non-limiting examples and embodiments.
[0129] Example
[0130] Preparation of anionic complex precursors
[0131] Various anion complex precursors were prepared according to the following examples:
[0132] Example 1: Pd citrate
[0133] Solid Pd acetate (6.33 g) was charged into a round bottom flask and 1.1 equivalents of citric acid (6.51 g) dissolved in 50 ml of water was added. The mixture was heated at 75 °C for 6 h until completely dissolved. This formed a deep red solution. The solution was filtered using 542 filter paper to remove any remaining solid impurities. The UV / VIS spectrum showed a peak at 388 nm. ICP (inductively coupled plasma analysis) produced a Pd analysis of 5.73 wt % Pd.
[0134] Example 2: Rh(III) Citric Acid
[0135] RhCl3 solution (46.46 g, 21.52% Rh) was diluted with water (150 mL) and K2CO3 (5 M solution) was added dropwise until the pH of the solution increased from 1.29 to 2.5 over a period of 15 minutes (to neutralize the free HCl present). Additional 5M K2CO3 solution was added dropwise until the pH reached 7.5. The mixture was heated at 40°C. At this stage, the solution turned red. Additional K2CO3 solution was added to raise the pH to 10.8 and then heated at 100°C for 2 hours, during which time a yellow-brown precipitate was formed. The solid was filtered and washed with deionized water until the conductivity reached 60 mS. The hydroxide was mixed with citric acid (40.84 g) and heated at 100°C, during which time the hydroxide dissolved in less than 4 h. ICP gave an Rh analysis of 6.52 wt% Rh and a Cl analysis of 20 ppm Cl.
[0136] Example 3: Rh(III) citrate (alternative method)
[0137] RhCl3 solution (106.27 g, 19.29% Rh) was diluted with water (300 mL). NaOH (5 M solution) was added dropwise until the pH of the solution increased from 1.29 to 2.5 over a period of 15 minutes (to neutralize the free HCl present). 5 M NaOH solution was continued to be added dropwise until the pH reached 7.5. The mixture was heated at 40°C to produce a hazy red solution. NaOH solution was continued to be added until the pH reached 10 and stirred for 4 h while the temperature was maintained at 40°C during which time a Rh(OH)3 precipitate was formed. After cooling, the precipitate was filtered and washed with deionized H2O until the conductivity of the solution reached 70 mS. A solution of citric acid (83.72 g) in water (400 ml) was prepared. The Rh(OH)3 precipitate was added thereto and the mixture was stirred and heated at 100°C. The hydroxide dissolved within 3 hours. The solution was filtered on a 542 filter and concentrated by evaporation to a concentration of about 8% Rh. ICP gave an Rh analysis of 8.01% Rh.
[0138] Catalyst product manufacturing and testing
[0139] Various catalyst preparations were prepared according to the following examples:
[0140] Example 4: Comparison of Pd absorption relative to conventional methods
[0141] Table 1 compares the Pd absorption values on alumina supported CeZrO2 mixed oxide (ACZ, composition Al2O3:CeO2:ZrO2=64:21:15) using palladium citrate or palladium nitrate as Pd precursor. The experiments were conducted by adding the Pd precursor to a slurry of the ACZ support, targeting a Pd loading of 2.3 wt%. After mixing for 90 minutes, the mixture was centrifuged and the supernatant was analyzed for Pd content. The Pd absorption value was calculated by the percentage of Pd adsorbed on the surface of the ACZ support. The results show that Pd citrate produced 90% Pd adsorption on the ACZ support, compared to 60% Pd absorption when Pd nitrate was used.
[0142] Table 1
[0143] Pd Precursor Absorption value (% adsorbed Pd) Pd Nitrate 60% Pd Citrate 90%
[0144] Example 5: Comparison of the performance of the catalyst products of the present invention relative to conventional PGM precursors Comparative Catalyst A :
[0145] A single layer PdRh TWC was prepared with only one catalytic region. The catalytic region consisted of both Pd and Rh, mixed in a slurry, supported on a washcoat of CeZr mixed oxide, ceria-zirconium-alumina and alumina sol as binders. Pd nitrate solution was used as the Pd source during the washcoat slurry preparation. The total washcoat loading of the catalytic region was about 3.5 g / in 3 , where the Pd loading is 48 g / ft 3 and Rh loading is 2g / ft 3 .
[0146] This washcoat was then applied from each side of a ceramic substrate (400 cpsi, 6 mil wall thickness, 4.16 inch diameter and 4 inch length) using a conventional coating procedure with a coating depth target of 50% of the substrate length for each coat, dried at 100°C, and calcined at 500°C for 45 min.
[0147] Catalyst B :
[0148] Catalyst B was prepared according to a similar procedure as Comparative Catalyst A, except that a Pd citrate solution was used as the Pd source during the washcoat slurry preparation for the catalytic zone. Both Comparative Catalyst A and Catalyst B had the same composition, but used different palladium precursors.
[0149] Catalyst B and Comparative Catalyst A were bench aged for 100 hours and the average temperature of the close-coupled block was 875°C. Vehicle emissions were tested under the Federal Test Procedure (FTP) on a commercial vehicle equipped with a 3.5L GTDI engine and a turbocharger, and the catalyst block was placed in an underfloor position, paired with a conventional close-coupled (CC) catalyst block. The NOx of the entire system under the FTP test cycle was x The / NMHC / CO emissions are summarized in Table 2. The system with Pd citrate showed a significant improvement in (NO x +NMHC) and an additional emissions reduction of 5 mg / mile for CO.
[0150] Table 2
[0151] catalyst <![CDATA[NO x (mg / mile)]]> NMHC (mg / mile) CO(mg / mile) Comparative Catalyst A 29 18 469 Catalyst B 25 17 404
[0152] Example 6: Comparison of the performance of the catalyst products of the present invention relative to conventional PGM precursors when using a zeolite support material
[0153] Comparative Catalysts C and D (having the same components except for the use of different Pd precursors) were prepared using the same washcoat slurry as Catalysts A and B and coated on a monolithic extruded zeolite substrate (4.16" x 4", 400 / 11, 55% beta zeolite). The 11 / 16" x 1" cores were aged on a laboratory shaker for 50 hours with 4-mode cycles at temperatures of 740°C to 840°C. The Pd distribution on the aged cores was characterized by EPMA (Electron Probe Microanalysis) method. Figure 1 The core prepared by Pd citrate Figure 2 The Pd nitrate has a relatively low Pd concentration compared to that in the substrate, demonstrating a lesser degree of Pd migration.
[0154] The full-size catalyst was placed in the baseplate position in the system and each system was aged for 100 hours with an average temperature of 875°C for the close-fit block. The aged baseplate catalyst was then paired with a conventional close-fit catalyst (0:78:2) to form a new system and tested on a Ford Flex equipped with a 3.5L GTDI engine and turbocharger. The NOx of the entire system under the FTP test cycle was x The / NMHC / CO emissions are summarized in Table 3. The system with Pd citrate showed a significant improvement in (NO x +NMHC) and an additional emissions reduction of 4 mg / mile for CO.
[0155] The results clearly show that the use of Pd citrate can minimize Pd migration to the zeolite substrate, which results in a catalyst with improved performance.
[0156] Table 3: System NO on 3.5L vehicle FTP test cycle x / NMHC / CO emissions (commonly used CC / 0:78:2+different UB / 0:48:2)
[0157]
[0158] Example 7: Light-off performance and OSC test in synthetic catalyst activity test
[0159] Comparative Catalyst E :
[0160] First catalytic zone:
[0161] The first catalytic zone consisted of Pd supported on a washcoat of CeZr mixed oxide, La stabilized alumina and Ba promoter, using Pd nitrate solution as the Pd source during washcoat slurry preparation. The washcoat loading of the first catalytic zone was about 1.8 g / in 3 , where the Pd loading is 24 g / ft 3 .
[0162] This washcoat was then applied from the inlet face of a ceramic substrate (400 cpsi, 4.3 mil wall thickness, 4.66 inch diameter and 4.5 inch length) using conventional coating procedures with a coating depth goal of 80% of the substrate length, dried at 100°C.
[0163] Second catalytic zone:
[0164] The second catalytic zone consisted of Rh supported on a washcoat of CeZr mixed oxide and La stabilized alumina. The washcoat loading of the second catalytic zone was about 1.3 g / in 3 , where the Rh loading is 4g / ft 3 .
[0165] The second washcoat was then applied from above using conventional coating procedures from the outlet face of the ceramic substrate containing the first catalytic zone, with a coating depth target of 80% of the substrate length, dried at 100°C, and calcined at 500°C for 45 min.
[0166] Catalyst F :
[0167] Catalyst F was prepared according to a procedure similar to Comparative Catalyst E, except that in the first catalytic zone, a Pd citrate solution was applied as a Pd source during washcoat slurry preparation.
[0168] Catalyst F and comparative catalyst E were tested on a synthetic catalyst activity test (SCAT) apparatus. At a gas flow rate of 10 vol% H2O + 14 vol% CO2 + 333 ppm C3H6 + 167 ppm C3H8 + 1.5 vol% CO + 0.5 vol% H2O + 1.15 vol% O2 + 1000 ppm NO and the balance N2 (space velocity is 60000 h -1 ), and the ignition performance was tested at a heating rate of 30°C / min. THC, CO and NO were calculated by comparing the concentrations of the feed gas and the gas at the catalyst outlet. x The conversion rate is 10 vol% H2O + 14 vol% CO2 + 333 ppm C3H6 + 167 ppm C3H8 + 0.5 vol% CO + 0.5 vol% H2O + 0.5 vol% O2 + 1000 ppm NO and the balance N2 gas flow rate (space velocity is 60000 h -1 ) OSC was tested at 450° C. Comparative Catalyst E and Catalyst F were hydrothermally aged at 980° C. for 4 hours at a flow rate of 5 L / min of 2 vol% O2+10 vol% H2O and balance N2.
[0169] Table 4 shows the HC, CO and NO of aged catalyst F and comparative catalyst E. x T 50 The data show that, surprisingly, the inventive catalyst F produces significantly improved light-off performance compared to the comparative catalyst E for CO, HC and NO. x With lower T values of about 23°C, 22.5°C and 17.5°C respectively 50 (T 50 is the temperature when the conversion reaches 50%). Meanwhile, the OSC of Catalyst F is about 30% higher than that of Comparative Catalyst E.
[0170] Table 4: SCAT ignition and OSC test results
[0171]
[0172] Example 8: Vehicle Testing Procedure and Results
[0173] Catalyst F and Comparative Catalyst E were bench aged for 100 hours using four aging cycle patterns with a peak temperature of 980°C. Vehicle emissions were conducted under the World Light Vehicle Test Procedure (WLTP) on a commercial vehicle equipped with a 1.6L turbo with the block placed in the close-coupled position. Emissions were measured before and after the catalyst. Table 5 shows the dilute bag emissions data from the vehicle tailpipe.
[0174] Table 5: Vehicle exhaust emission results on WLTP
[0175]
[0176] Table 5 shows the bag data from the tailpipe of Test Vehicle A. Catalyst F of the present invention has significantly reduced THC, NMHC, CO and NO compared to Comparative Catalyst E. x emissions (reduced by 19%, 20%, 29% and 17% respectively).
[0177] Embodiment 1. A method of making a catalyst article, the method comprising:
[0178] providing an anionic complex comprising a PGM and a carboxylate ion;
[0179] providing carrier materials;
[0180] applying the anionic complex to the support material to form a supported support material;
[0181] placing the supported support material on a substrate; and
[0182] The loaded support material is heated to form PGM nanoparticles on the support material.
[0183] Embodiment 2. The method according to embodiment 1, wherein the carboxylate ion comprises two or more carboxyl functional groups.
[0184] Embodiment 3. The method according to embodiment 1 or 2, wherein the carboxylate ion comprises 2-6 carbon atoms.
[0185] Embodiment 4. The method according to any of the preceding embodiments, wherein the carboxylate ion comprises a hydroxyl group, preferably an α-hydroxy acid functional group.
[0186] Embodiment 5. A method according to any one of embodiments 1-3, wherein the carboxylate ion comprises one or more of citrate, malate, malonate, succinate, tartrate, glutarate, tartronate, oxalate, lactate and glycolate.
[0187] Embodiment 6. The method according to any of the preceding embodiments, wherein the carboxylate ions comprise citrate and / or malonate.
[0188] Embodiment 7. A method according to any of the preceding embodiments, wherein the PGM is selected from one or more of rhodium, palladium, platinum and ruthenium.
[0189] Embodiment 8. The method according to embodiment 7, wherein the PGM comprises rhodium, palladium, platinum or a combination thereof, preferably rhodium and / or palladium.
[0190] Embodiment 9. A method according to any of the preceding embodiments, wherein the anion complex comprises one or more of the following: Pt(IV) malonate, Pt(IV) succinate, Pt(II, IV) oxalate, Pd(II) citrate, Pd(II) lactate, Pd(II) oxalate, Pd(II) glycolate, Pd(II) malate, Rh(II) citrate, Rh(III) citrate, Rh(II) lactate, Rh(III) lactate and Ru(III) oxalate.
[0191] Embodiment 10. A method according to any one of the preceding embodiments, wherein the anion complex is provided in the form of an aqueous solution comprising the anion complex, preferably wherein the pH of the aqueous solution is 8 or less, more preferably 7 or less.
[0192] Embodiment 11. The method of embodiment 10, wherein the aqueous solution does not contain PGM nitrates.
[0193] Embodiment 12. The method according to embodiment 10 or 11, wherein the anionic complex has a counterion comprising H + , H3O + and NH4 + One or more of, preferably H + and / or H3O + composition.
[0194] Embodiment 13. The method of any one of Embodiments 10-12, wherein the aqueous solution does not contain elemental inorganic cations.
[0195] Embodiment 14. The method according to any one of the preceding embodiments, wherein the anion complex comprises a compound selected from water, OH - , acetate ion and one or more additional ligands bridging the O atom.
[0196] Embodiment 15. The method according to any of the preceding embodiments, wherein the anionic complex comprises more than one PGM center.
[0197] Embodiment 16. A method according to any of the preceding embodiments, wherein the support material comprises an oxide, preferably one or more of Al2O3, SiO2, TiO2, CeO2, ZrO2, CeO2-ZrO2, V2O5, La2O3 and zeolite.
[0198] Embodiment 17. The method according to any of the preceding embodiments, wherein the support material comprises alumina, preferably gamma-alumina.
[0199] Embodiment 18. The method of any of the preceding embodiments, wherein the support material comprises ceria-zirconia.
[0200] Embodiment 19. The method of any of the preceding embodiments, wherein the support material comprises alumina and ceria-zirconia.
[0201] Embodiment 20. The method of any one of Embodiments 17-19, wherein the alumina and / or ceria-zirconia is doped.
[0202] Embodiment 21. A method according to Embodiment 19, wherein the alumina and / or ceria-zirconia is doped with oxides of one or more of lanthanum, neodymium, yttrium, niobium, praseodymium, hafnium, molybdenum, titanium, vanadium, zinc, cadmium, manganese, iron, copper, calcium, barium, strontium, cesium, magnesium, potassium and sodium, preferably one or more of lanthanum, neodymium, praseodymium and yttrium.
[0203] Embodiment 22. A method according to Embodiment 20 or 21, wherein the dopant is present in the alumina and / or ceria-zirconia in an amount of 0.001 wt % to 20 wt %, preferably 0.5 wt % to 10 wt %.
[0204] Embodiment 23. The method of any preceding embodiment, wherein the support material comprises a zeolite.
[0205] Embodiment 24. The method according to any one of the preceding embodiments, wherein the support material is in the form of a powder having a D90 of 0.1 to 25 μm, preferably 0.5 to 20 μm, more preferably 1-15 μm.
[0206] Embodiment 25. The method according to any one of the preceding embodiments, wherein providing the anion complex comprises:
[0207] providing a PGM hydroxide and / or a water-insoluble PGM salt, preferably a PGM acetate;
[0208] contacting the PGM hydroxide and / or water-insoluble PGM salt with an aqueous solution of a carboxylic acid; and
[0209] The anionic complex is optionally recovered in the form of an aqueous solution comprising the anionic complex.
[0210] Embodiment 26. A method according to embodiment 25, wherein the PGM of the PGM hydroxide is rhodium and / or platinum, and / or the PGM of the water-insoluble PGM salt, preferably the PGM acetate, is palladium.
[0211] Embodiment 27. A method according to any one of the preceding embodiments, wherein applying the anionic complex to the carrier material comprises contacting the carrier material with an aqueous solution comprising the anionic complex, preferably wherein contacting the carrier material with the aqueous solution is carried out at a pH of 8 or less, more preferably 7 or less.
[0212] Embodiment 28. A method according to any one of the preceding embodiments, wherein the supported support material is placed on the substrate in the form of a slurry, preferably wherein the pH of the slurry is 8 or less, more preferably 7 or less.
[0213] Embodiment 29. The method of embodiment 28, wherein the slurry is prepared by a method comprising:
[0214] applying the anionic complex to a carrier according to the method of embodiment 27; and
[0215] Optionally, one or more of the following is added to the aqueous solution: an oxygen storage material, preferably ceria-zirconia; a promoter salt; a binder; an acid or a base; a thickener; and a reducing agent.
[0216] Embodiment 30. The method according to any of the preceding embodiments, wherein the loading comprises a support coating.
[0217] Embodiment 31. A method according to any of the preceding embodiments, wherein each step of applying the anionic complex to a support material, placing the supported support material on a substrate, and heating the supported support material is performed at a pH of 8 or less, preferably 7 or less.
[0218] Embodiment 32. The method according to any one of embodiments 28-31, wherein the solid content of the slurry is 10-40%, preferably 15-35%.
[0219] Embodiment 33. The method of any one of embodiments 28-32, wherein the slurry further comprises one or more of the following:
[0220] Oxygen storage material, preferably ceria-zirconia;
[0221] Accelerator salts;
[0222] Binder;
[0223] Acid or base;
[0224] Thickeners; and
[0225] reducing agent.
[0226] Embodiment 34. A method according to any one of Embodiments 28-33, further comprising placing an additional slurry on the substrate, the additional slurry comprising one or more of the following: additional support material; oxygen storage material; promoter salt; binder; acid or base; thickener; and reducing agent, wherein placing the additional slurry on the substrate is performed before placing the supported support material on the substrate and / or after heating the supported support material to form PGM nanoparticles on the support material.
[0227] Embodiment 35. A method according to any one of Embodiments 28-33, further comprising placing an additional slurry on the substrate, the additional slurry comprising one or more of the following: an additional anion complex comprising PGM and carboxylate ions; an additional support material; an oxygen storage material; a promoter salt; a binder; an acid or a base; a thickener; and a reducing agent, wherein placing the additional slurry on the substrate is performed after placing the supported support material on the substrate and before heating the supported support material to form PGM nanoparticles on the support material.
[0228] Embodiment 36. The method of any one of Embodiments 28-35, wherein placing the supported support material on a substrate comprises contacting the slurry with the substrate, and optionally:
[0229] applying a vacuum to the substrate, and / or
[0230] The slurry on the substrate is dried.
[0231] Embodiment 37. The method according to embodiment 36, wherein the drying is carried out under the following conditions:
[0232] 60°C to 200°C, preferably 70°C to 130°C; and / or
[0233] The process is performed for 10-360 minutes, preferably 15-60 minutes.
[0234] Embodiment 38. A method according to any of the preceding embodiments, wherein the substrate comprises cordierite.
[0235] Embodiment 39. A method according to any of the preceding embodiments, wherein the substrate is in the form of a honeycomb monolith, a wall flow filter, or a flow-through filter.
[0236] Embodiment 40. The method according to any one of the preceding embodiments, wherein the heating is carried out under the following conditions:
[0237] 400°C-700°C, preferably 400°C-600°C, more preferably 450°C-600°C; and / or
[0238] The process is carried out for 10-360 minutes, preferably 35-120 minutes.
[0239] Embodiment 41. A method according to any of the preceding embodiments, wherein the heating comprises calcining.
[0240] Embodiment 42. A method according to any of the preceding embodiments, wherein the D50 of the nanoparticles is 0.1 nm to 25 nm, preferably 0.2 to 10 nm, more preferably 0.2 to 5 nm.
[0241] Embodiment 43. A catalyst product obtainable by the method of any one of the preceding embodiments, wherein the catalyst product is used in an emission treatment system.
[0242] Embodiment 44. The catalyst product according to Embodiment 43 is used for three-way catalysis.
[0243] Embodiment 45. The catalyst article according to Embodiment 43 is used for diesel oxidation catalysis.
[0244] Embodiment 46. The catalyst product according to embodiment 43 is used for NO x Trap catalysis.
[0245] Embodiment 47. The catalyst article according to any one of Embodiments 43-46, wherein the washcoat loading is 0.5 g / in 3 Up to 8g / in 3 .
[0246] Embodiment 48. The catalyst article of any one of Embodiments 43-47, wherein the substrate comprises a wall flow filter substrate.
[0247] Embodiment 49. The catalyst article of any one of Embodiments 43-47, wherein the substrate comprises a wall flow substrate.
[0248] Embodiment 50. The catalyst article of any of Embodiments 43-49, wherein the catalyst article comprises a first catalytic region comprising a first PGM component, and optionally further comprises a second catalytic region comprising a second PGM component.
[0249] Embodiment 51. A catalytic article according to Embodiment 50, wherein the first catalytic region is directly supported / deposited on the substrate.
[0250] Embodiment 52. The catalytic article of Embodiment 50, wherein the second catalytic region is directly supported / deposited on the substrate.
[0251] Embodiment 53. The catalytic article of any one of Embodiments 50-52, wherein the first and / or second PGM components are selected from platinum, palladium, rhodium, and mixtures of two or more thereof.
[0252] Embodiment 54. The catalytic article of Embodiment 53, wherein the first PGM component and the second PGM component are different.
[0253] Embodiment 55. The catalytic article of Embodiment 54, wherein the first PGM component is palladium and the second PGM component is rhodium.
[0254] Embodiment 56. The catalyst article of any one of Embodiments 43-55, comprising 0.1 g / ft 3 Up to 50g / ft 3 Rhodium, preferably 0.5 g / ft 3 Up to 25g / ft 3 of rhodium.
[0255] Embodiment 57. The catalyst article of any one of Embodiments 43-56 comprises 1 g / ft 3 Up to 300g / ft 3 Palladium, preferably 10 g / ft 3 Up to 100g / ft 3 of palladium.
[0256] Embodiment 58. The catalyst article of any one of Embodiments 43-57, comprising 1 g / ft 3 Up to 300g / ft 3 Palladium, preferably 10 g / ft 3 Up to 100g / ft 3 of platinum.
[0257] Embodiment 59. An emission treatment system comprising the catalyst article according to any one of Embodiments 43-58.
[0258] Embodiment 60. An emission treatment system according to Embodiment 59, which is used in a gasoline engine.
[0259] Embodiment 61. An emission treatment system according to Embodiment 60, wherein the gasoline engine operates under stoichiometric conditions.
[0260] Embodiment 62. A method of treating exhaust gas, the method comprising:
[0261] Providing the catalyst article of any one of embodiments 43-58; and
[0262] The catalyst article is contacted with an exhaust gas.
[0263] Embodiment 63. A method according to Embodiment 62, wherein the exhaust gas comes from a gasoline engine.
[0264] Embodiment 64. A method according to Embodiment 63, wherein the gasoline engine operates under stoichiometric conditions.
[0265] The foregoing detailed description is provided by way of explanation and illustration and is not intended to limit the scope of the appended claims. Many variations of the presently preferred embodiments shown herein will be apparent to those skilled in the art and remain within the scope of the appended claims and their equivalents.
Claims
1. A method for producing a catalyst product, the method comprising: providing an anionic complex comprising a PGM and a carboxylate ion; providing carrier materials; applying the anionic complex to the support material to form a supported support material; placing the loaded carrier material on a substrate; heating the supported support material to form PGM nanoparticles on the support material; and wherein the carboxylate ion comprises two or more carboxyl functional groups and comprises a hydroxyl group.
2. The method of claim 1, wherein the carboxylate ion comprises 2-6 carbon atoms.
3. The method of claim 1, wherein the carboxylate ion comprises an alpha-hydroxy acid functional group.
4. The method of claim 1, wherein the carboxylate ions comprise one or more of citrate, malate, tartrate, tartronate, and lactate. The method of claim 1 , wherein the carboxylate ion comprises citrate.
6. The method of claim 1, wherein the PGM is selected from one or more of rhodium, palladium, platinum and ruthenium.
7. The method of claim 6, wherein the PGM comprises rhodium, palladium, platinum or a combination thereof.
8. The method of claim 6, wherein the PGM comprises rhodium and / or palladium.
9. The method of claim 1, wherein the anionic complex comprises one or more of the following: Pd(II) citrate, Pd(II) lactate, Pd(II) malate, Rh(II) citrate, Rh(III) citrate, Rh(II) lactate, and Rh(III) lactate.
10. The method of claim 1, wherein the anionic complex is provided in the form of an aqueous solution comprising the anionic complex. The method according to claim 10 , wherein the pH of the aqueous solution is 8 or less.
12. The method according to claim 10, wherein the pH of the aqueous solution is 7 or less.
13. The method of any one of claims 10-12, wherein the aqueous solution does not contain PGM nitrates.
14. The method of claim 1, wherein the anionic complex comprises more than one PGM center.
15. The method of claim 1, wherein the support material comprises an oxide.
16. The method of claim 1, wherein the support material comprises one or more of Al2O3, SiO2, TiO2, CeO2, ZrO2, CeO2-ZrO2, V2O5, La2O3 and zeolite.
17. The method of claim 1, wherein providing the anionic complex comprises: providing a PGM hydroxide and / or a water-insoluble PGM salt; contacting the PGM hydroxide and / or water-insoluble PGM salt with an aqueous solution of a carboxylic acid; and The anionic complex is optionally recovered in the form of an aqueous solution comprising the anionic complex.
18. The method of claim 17, wherein the water-insoluble PGM salt is PGM acetate.
19. The method of claim 17, wherein the PGM of the PGM hydroxide is rhodium and / or platinum, and / or the PGM of the water-insoluble PGM salt is palladium.
20. The method of claim 18, wherein the PGM of the PGM acetate is palladium.
21. The method of claim 1, wherein the substrate is in the form of a honeycomb monolith, a wall flow filter, or a flow-through filter.
22. Catalyst article obtainable by the process according to claim 1, said catalyst article being useful in an emission treatment system.
23. The catalyst product according to claim 22, which is used for three-way catalysis, diesel oxidation catalysis or NO x Trap catalysis.
24. The catalyst article of claim 22, wherein the catalyst article comprises a first catalytic region comprising a first PGM component, and optionally further comprises a second catalytic region comprising a second PGM component.
25. An emission treatment system comprising the catalyst article of claim 22.
26. A method for treating waste gas, the method comprising: Providing a catalyst product according to claim 22; and The catalyst article is contacted with an exhaust gas.
Citation Information
Patent Citations
Ammonia slip catalyst having platinum impregnated on high porosity substrates
CN106457216A
Process for removing oxidisable gaseous compounds from a gas mixture by means of a platinum-containing oxidation catalyst
CN107303468A
Diesel oxidation catalyst comprising platinum group metal nanoparticles
CN108778501A
Hydrocarbon trap catalyst
CN112118906A
Three-way conversion catalysts and methods for the preparation therefor
CN1230899A