Zn with core-shell structure 1-x Cu x Preparation methods and applications of O / TiO2 photocatalytic composite materials

By preparing a core-shell structured Zn1-xCuxO/TiO2 composite material, the problem of narrow absorption range of titanium dioxide photocatalytic materials to sunlight was solved, the photocatalytic performance was improved and the preparation process was simplified, making it suitable for the field of photocatalysis.

CN115608367BActive Publication Date: 2026-11-17NORTH CHINA UNIV OF WATER RESOURCES & ELECTRIC POWER +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211229868.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-08
Publication Date
2026-11-17
Estimated Expiration
2042-10-08

AI Technical Summary

Technical Problem

Existing titanium dioxide photocatalytic materials have a narrow absorption range for sunlight, insufficient photocatalytic performance, and a complicated preparation process, making large-scale production difficult.

Method used

A method for preparing Zn1-xCuxO/TiO2 composite materials with a core-shell structure is proposed. This method involves the preparation of ZIF precursor, titanium source pretreatment, and composite material preparation. Combined with chlorine-doped titanium dioxide, a pn heterojunction is formed, which improves the light absorption range and photocatalytic activity.

Benefits of technology

It achieves broad-spectrum absorption of visible light, improves photocatalytic activity, simplifies the preparation process, and facilitates large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115608367B_ABST
    Figure CN115608367B_ABST
Patent Text Reader

Abstract

This invention relates to the field of nanomaterials and discloses a Zn with excellent photocatalytic performance. 1‑x Cu x Preparation and application of O / TiO2 composite materials: This invention utilizes ZIF precursors prepared by mechanochemical method and hydrothermal method using microspheres to synthesize Zn with modified TiO2. 1‑x Cu x O / TiO2 composite material, synthesized Zn 1‑ x Cu x The O / TiO2 composite material exhibits a core-shell structure and good photocatalytic activity. The preparation method described in this invention is simple and controllable, saves energy, and yields products with large specific surface area, good dispersibility, uniform sample morphology, and no agglomeration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nanomaterials, specifically to a Zn with a core-shell structure. 1-x Cu x Preparation method and application of O / TiO2 photocatalytic composite material. Background Technology

[0002] In recent years, the use of semiconductor photocatalysts to produce hydrogen through water splitting has attracted widespread attention because it offers a new approach to solving the global energy crisis and environmental pollution problems. By preparing and using photocatalysts, water can be split to obtain hydrogen, solar energy can be efficiently utilized to acquire and store energy, and no waste that pollutes the environment is generated. Furthermore, photocatalysts can reduce carbon dioxide concentration to mitigate the greenhouse effect, and can also catalytically degrade harmful wastes such as dye waste, organic pollutants, and toxic waste to achieve environmental purification.

[0003] MOFs, as organic-inorganic hybrid materials, also known as coordination polymers, are crystalline porous materials with a periodic network structure formed by the self-assembly of metal ions or metal clusters with organic linkers through coordination bonds. They possess characteristics such as high specific surface area, large pore volume, and easily adjustable pore size. However, single photocatalytic materials exhibit low photocatalytic performance and a relatively small absorption range of the solar spectrum, failing to fully utilize sunlight for photocatalysis. This not only reduces photocatalytic efficiency but also hinders the widespread application of photocatalysis technology. To more fully and effectively utilize sunlight and improve photocatalytic efficiency, scientists have combined compatible materials with single photocatalysts to form photocatalytic composite materials with heterostructures. This not only broadens the absorption range of the solar spectrum for the photocatalytic materials but also creates channels between the two materials, reducing the recombination rate of electrons and holes, thereby improving the activity of the photocatalyst.

[0004] Because of its small particle size and large specific surface area, nano-titanium dioxide has a wide absorption range for sunlight, absorbing most of the light. Therefore, titanium dioxide is widely used in photocatalysis and photoelectric conversion due to its excellent photoelectric properties, strong oxidizing ability, low cost, non-toxicity, and stability against optical and chemical corrosion.

[0005] However, conventional titanium dioxide has a narrow absorption spectrum, resulting in insufficient utilization of solar energy and inadequate photocatalytic performance. It can only be excited by light with a wavelength of less than or equal to 387 nm, meaning it can only absorb and utilize ultraviolet light for excitation. However, ultraviolet light accounts for only 5% of the total solar energy, leaving a large amount of light energy unused. Moreover, ultraviolet light poses radiation hazards. Although some modified titanium dioxide has good photocatalytic performance, its preparation process is relatively complicated, making large-scale production impossible.

[0006] Therefore, there is a need to provide a method for preparing titanium dioxide composite materials that has a simple preparation process and good photocatalytic effect. Summary of the Invention

[0007] The technical problem solved by this invention is to improve the absorption range of titanium dioxide to the solar spectrum by doping modification, thereby enhancing the photocatalytic performance of the material and preparing Zn with good photocatalytic performance. 1-x Cu x O / TiO2 composite material.

[0008] The technical solution of this invention is: Zn with a core-shell structure 1-x Cu x The preparation method of O / TiO2 photocatalytic composite material specifically includes: Preparation of S1 and ZIF precursors ZIF precursors were prepared using zinc, copper, and 2-methylimidazole sources; S2, Zn 1-x Cu x Preparation of O / TiO2 composite materials S2-1, Titanium source pretreatment Formaldehyde and methylamine are mixed in a molar ratio of 1-2:1, and then mixed with toluene in a mass ratio of 1:10-15. The mixture is heated at 150-250°C for 2-3 hours to obtain transition solution A. 4-Carboxybenzaldehyde and graphene are mixed in a mass ratio of 10-15:1 to obtain transition solution B. Transition solution A and transition solution B are then mixed in a volume ratio of 10:1-3 and heated for 4-8 hours to obtain transition solution C. Toluene in transition solution C is then removed by rotary evaporation, and the solution is dried at room temperature and pressure for 8-12 hours to obtain a graphene matrix. The graphene matrix is ​​then mixed with TiO2 in a molar ratio of 1-2:1 and mechanically dispersed for 30-60 minutes to obtain titanium dioxide / graphene composite powder. S2-2, Preparation of matrix solution Titanium dioxide / graphene composite powder was ultrasonically dispersed in an organic solvent with a mass ratio of 5~8:1 to obtain dispersion solution B. Then, dispersion solution B was mixed with active solution at a volume ratio of 5:1~2 and stirred for 10~20 min to obtain matrix solution. S2-3, Preparation of Composite Materials The ZIF precursor obtained in S1 was ultrasonically dispersed in the matrix solution obtained in S2-2, heated at 150-200℃ for 4-8 h, and then centrifuged at 4000-5000 r / min to obtain Zn. 1-x Cu xO / TiO2 composite material.

[0009] Further, the method for preparing the active solution in step S2-2 is as follows: polyvinylpyrrolidone, polyacrylamide, acetic acid and water are mixed in a mass ratio of 1~2:1~2:1~3:10~15 and then ultrasonically treated for 10~20 min to obtain the active solution; The active solution provides an acidic environment during the preparation of the core-shell catalyst, which allows the colloidal particles to be uniformly dispersed in the solution. At the same time, it also plays a role in colloidal protection, stabilizing the colloidal particles and facilitating their subsequent coating onto the matrix.

[0010] Further, the ZIF precursor uses a first ZIF precursor; the specific preparation method of the first ZIF precursor in step S1 is as follows: a Cu source and a Zn source with a molar ratio of 1:1~3 are mixed and then added to a dispersion solution A with a molar ratio of 1:10~15 for ultrasonic dispersion to obtain a mother liquor; wherein, the dispersion solution A is a mixture of polycarbonate and water with a molar ratio of 1:10~15; n-butanol and m-phenylenediamine are mixed with a molar ratio of 8~10:1 and then added dropwise to the mother liquor at a volume ratio of 2~3:2 to obtain an upstream solution; then the upstream solution is heated at 60~ Heating at 80℃ for 2-3 hours, followed by cooling and drying at room temperature and pressure for 8-12 hours, yields a matrix. The matrix is ​​then heated at 100-120℃ for 1-2 hours, followed by heating to 400-450℃ for 3-5 hours to obtain CuZn microspheres. CuZn microspheres, 2-methylimidazole, and potassium chloride are mixed in a molar ratio of 10:8-10:1-2 and ground for 5-10 minutes to obtain mixed powder A. A grinding aid solution is then added to mixed powder A at a volume ratio of 1:5-8, and the mixture is ball-milled for 20-30 minutes to obtain mixed powder B. After washing, the powder is dried at room temperature and pressure for 12-24 hours to obtain the first ZIF precursor. This method first prepares CuZn microspheres with good surface density, and then adds a small amount of grinding aid solution to the solid phase to prepare ZIF precursor by mechanochemical method. Compared with using Cu and Zn directly, CuZn microspheres have a larger specific surface area and surface permeability, which is more conducive to binding to the framework material and obtaining a denser and more uniform ZIF precursor.

[0011] Furthermore, the grinding aid solution is prepared by mixing trimethylolpropane and Cr2O3-Al2O3 in a molar ratio of 10~15:1, then mixing it with 10% ammonia in a molar ratio of 1:1~2, and then heating it at 300~350℃ for 3~5h to obtain intermediate solution A; Then, methylstyrene with a molar ratio of 1~2:10 to intermediate solution A is added, and the mixture is heated for 1~2 hours at 200~250 kPa and 100~150 °C to obtain intermediate solution B. Then, intermediate solution B, 10% ammonia water, and hydrogen peroxide are mixed at a volume ratio of 5~8:1:1~2 and heated at 50~60℃ for 1~2 hours. After cooling, the mixture is mixed with methanol at a volume ratio of 1:3~5 to obtain a grinding aid solution. During the grinding process, the mixed powder A gradually becomes finer, its specific surface area increases, and its surface becomes charged due to broken bonds. The particles adsorb to each other and agglomerate, which reduces the efficiency of crushing and reaction. Adding a grinding aid solution can prevent particle agglomeration, improve material flowability, thereby increasing grinding efficiency and shortening grinding time. Moreover, the grinding aid can also reduce the activation energy of the reaction, accelerate the reaction rate, and improve the conversion rate of raw materials.

[0012] Further, the ZIF precursor is a second ZIF precursor; the specific preparation method of the second ZIF precursor in step S1 is as follows: 2-methylimidazole and deionized water are mixed at a mass ratio of 1:10~15 to obtain precursor solution A; copper nitrate and deionized water are mixed at a mass ratio of 1:10~15 to obtain precursor solution B; then precursor solution A, with a volume ratio of 2:2~3 to precursor solution B, is added dropwise to precursor solution B and magnetically stirred at 100~150℃ for 2~4h to obtain a mixed solution; then the mixed solution is electrolyzed using a zinc sheet as the anode and a carbon rod as the cathode, and then centrifuged to obtain the second ZIF precursor; The hydrothermal method is used to bind Cu to the framework material first, and then Zn can be more easily bound to the framework material by electrolyzing the mixed solution. The stepwise processing can improve the preparation efficiency and yield of ZIF precursor.

[0013] Furthermore, after centrifugation, the second ZIF precursor is washed 2-3 times with ultrapure water and organic solvent, then soaked in organic solvent for 4-6 hours, followed by centrifugation at 4000-5000 r / min, and dried to obtain the second ZIF precursor. Ultrapure water can wash away inorganic residues such as copper nitrate, while soaking in organic solvents can remove residual 2-methylimidazole. After washing, a ZIF precursor with higher purity can be obtained.

[0014] Furthermore, the precursor solution B also contains a surfactant with a volume ratio of 1:18~25 to the precursor solution B, specifically sodium dodecyl sulfate and anionic polyacrylamide with a molar ratio of 4:1~2. The addition of surfactants can disperse the components in the solution and protect the colloidal particles, ultimately resulting in a second ZIF precursor with better morphology and performance.

[0015] Further, the TiO2 in step S2 is chlorine-doped titanium dioxide; the preparation method of the chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 4~5:1:1~2:5~8 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 15~20:1 to obtain precursor solution D; precursor solution D with a volume ratio of 2:2~3 to precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 70~90℃ for 3~5h to obtain gel; then the gel is baked at 400~500℃ for 1.5~2.5h to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 1~2:10~15 and heated at 100~130℃ for 2~4h, centrifuged and dried to obtain chlorine-doped titanium dioxide; The carboxyl group in propionic acid can lower the valence band edge of TiO2, and the electron-withdrawing effect of chloride ions can further lower the valence band edge of TiO2. The reduction of the valence band edge position improves the oxidation ability of photogenerated holes. At the same time, the electron-withdrawing effect of carboxyl groups and chloride ions can accelerate the migration of electrons to the surface and reduce the recombination rate of photocarriers. Therefore, chlorine-doped titanium dioxide has higher photocatalytic activity than TiO2.

[0016] Further, the characteristic is that the Zn described in steps S2-3 1-x Cu x The O / TiO2 composite material is further purified; the purification process specifically involves: removing the Zn... 1-x Cu x The O / TiO2 composite material was calcined at 300~500℃ for 3~5h, cooled and washed, and then dried at room temperature and pressure. Calcination can reduce Zn 1-x Cu x Removal of the organic framework from the O / TiO2 composite material yields purer Zn. 1-x Cu x O / TiO2 composite material.

[0017] Furthermore, the composite material Zn 1-x Cu x O / TiO2 is applied in the field of photocatalysis; Zn 1-x Cu x O / TiO2 composite materials exhibit good photocatalytic effects on methyl orange under acidic conditions, and therefore can be applied in the field of photocatalysis.

[0018] The beneficial effects of this invention are: compared with the prior art, the ZIF precursor of this invention is more dense and uniform, the resulting composite material has a larger specific surface area, better dispersibility, uniform sample morphology, no agglomeration, and the preparation process is simple and rapid; Zn 1-x Cu x The composite of O and TiO2, with TiO2 as a single crystal tightly coated on zinc copper oxide, exhibits a core-shell nanocrystal structure. This structure provides excellent light absorption in the visible light region, further extending the absorption sideband and forming a pn heterojunction. This facilitates electron-hole separation and effectively suppresses carrier recombination, resulting in superior visible light photocatalytic treatment efficiency for methyl orange. The titanium source used in this invention is modified TiO2, which, through doping with other elements, achieves higher photocatalytic activity than conventional TiO2, further enhancing the final Zn content. 1-x Cu x The O / TiO2 composite material exhibits high photocatalytic activity; moreover, the process of this invention is simple and easy to use on a large scale. Attached Figure Description

[0019] Figure 1 , 2 3. Zn synthesized using TiO2 as the titanium source 1-x Cu x XRD patterns of O / TiO2 nanocrystals; among which... Figure 1 This is a comparison chart with the copper oxide standard card; Figure 2 This is a comparison chart with the zinc oxide standard card; Figure 3 This is a comparison chart with the titanium dioxide standard card.

[0020] Figure 4 , 5 6 represents the synthesis of Zn using tetrabutyl titanate as the titanium source. 1-x Cu x XRD pattern of O / TiO2 crystal; where... Figure 4 This is a comparison chart with the copper oxide standard card; Figure 5 This is a comparison chart with the zinc oxide standard card; Figure 6 This is a comparison chart with the titanium dioxide standard card.

[0021] Figure 7 , 8 9 and 10 are Zn synthesized using TiO2 as the titanium source. 1-x Cu x SEM images of O / TiO2 nanocrystals at different magnifications; among them... Figure 7 The electron microscope scale bar is 5 μm. Figure 8 The electron microscope scale bar is 1 μm. Figure 9 , Figure 10 The electron microscope scale bar is 500 nm.

[0022] Figure 11, 12 Zn was synthesized in an acid-free environment using tetrabutyl titanate as the titanium source, with a zinc-copper to titanium molar ratio of 1:2. 1- x Cu x SEM images of O / TiO2 nanocrystals at different magnifications; among them... Figure 11 The electron microscope scale bar is 5 μm. Figure 12 The electron microscope scale bar is 500 nm.

[0023] Figure 13 , 14 Zn was synthesized under acidic conditions using tetrabutyl titanate as the titanium source, with a molar ratio of zinc, copper, and titanium of 1:2. 1- x Cu x SEM images of O / TiO2 nanocrystals at different magnifications; among them... Figure 13 The electron microscope scale bar is 5 μm. Figure 12 The electron microscope scale bar is 500 nm.

[0024] Figure 15 , 16 17 and 18 describe the synthesis of Zn under acidic conditions using tetrabutyl titanate as the titanium source, with a zinc-copper to titanium molar ratio of 1:2. 1-x Cu x TEM images of O / TiO2 nanocrystals; among them... Figure 15 The electron microscope scale bar is 100 nm. Figure 16 The electron microscope scale bar is 200 nm. Figure 17 , Figure 18 The electron microscope scale bar is 10 nm.

[0025] Figure 19 , 20 Zn is synthesized under acidic conditions using tetrabutyl titanate as the titanium source and a zinc-copper-titanium molar ratio of 1:2. 1-x Cu x High-magnification TEM image of O / TiO2 crystal; among which... Figure 19 The electron microscope scale bar is 10 nm. Figure 20 The length of the electron microscope scale in Fourier space is 10 (1 / nm).

[0026] Figure 21 It is Zn 1-x Cu x The curve of methyl orange degradation by O / TiO2 composite material. Detailed Implementation

[0027] Example 1 Zn with core-shell structure 1-x Cu x The preparation method of O / TiO2 photocatalytic composite material specifically includes: S1. Copper nitrate and zinc nitrate were mixed in a molar ratio of 1:1 to obtain a metal salt. The metal salt was then dissolved in an organic solvent and magnetically stirred for 10 min. 2-Methylimidazole, in a molar ratio of 1:8 to the metal salt, was dissolved in the organic solvent and magnetically stirred for 10 min. The two solutions were then mixed and magnetically stirred for 30 min. The mixture was then poured into a hydrothermal reactor and reacted at 140℃ for 1 h. After centrifugation, washing, and drying, Zn was obtained. 1-x Cu x O precursor; wherein, the organic solvent is specifically anhydrous ethanol; S2, Zn 1-x Cu x The O precursor was placed in a muffle furnace, the temperature was adjusted to 550℃, and calcined for 3 hours to remove the ZIF framework and obtain Zn. 1-x Cu x O; S3. Calcined Zn 1-x Cu x O was dispersed into the dispersion solution and magnetically stirred for 10 min; then it was combined with Zn 1-x Cu x A titanium source with a molar ratio of 1:1 was dispersed in dispersion solution C and magnetically stirred for 10 min. After stirring, the two solutions were mixed and stirred for 30 min. The solution was then poured into a hydrothermal reactor and hydrothermally reacted at 140 °C for 2 h. After centrifugation, washing, drying, and grinding, Zn was obtained. 1-x Cu x O / TiO2 composite material; wherein, the titanium source is specifically TiO2 powder; the dispersion solution C is specifically anhydrous ethanol, and the amount used is 10% of the solvent volume.

[0028] It should be noted that: Zn 1-x Cu x The molar ratio of O to the titanium source can also be 1:2 or 1:3, and the titanium source can also be tetrabutyl titanate.

[0029] Example 2 Zn with core-shell structure 1-x Cu x The preparation method of O / TiO2 photocatalytic composite material specifically includes: Preparation of S1 and ZIF precursors Copper nitrate and zinc nitrate were mixed in a 1:1 molar ratio to obtain a metal salt. The metal salt was then dissolved in an organic solvent and magnetically stirred for 10 min. Next, 2-methylimidazole, in a 1:8 molar ratio with the metal salt, was dissolved in the organic solvent and magnetically stirred for 10 min. The two solutions were then mixed and magnetically stirred for 30 min. The mixture was then poured into a hydrothermal reactor and reacted at 140 °C for 1 h. After centrifugation, washing, and drying, Zn was obtained. 1-x Cux O precursor; wherein, the organic solvent is specifically anhydrous ethanol; Tetrabutyl titanate at a molar ratio of 1:1 to the ZIF precursor was added dropwise to an ethanol solution under magnetic stirring. After the addition was completed, the solution was stirred for 30 min to obtain base solution A. PVP (polyvinylpyrrolidone) at a molar ratio of 1:20 to tetrabutyl titanate was dissolved in deionized water and stirred for 20 min to obtain base solution B. Then, the ZIF precursor was added to anhydrous methanol and ultrasonically dispersed for 20 min to obtain base solution C.

[0030] Add base solution B to base solution C and stir for 30 minutes to obtain base solution D; S2, Zn 1-x Cu x Preparation of O / TiO2 composite materials Solution A was added dropwise to solution D with stirring and stirred for 1 hour. Then, the solution was ultrasonically dispersed for 30 minutes and placed in a hydrothermal reactor to react at a constant temperature of 200°C for 1 hour.

[0031] The obtained product was washed, dried, and ground, then placed in a crucible and calcined at 500°C for 4 hours to obtain Zn. 1-x Cu x O / TiO2 composite material.

[0032] It should be noted that: Zn 1-x Cu x The molar ratio of O to the titanium source can also be 1:2 or 1:3, and the titanium source can also be tetrabutyl titanate.

[0033] Example 3 Zn with core-shell structure 1-x Cu x The preparation method of O / TiO2 photocatalytic composite material specifically includes: Preparation of S1 and ZIF precursors A Cu source and a Zn source with a molar ratio of 1:1 were mixed and then added to dispersion solution A with a molar ratio of 1:10 for ultrasonic dispersion to obtain a mother liquor; wherein, dispersion solution A is a mixture of polycarbonate and water with a molar ratio of 1:10. n-Butanol and m-phenylenediamine were mixed in a molar ratio of 8:1 and then added dropwise to the mother liquor in a volume ratio of 1:1 to obtain the upstream solution. The upstream solution was then heated at 60°C for 2 hours, cooled, and dried at room temperature and pressure for 8 hours to obtain the matrix. The substrate was then heated at 100℃ for 1 hour, and then heated to 400℃ for 3 hours to obtain CuZn microspheres. CuZn microspheres, 2-methylimidazole, and potassium chloride were mixed in a molar ratio of 10:8:1 and ground for 5 min to obtain mixed powder A. Then, a grinding aid solution was added to mixed powder A in a volume ratio of 1:5, and the mixture was ball-milled for 20 min to obtain mixed powder B. After washing, the mixture was dried at room temperature and pressure for 12 h to obtain the first ZIF precursor. The grinding aid solution is prepared by mixing trimethylolpropane and Cr2O3-Al2O3 in a molar ratio of 10~15:1, then mixing it with 10% ammonia water in a molar ratio of 1:1, and then heating it at 300℃ for 3 hours to obtain intermediate solution A. Then, methylstyrene with a molar ratio of 1:10 to intermediate solution A was added, and the mixture was heated at 200 kPa and 100 °C for 1 hour to obtain intermediate solution B. Then, intermediate solution B, 10% ammonia water, and hydrogen peroxide were mixed in a volume ratio of 5:1:1 and heated at 50°C for 1 hour. After cooling, the mixture was mixed with methanol in a volume ratio of 1:3 to obtain a grinding aid solution. S2, Zn 1-x Cu x Preparation of O / TiO2 composite materials S2-1, Titanium source pretreatment Formaldehyde and methylamine were mixed in a molar ratio of 1:1, and then mixed with toluene in a mass ratio of 1:10. The mixture was heated at 150°C for 2 hours to obtain transition solution A. 4-Carboxybenzaldehyde and graphene were mixed in a mass ratio of 10:1 to obtain transition solution B. Transition solution A and transition solution B were then mixed in a volume ratio of 10:1 and heated for 4 hours to obtain transition solution C. Toluene in transition solution C was removed by rotary evaporation, and then dried at room temperature and pressure for 8 hours to obtain a graphene matrix. The graphene matrix was then mixed with TiO2 in a molar ratio of 1:1 and mechanically dispersed for 30 minutes to obtain titanium dioxide / graphene composite powder. S2-2, Preparation of matrix solution The titanium dioxide / graphene composite powder was ultrasonically dispersed in an organic solvent with a mass ratio of 5:1 to the titanium dioxide / graphene composite powder to obtain dispersion solution B. Then, dispersion solution B was mixed with active solution at a volume ratio of 5:1 and stirred for 10 min to obtain matrix solution. The active solution is prepared by mixing polyvinylpyrrolidone, polyacrylamide, acetic acid and water in a mass ratio of 1:1:1:10 and then sonicating for 10 minutes to obtain the active solution. S2-3, Preparation of Composite Materials The ZIF precursor obtained in S1 was ultrasonically dispersed in the matrix solution obtained in S2-2, heated at 150℃ for 4 h, and then centrifuged at 4000 r / min to obtain Zn. 1-x Cu x O / TiO2 composite material; Zn 1-x Cu x The O / TiO2 composite material was calcined at 300℃ for 3 hours, cooled, washed, and then dried at room temperature and pressure to obtain Zn with higher purity. 1-x Cu x O / TiO2 composite material.

[0034] Zn 1-x Cu x O / TiO2 composite materials can be applied in the field of photocatalysis.

[0035] Example 4 The difference from Example 3 is that TiO2 in step S2 is chlorine-doped titanium dioxide. The preparation method of chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 4:1:1:5 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 15:1 to obtain precursor solution D; precursor solution D with a volume ratio of 1:1 with precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 70°C for 3 hours to obtain gel; then the gel is baked at 400°C for 1.5 hours to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 1:10 and heated at 100°C for 2 hours, centrifuged and dried to obtain chlorine-doped titanium dioxide.

[0036] Example 5 Zn with core-shell structure 1-x Cu x The preparation method of O / TiO2 photocatalytic composite material specifically includes: Preparation of S1 and ZIF precursors A Cu source and a Zn source with a molar ratio of 1:2 were mixed and then added to dispersion solution A with a molar ratio of 1:12 for ultrasonic dispersion to obtain a mother liquor; wherein, dispersion solution A is a mixture of polycarbonate and water with a molar ratio of 1:12. n-Butanol and m-phenylenediamine were mixed in a molar ratio of 9:1 and then added dropwise to the mother liquor in a volume ratio of 5:4 to obtain the upstream solution. The upstream solution was then heated at 70°C for 2.5 h, cooled, and dried at room temperature and pressure for 10 h to obtain the matrix. The matrix was then heated at 110℃ for 1.5 h, and then heated to 425℃ for 4 h to obtain CuZn microspheres; CuZn microspheres, 2-methylimidazole, and potassium chloride were mixed in a molar ratio of 10:9:1 and ground for 8 min to obtain mixed powder A. Then, a grinding aid solution was added to mixed powder A in a volume ratio of 1:6, and the mixture was ball-milled for 25 min to obtain mixed powder B. After washing, the mixture was dried at room temperature and pressure for 18 h to obtain the first ZIF precursor. The grinding aid solution is prepared by mixing trimethylolpropane and Cr2O3-Al2O3 in a molar ratio of 12:1, then mixing it with 10% ammonia in a molar ratio of 2:3, and then heating it at 325℃ for 4 hours to obtain intermediate solution A. Then, methylstyrene with a molar ratio of 3:20 to intermediate solution A was added, and the mixture was heated at 225 kPa and 125 °C for 1.5 h to obtain intermediate solution B. Then, intermediate solution B, 10% ammonia water, and hydrogen peroxide were mixed at a volume ratio of 6:1:1 and heated at 55°C for 1.5 hours. After cooling, the mixture was mixed with methanol at a volume ratio of 1:4 to obtain a grinding aid solution. S2, Zn 1-x Cu x Preparation of O / TiO2 composite materials S2-1, Titanium source pretreatment Formaldehyde and methylamine were mixed at a molar ratio of 3:2, and then mixed with toluene at a mass ratio of 1:12. The mixture was heated at 200°C for 2.5 h to obtain transition solution A. 4-Carboxybenzaldehyde and graphene were mixed at a mass ratio of 12:1 to obtain transition solution B. Transition solution A and transition solution B were then mixed at a volume ratio of 10:2 and heated for 6 h to obtain transition solution C. Toluene in transition solution C was removed by rotary evaporation, and then dried at room temperature and pressure for 10 h to obtain a graphene matrix. The graphene matrix was then mixed with TiO2 at a molar ratio of 3:2 and mechanically dispersed for 45 min to obtain titanium dioxide / graphene composite powder. S2-2, Preparation of matrix solution The titanium dioxide / graphene composite powder was ultrasonically dispersed in an organic solvent with a mass ratio of 6:1 to obtain dispersion solution B. Then, dispersion solution B was mixed with active solution at a volume ratio of 10:3 and stirred for 15 min to obtain matrix solution. The active solution is prepared by mixing polyvinylpyrrolidone, polyacrylamide, acetic acid and water in a mass ratio of 1:1:1:12 and then sonicating for 15 minutes to obtain the active solution. S2-3, Preparation of Composite Materials The ZIF precursor obtained in S1 was ultrasonically dispersed in the matrix solution obtained in S2-2, heated at 175℃ for 6 h, and then centrifuged at 4500 r / min to obtain Zn. 1-x Cu x O / TiO2 composite material; Zn 1-x Cu x The O / TiO2 composite material was calcined at 400℃ for 4 hours, cooled, washed, and then dried at room temperature and pressure to obtain Zn with higher purity. 1-x Cu x O / TiO2 composite material.

[0037] Zn 1-x Cu x O / TiO2 composite materials can be applied in the field of photocatalysis.

[0038] Example 6 The difference from Example 5 is that step S2TiO2 uses chlorine-doped titanium dioxide. The preparation method of chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 4:1:1:7 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 18:1 to obtain precursor solution D; precursor solution D with a volume ratio of 4:5 to precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 80°C for 4 hours to obtain gel; then the gel is baked at 450°C for 2 hours to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 1:8 and heated at 120°C for 3 hours, centrifuged and dried to obtain chlorine-doped titanium dioxide.

[0039] Example 7 Zn with core-shell structure 1-x Cu x The preparation method of O / TiO2 photocatalytic composite material specifically includes: Preparation of S1 and ZIF precursors A Cu source and a Zn source with a molar ratio of 1:3 were mixed and then added to dispersion solution A with a molar ratio of 1:15 for ultrasonic dispersion to obtain a mother liquor; wherein, dispersion solution A is a mixture of polycarbonate and water with a molar ratio of 1:15. n-Butanol and m-phenylenediamine were mixed in a molar ratio of 10:1 and then added dropwise to the mother liquor in a volume ratio of 3:2 to obtain the upstream solution. The upstream solution was then heated at 80°C for 3 hours, cooled, and dried at room temperature and pressure for 12 hours to obtain the matrix. The substrate was then heated at 120℃ for 2 hours, and then heated to 450℃ for 5 hours to obtain CuZn microspheres. CuZn microspheres, 2-methylimidazole, and potassium chloride were mixed in a molar ratio of 5:5:1 and ground for 10 min to obtain mixed powder A. Then, a grinding aid solution was added to mixed powder A in a volume ratio of 1:8, and the mixture was ball-milled for 30 min to obtain mixed powder B. After washing, the mixture was dried at room temperature and pressure for 24 h to obtain the first ZIF precursor. The grinding aid solution is prepared by mixing trimethylolpropane and Cr2O3-Al2O3 in a molar ratio of 15:1, then mixing it with 10% ammonia in a molar ratio of 1:2, and then heating it at 350℃ for 5 hours to obtain intermediate solution A. Then, methylstyrene with a molar ratio of 1:5 to intermediate solution A was added, and the mixture was heated for 2 hours at 250 kPa and 150 °C to obtain intermediate solution B. Then, intermediate solution B, 10% ammonia water, and hydrogen peroxide were mixed at a volume ratio of 8:1:2 and heated at 60°C for 2 hours. After cooling, the mixture was mixed with methanol at a volume ratio of 1:5 to obtain a grinding aid solution. S2, Zn 1-x Cu x Preparation of O / TiO2 composite materials S2-1, Titanium source pretreatment Formaldehyde and methylamine were mixed at a molar ratio of 2:1, and then mixed with toluene at a mass ratio of 1:15. The mixture was heated at 250°C for 3 hours to obtain transition solution A. 4-Carboxybenzaldehyde and graphene were mixed at a mass ratio of 15:1 to obtain transition solution B. Transition solution A and transition solution B were then mixed at a volume ratio of 10:3 and heated for 8 hours to obtain transition solution C. Toluene in transition solution C was then removed by rotary evaporation, and the solution was dried at room temperature and pressure for 12 hours to obtain a graphene matrix. The graphene matrix was then mixed with TiO2 at a molar ratio of 2:1 and mechanically dispersed for 30-60 minutes to obtain titanium dioxide / graphene composite powder. S2-2, Preparation of matrix solution Titanium dioxide / graphene composite powder was ultrasonically dispersed in an organic solvent with a mass ratio of 8:1 to obtain dispersion solution B. Then, dispersion solution B was mixed with active solution at a volume ratio of 5:2 and stirred for 20 min to obtain matrix solution. The active solution is prepared by mixing polyvinylpyrrolidone, polyacrylamide, acetic acid and water in a mass ratio of 2:2:3:15 and then sonicating for 20 minutes to obtain the active solution. S2-3, Preparation of Composite Materials The ZIF precursor obtained in S1 was ultrasonically dispersed in the matrix solution obtained in S2-2, heated at 200℃ for 8 h, and then centrifuged at 5000 r / min to obtain Zn. 1-x Cu x O / TiO2 composite material; Zn 1-x Cu x The O / TiO2 composite material was calcined at 500℃ for 5 hours, cooled, washed, and then dried at room temperature and pressure to obtain Zn with higher purity. 1-x Cu x O / TiO2 composite material.

[0040] Zn 1-x Cu x O / TiO2 composite materials can be applied in the field of photocatalysis.

[0041] Example 8 The difference from Example 7 is that TiO2 in step S2 is chlorine-doped titanium dioxide. The preparation method of chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 5:1:2:8 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 20:1 to obtain precursor solution D; precursor solution D with a volume ratio of 2:3 to precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 90°C for 5 hours to obtain gel; then the gel is baked at 500°C for 2.5 hours to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 2:15 and heated at 130°C for 4 hours, centrifuged and dried to obtain chlorine-doped titanium dioxide.

[0042] Example 9 The difference from Example 3 is that the ZIF precursor used in step S1 is a second ZIF precursor. The specific preparation method of the second ZIF precursor is as follows: 2-methylimidazole and deionized water are mixed at a mass ratio of 1:10 to obtain precursor solution A; copper nitrate and deionized water are mixed at a mass ratio of 1:10 to obtain precursor solution B; then precursor solution A, with a volume ratio of 1:1 to precursor solution B, is added dropwise to precursor solution B and magnetically stirred at 100°C for 2 hours to obtain a mixed solution; then the mixed solution is electrolyzed using a zinc sheet as the anode and a carbon rod as the cathode. After centrifugation, the second ZIF precursor is washed twice with ultrapure water and organic solvent, then soaked in organic solvent for 4 hours, then centrifuged at 4000 r / min, washed, and dried to obtain the second ZIF precursor. The precursor solution B also contains a surfactant in a volume ratio of 1:18 to the precursor solution B. The surfactant is sodium dodecyl sulfate and anionic polyacrylamide in a molar ratio of 4:1.

[0043] Example 10 The difference from Example 9 is that TiO2 in step S2 is chlorine-doped titanium dioxide. The preparation method of chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 4:1:1:5 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 15:1 to obtain precursor solution D; precursor solution D with a volume ratio of 1:1 with precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 70°C for 3 hours to obtain gel; then the gel is baked at 400°C for 1.5 hours to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 1:10 and heated at 100°C for 2 hours, centrifuged and dried to obtain chlorine-doped titanium dioxide.

[0044] Example 11 The difference from Example 5 is that the ZIF precursor in step S1 is a second ZIF precursor. The specific preparation method of the second ZIF precursor is as follows: 2-methylimidazole and deionized water are mixed at a mass ratio of 1:12 to obtain precursor solution A; copper nitrate and deionized water are mixed at a mass ratio of 1:12 to obtain precursor solution B; then precursor solution A with a volume ratio of 4:5 to precursor solution B is added dropwise to precursor solution B and magnetically stirred at 125°C for 3 hours to obtain a mixed solution; then the mixed solution is electrolyzed with zinc sheet as anode and carbon rod as cathode, centrifuged, and then the second ZIF precursor is washed three times with ultrapure water and organic solvent respectively, then soaked in organic solvent for 5 hours, then centrifuged at 4500 r / min, washed, and dried to obtain the second ZIF precursor. The precursor solution B also contains a surfactant in a volume ratio of 1:20 to the precursor solution B. The surfactant is sodium dodecyl sulfate and anionic polyacrylamide in a molar ratio of 8:3.

[0045] Example 12 The difference from Example 11 is that the TiO2 used in step S2 is chlorine-doped titanium dioxide. The preparation method of chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 4:1:1:7 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 18:1 to obtain precursor solution D; precursor solution D with a volume ratio of 4:5 with precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 80°C for 4 hours to obtain gel; then the gel is baked at 450°C for 2 hours to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 1:8 and heated at 120°C for 3 hours, centrifuged and dried to obtain chlorine-doped titanium dioxide.

[0046] Example 13 The difference from Example 7 is that the ZIF precursor in step S1 is a second ZIF precursor. The specific preparation method of the second ZIF precursor is as follows: 2-methylimidazole and deionized water are mixed at a mass ratio of 1:15 to obtain precursor solution A; copper nitrate and deionized water are mixed at a mass ratio of 1:15 to obtain precursor solution B; then precursor solution A with a volume ratio of 2:3 to precursor solution B is added dropwise to precursor solution B and magnetically stirred at 150°C for 4 hours to obtain a mixed solution; then the mixed solution is electrolyzed with zinc sheet as anode and carbon rod as cathode, centrifuged, and then the second ZIF precursor is washed three times with ultrapure water and organic solvent respectively, then soaked in organic solvent for 6 hours, then centrifuged at 5000 r / min, washed, and dried to obtain the second ZIF precursor. The precursor solution B also contains a surfactant in a volume ratio of 1:25 to the precursor solution B. The surfactant is sodium dodecyl sulfate and anionic polyacrylamide in a molar ratio of 2:1.

[0047] Example 14 The difference from Example 13 is that step S2TiO2 uses chlorine-doped titanium dioxide. The preparation method of chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 5:1:2:8 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 20:1 to obtain precursor solution D; precursor solution D with a volume ratio of 2:3 to precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 90°C for 5 hours to obtain gel; then the gel is baked at 500°C for 2.5 hours to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 2:15 and heated at 130°C for 4 hours, centrifuged and dried to obtain chlorine-doped titanium dioxide.

[0048] Experimental Example 1 Zn with core-shell structure 1-x Cu x Methods for preparing O / TiO2 photocatalytic composite materials include: S1. Weigh 0.6082 g of zinc nitrate hexahydrate and 0.44334 g of copper nitrate hexahydrate into a 100 ml flask, add 30 ml of methanol solution, and stir magnetically for 10 min. Weigh 1.9212 g of 2-methylimidazole into another flask, add 30 ml of methanol solution, and stir magnetically for 10 min. Then mix the two flasks and stir for 30 min. Pour the well-mixed solution into a 100 ml hydrothermal reactor and react at 140 °C for 1 h. After the reactor has cooled completely, place the product in a centrifuge tube, centrifuge, wash, and dry to obtain Zn. 1-x Cu x O precursor; S2. Place the ZIF precursor into a muffle furnace, adjust the temperature to 550℃, and calcine for 3 hours to remove the ZIF skeleton. S3. Calcined Zn 1-x Cu x O was dispersed in 20 ml of ethanol and magnetically stirred for 10 min. Then, 0.120 g of titanium dioxide powder was dispersed in 20 ml of ethanol and magnetically stirred for 10 min. After both were stirred separately, they were combined and stirred for 30 min. The solution was then poured into a hydrothermal reactor and hydrothermally reacted at 140℃ for 2 h. Afterward, the solution was centrifuged, washed, dried, and ground to obtain Zn. 1-x Cu x O / TiO2 composite material.

[0049] Experimental Example 2 Unlike Experiment 1, 0.7300g of zinc nitrate hexahydrate and 0.3547g of copper nitrate hexahydrate were used.

[0050] Experimental Example 3 Unlike Experiment 1, 0.9732g of zinc nitrate hexahydrate and 0.1773g of copper nitrate hexahydrate were used.

[0051] Experiment Example 4 Zn with core-shell structure 1-x Cu x The preparation method of O / TiO2 photocatalytic composite material specifically includes: S1. Weigh 0.6082g of zinc nitrate hexahydrate and 0.44334g of copper nitrate hexahydrate into a 100ml flask, add 30ml of methanol solution, and stir magnetically for 10min. Weigh 1.9212g of 2-methylimidazole into another flask, add 30ml of methanol solution, and stir magnetically for 10min. Then mix the two and stir for 30min. Pour the well-mixed solution into a 100ml hydrothermal reactor and react at 140℃ for 1h. After the reactor has cooled down, place the product in a centrifuge tube, centrifuge, wash, and dry to obtain the ZIF precursor.

[0052] Under magnetic stirring, 0.5 ml of tetrabutyl titanate was added dropwise to 20 ml of ethanol solution. After the addition was completed, the mixture was stirred for 30 min to obtain base solution A. 0.5 g of PVP (polyvinylpyrrolidone) was dissolved in 20 ml of deionized water and stirred for 20 min to obtain solution base B. Then, the ZIF precursor was added to 20 ml of anhydrous methanol and ultrasonically dispersed for 20 min to obtain base solution C.

[0053] Add base solution B to base solution C and stir for 30 minutes to obtain base solution D; S2. Add base solution A dropwise to base solution D while stirring, and continue stirring for 1 hour. Then, disperse the solution by ultrasonication for 30 minutes. Pour the solution into a 100 ml hydrothermal reactor and react at a constant temperature of 200 °C for 1 hour.

[0054] The obtained product was washed, dried, and ground, then placed in a crucible and calcined at 500°C for 4 hours to finally obtain Zn. 1-x Cu x O / TiO2 composite material.

[0055] Experimental Example 5 Unlike the experimental example, 1.1 ml of tetrabutyl titanate was taken in S1.

[0056] Experimental Example 6 Unlike the experimental example, 1.6 ml of tetrabutyl titanate was taken in S1.

[0057] XRD test Figure 1 , 2 3. Zn synthesized using TiO2 as the titanium source 1-x Cu x XRD pattern of O / TiO2 nanocrystals. The figure shows that the peaks of copper oxide, zinc oxide, and titanium dioxide standard cards are similar to those of Zn. 1-x Cu x Both O / TiO2 nanocrystals exhibit matching characteristic peaks, which indicates that Zn 1-x Cu x The O / TiO2 composite material was successfully synthesized.

[0058] Figure 4 , 5 6 represents the synthesis of Zn using tetrabutyl titanate as the titanium source. 1-x Cu x XRD pattern of O / TiO2 crystals. In the diagram, a represents a 1:1 molar ratio of zinc, copper, and titanium under acidic conditions; b represents a 1:2 molar ratio under acidic conditions; c represents a 1:3 molar ratio under acidic conditions; d represents a 1:1 molar ratio under acid-free conditions; e represents a 1:2 molar ratio under acid-free conditions; and f represents a 1:3 molar ratio under acid-free conditions. The graph shows the peaks of copper oxide, zinc oxide, and titanium dioxide according to the standard cards and the Zn... 1-x Cu x Both O / TiO2 nanocrystals exhibit matching characteristic peaks, which indicates that Zn 1-x Cu x The O / TiO2 composite material was successfully synthesized.

[0059] SEM test Figures 7-10 Synthesis of Zn using TiO2 as a titanium source 1-x Cu x SEM images of O / TiO2 nanocrystals at different magnifications. The images show that titanium dioxide particles are coated with Zn. 1-x Cu x On O, a spherical morphology is formed, and the particles are relatively uniform.

[0060] Figure 11 , 12 Zn was synthesized in an acid-free environment using tetrabutyl titanate as the titanium source, with a zinc-copper to titanium molar ratio of 1:2. 1- x Cu x SEM images of O / TiO2 nanocrystals at different magnifications. The images show that under these conditions, the material particles are square and uniform, with a relatively small particle size, a large specific surface area, and no agglomeration occurs.

[0061] Figure 13 , 14 Zn was synthesized under acidic conditions using tetrabutyl titanate as the titanium source, with a molar ratio of zinc, copper, and titanium of 1:2. 1- x Cu x SEM images of O / TiO2 nanocrystals at different magnifications. The image shows the Zn formed when the zinc-copper composite material is in an acidic environment with a zinc-copper to titanium molar ratio of 1:2. 1-x Cu x O / TiO2 composite material, made of Figures 15-18 It can be seen that the material has relatively uniform particle size, small particle size, and large specific surface area. Through comparison, it was found that the sample morphology is the best under these conditions.

[0062] TEM test Figure 19 , 20 Zn was synthesized under acidic conditions using tetrabutyl titanate as the titanium source and a zinc-copper-titanium molar ratio of 1:2. 1- x Cu x TEM image of O / TiO2 nanocrystals. This TEM image shows that Zn... 1-x Cu x O / TiO2 nanocrystal particles exhibit a core-shell structure, and each Zn 1-x Cu x The O / TiO2 nanocrystal particles have a relatively large specific surface area and are uniform in size. A clear grating can be seen in the magnified image. Figure 19 It can be seen that the interplanar spacing of the nanocrystal particles is 0.3265 nanometers. Furthermore, the central part is polycrystalline, while the outermost crystal particles are all monocrystalline.

[0063] Photocatalytic performance test Figure 21 Zn was synthesized under acidic conditions using tetrabutyl titanate as the titanium source and a zinc-copper-titanium molar ratio of 1:2. 1-x Cu x The degradation curves of methyl orange in the O / TiO2 composite material are shown. The degradation of methyl orange over the same time period is compared with that of the synthesized Zn. 1-x Cu x The photocatalytic performance of the O / TiO2 composite material was tested, and the results showed that: Zn 1-x Cu x The photocatalytic efficiencies of the O / TiO2 composite material at 60 min were 60% and 17%, respectively, indicating that Zn 1-x Cu x The O / TiO2 composite material exhibits good photocatalytic performance.

Claims

1. Zn with a core-shell structure 1-x Cu x The method for preparing O / TiO2 photocatalytic composite material is characterized by, Specifically, it includes: Preparation of S1 and ZIF precursors ZIF precursors were prepared using zinc, copper, and 2-methylimidazole sources; S2, Zn 1-x Cu x Preparation of O / TiO2 composite materials S2-1, Titanium source pretreatment Formaldehyde and methylamine are mixed in a molar ratio of 1-2:1, and then mixed with toluene in a mass ratio of 1:10-15. The mixture is heated at 150-250°C for 2-3 hours to obtain transition solution A. 4-Carboxybenzaldehyde and graphene are mixed in a mass ratio of 10-15:1 to obtain transition solution B. Transition solution A and transition solution B are then mixed in a volume ratio of 10:1-3 and heated for 4-8 hours to obtain transition solution C. Toluene in transition solution C is then removed by rotary evaporation, and the solution is dried at room temperature and pressure for 8-12 hours to obtain a graphene matrix. The graphene matrix is ​​then mixed with TiO2 in a molar ratio of 1-2:1 and mechanically dispersed for 30-60 minutes to obtain titanium dioxide / graphene composite powder. S2-2, Preparation of matrix solution Titanium dioxide / graphene composite powder was ultrasonically dispersed in an organic solvent with a mass ratio of 5~8:1 to obtain dispersion solution B. Then, dispersion solution B was mixed with active solution at a volume ratio of 5:1~2 and stirred for 10~20 min to obtain matrix solution. S2-3, Preparation of Composite Materials The ZIF precursor obtained in S1 was ultrasonically dispersed in the matrix solution obtained in S2-2, heated at 150-200℃ for 4-8 h, and then centrifuged at 4000-5000 r / min to obtain Zn. 1-x Cu x O / TiO2 composite material; The method for preparing the active solution in step S2-2 is as follows: polyvinylpyrrolidone, polyacrylamide, acetic acid and water are mixed in a mass ratio of 1~2:1~2:1~3:10~15 and then ultrasonically treated for 10~20 min to obtain the active solution; The ZIF precursor mentioned in step S1 uses a first ZIF precursor; the specific preparation method of the first ZIF precursor is as follows: a Cu source and a Zn source with a molar ratio of 1:1~3 are mixed and then added to a dispersion solution A with a molar ratio of 1:10~15 for ultrasonic dispersion to obtain a mother liquor; wherein, the dispersion solution A is a mixture of polycarbonate and water with a molar ratio of 1:10~15; n-butanol and m-phenylenediamine are mixed with a molar ratio of 8~10:1 and then added dropwise to the mother liquor at a volume ratio of 2~3:2 to obtain an upstream solution; then the upstream solution is heated at 60~80℃. Heating under certain conditions for 2-3 hours, followed by cooling and drying at room temperature and pressure for 8-12 hours, yields a matrix. The matrix is ​​then heated at 100-120℃ for 1-2 hours, followed by heating to 400-450℃ for 3-5 hours to obtain CuZn microspheres. CuZn microspheres, 2-methylimidazole, and potassium chloride are mixed in a molar ratio of 10:8-10:1-2 and ground for 5-10 minutes to obtain mixed powder A. A grinding aid solution is then added to mixed powder A at a volume ratio of 1:5-8, and ball-milled for 20-30 minutes to obtain mixed powder B. After washing, the powder is dried at room temperature and pressure for 12-24 hours to obtain the first ZIF precursor. The grinding aid solution is prepared by mixing trimethylolpropane and Cr2O3-Al2O3 in a molar ratio of 10-15:1, then mixing it with 10% ammonia in a molar ratio of 1:1-2, and then heating it at 300-350℃ for 3-5 hours to obtain intermediate solution A. Then, methylstyrene with a molar ratio of 1~2:10 to intermediate solution A is added, and the mixture is heated for 1~2 hours at 200~250 kPa and 100~150 °C to obtain intermediate solution B. Then, intermediate solution B, 10% ammonia water, and hydrogen peroxide are mixed at a volume ratio of 5~8:1:1~2 and heated at 50~60℃ for 1~2 hours. After cooling, the mixture is mixed with methanol at a volume ratio of 1:3~5 to obtain a grinding aid solution. The ZIF precursor mentioned in step S1 is a second ZIF precursor. The specific preparation method of the second ZIF precursor is as follows: 2-methylimidazole and deionized water are mixed at a mass ratio of 1:10~15 to obtain precursor solution A; copper nitrate and deionized water are mixed at a mass ratio of 1:10~15 to obtain precursor solution B; then precursor solution A with a volume ratio of 2:2~3 to precursor solution B is added dropwise to precursor solution B and magnetically stirred at 100~150℃ for 2~4h to obtain a mixed solution; then the mixed solution is electrolyzed with zinc sheet as anode and carbon rod as cathode, and then centrifuged to obtain the second ZIF precursor. The TiO2 mentioned in step S2 is chlorine-doped titanium dioxide; the preparation method of chlorine-doped titanium dioxide is as follows: methanol, 2,3,5,6-tetrachloropyridine, propionic acid and ultrapure water are mixed in a mass ratio of 4~5:1:1~2:5~8 to obtain precursor solution C; methanol and tetrabutyl titanate are mixed in a mass ratio of 15~20:1 to obtain precursor solution D; precursor solution D with a volume ratio of 2:2~3 to precursor solution C is added dropwise to precursor solution C under stirring, and then heated at 70~90℃ for 3~5h to obtain gel; then the gel is baked at 400~500℃ for 1.5~2.5h to obtain dry gel; then the dry gel and precursor solution D are mixed in a volume ratio of 1~2:10~15 and heated at 100~130℃ for 2~4h, centrifuged and dried to obtain chlorine-doped titanium dioxide; After centrifugation, the second ZIF precursor is washed 2-3 times with ultrapure water and organic solvent, then soaked in organic solvent for 4-6 hours, then centrifuged and washed at 4000-5000 r / min, and dried to obtain the second ZIF precursor. The precursor solution B also contains a surfactant with a volume ratio of 1:18~25 to the precursor solution B. The surfactant is specifically sodium dodecyl sulfate and anionic polyacrylamide with a molar ratio of 4:1~2.

2. The Zn with a core-shell structure according to claim 1 1-x Cu x The method for preparing O / TiO2 photocatalytic composite material is characterized by, The Zn mentioned in step S2-3 1-x Cu x The O / TiO2 composite material is further purified; the purification process specifically involves: removing the Zn... 1-x Cu x The O / TiO2 composite material was calcined at 300~500℃ for 3~5h, cooled and washed, and then dried at room temperature and pressure.

3. Zn with a core-shell structure prepared by the preparation method according to any one of claims 1 to 2 1-x Cu x The application of O / TiO2 photocatalytic composite materials is characterized by... It is applied in the field of photocatalysis.

Citation Information

Patent Citations

  • Cu-doped ZnO / graphene composite photocatalyst and preparation method thereof

    CN103182307A

  • Preparation method of TiO2 / ZIF-8 composite photocatalyst

    CN109499620A

  • Preparation method of photo catalytic active chlorine adulterated titanium dioxide nano material

    CN1555915A