A hydrogen-bond cross-linked high-performance polyarylene imide ether nitrile and a preparation method thereof

Through hydrogen bond cross-linking technology, the problem of poor film-forming and toughness of polyarylene ether nitrile when improving its mechanical properties and thermal stability has been solved, and polyarylimine ether nitrile with high strength, high toughness and high thermal stability has been achieved. The preparation simplifies the process and is suitable for industrial production.

CN115612093BActive Publication Date: 2024-10-18SOUTHWEAT UNIV OF SCI & TECH +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211377911.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-10-18
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

While existing polyaryl ether nitrile improves mechanical properties and thermal stability, its film-forming properties and toughness deteriorate, and the synthesis process is complex, making it unsuitable for industrial production.

Method used

Using hydrogen-bonded cross-linked high-performance polyarylimine ether nitriles, by adjusting the molar ratio of dihydroxydiphenylamine and 2,6'-difluorobenzene cyanide monomers and adding potassium carbonate, combined with specific process steps and conditions, Polymers with excellent film-forming properties and toughness are produced.

Benefits of technology

It achieves high strength, high toughness and high thermal stability of polyarylimine ether nitrile, while simplifying the preparation process, being suitable for industrial production, and increasing the glass transition temperature and decomposition temperature of the polymer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure BDA0003927515380000021
    Figure BDA0003927515380000021
Patent Text Reader

Abstract

The invention provides a high-performance polyarylene imine ether nitrile cross-linked by hydrogen bonds and a preparation method thereof, and provides a structural formula of a high-performance polyarylene imine ether nitrile cross-linked by hydrogen bonds, and during its preparation, dimethoxydiphenylamine is used as a raw material, and a dihydroxydiphenylamine monomer is obtained under the catalysis of boron tribromide; dihydroxydiphenylamine and 2,6'-difluorobenzonitrile are used as monomers, and polyarylene imine ether nitrile with different structures is obtained under the catalysis of potassium carbonate. The polyarylene imine ether nitrile prepared by the present invention has excellent film-forming properties, and a polyarylene imine ether nitrile film is obtained by a solution casting method. The prepared polymer film has excellent mechanical properties, a high glass transition temperature and a high decomposition temperature, and the preparation method is simple, and is suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a hydrogen-bond cross-linked high-performance polyarylene imine ether nitrile and a preparation method thereof. Background Art

[0002] Polyarylethernitrile is a special engineering plastic containing phenylene and ether bonds on the main chain and cyano (-CN) characteristic functional groups on the side chain. Since the main chain of polyarylethernitrile molecules contains a large number of rigid aromatic ring structures and flexible ether bond structures, this type of polymer has many advantages such as high strength, high temperature resistance, creep resistance, and corrosion resistance. It has been widely used in high-tech fields such as national defense, aerospace, electronic information, and biomedicine. With the development of various new technologies, the fields of national defense, aerospace, and aviation have put forward higher requirements on the performance of polyarylethernitrile. The research and development of polyarylethernitrile with better mechanical properties and thermal stability has become a scientific problem that needs to be solved urgently and is also of great research value.

[0003] By adding a crosslinking agent, the cyano groups in the polyarylethernitrile chain are crosslinked into a ring to form a spatial network structure to improve the tensile strength and heat resistance of the polyarylethernitrile. However, the change in structure makes the film-forming property and toughness of the polyarylethernitrile worse, and the introduction of a crosslinking agent makes the synthesis process cumbersome, which is not conducive to industrial production. The toughness of the polyarylethernitrile can be improved by introducing a flexible fatty chain, but the introduction of a flexible structure will reduce the original mechanical strength and heat resistance of the polyarylethernitrile. Therefore, it is very necessary to synthesize a new polyarylethernitrile polymer with high strength, high toughness and high thermal stability. Summary of the invention

[0004] In view of the above problems existing in the prior art, the present invention provides a hydrogen-bond cross-linked high-performance polyarylene imine ether nitrile and a preparation method thereof. The prepared polyarylene imine ether nitrile has excellent film-forming property and toughness, as well as excellent mechanical properties, a high glass transition temperature and a high decomposition temperature. The preparation method is simple and suitable for industrial production.

[0005] To achieve the above object, the technical solution adopted by the present invention to solve the technical problem is: to provide a high-performance polyarylene imide ether nitrile cross-linked by hydrogen bonds, the structural formula of which is:

[0006]

[0007] in,

[0008] The method for preparing the hydrogen-bond cross-linked high-performance polyarylene imine ether nitrile comprises the following steps:

[0009] (1) adding a potassium carbonate catalyst to dihydroxydiphenylamine and 2,6'-difluorobenzonitrile monomers in a reactor to obtain a mixture; adding an organic solvent and toluene in a volume ratio of 10:1 to the reactor, and mixing the organic solvent with the mixture to obtain a mixed solution;

[0010] (2) heating the mixed solution obtained in step (1) to 140° C., distilling off toluene, then heating to 180-190° C. and reacting for 8-10 h, cooling to room temperature and then slowly adding to 500 mL of distilled water, filtering, and obtaining a solid;

[0011] (3) The solid obtained in step (2) is crushed, boiled and washed with distilled water for 2-3 times, extracted with 250 mL of methanol for 20-24 h, and dried to obtain a hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile.

[0012] Furthermore, in step (1), the molar ratio of dihydroxydiphenylamine, 2,6'-difluorobenzonitrile monomer and potassium carbonate is 1:1:2-4.

[0013] Furthermore, in step (1), the molar ratio of dihydroxydiphenylamine, 2,6'-difluorobenzonitrile monomer and potassium carbonate is 1:1:3.

[0014] Furthermore, the dihydroxydiphenylamine is 4,4'-dihydroxydiphenylamine or 3,3'-dihydroxydiphenylamine.

[0015] Furthermore, in step (1), the solid-liquid mass ratio of the mixture to the organic solvent is 1:7-9.

[0016] Furthermore, in step (1), the solid-liquid mass ratio of the mixture to the organic solvent is 1:8.

[0017] Furthermore, the organic solvent is N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide or sulfolane.

[0018] Furthermore, in step (3), vacuum drying is performed at 100° C. and 0.1 MPa for 10 h, or drying is performed at 100-150° C. for 24 h.

[0019] In summary, the present invention has the following advantages:

[0020] 1. The preparation process provided by the present invention is simple and has low preparation cost; the polyarylene imine ether nitrile polymer is prepared by a nucleophilic substitution polycondensation reaction by simply regulating the reaction temperature and the ratio of monomers.

[0021] 2. The structure of the polymer is regulated and modified by changing the structure of AR; high-strength films can be prepared by casting, and the films have good mechanical properties (tensile strength>110MPa, elongation at break>20%, glass transition temperature>190°C).

[0022] 3. The -H on the imine group and the -N on the cyano group on the molecular chain easily form hydrogen bond interactions, which increases the energy dissipation of the polymer and greatly improves the mechanical properties of the polymer.

[0023] 4. The benzene ring in the polymer main chain can effectively improve the rigidity of the polymer chain and give the polyaromatic imide ether nitrile a higher glass transition temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the H NMR spectrum of 4,4'-dihydroxydiphenylamine in Example 1;

[0025] Figure 2 This is the H NMR spectrum of the hydrogen-bonded cross-linked high-performance polyarylene imine ether nitrile (4-PIEN) obtained in Example 1;

[0026] Figure 3 Schematic diagram of hydrogen bonding in the hydrogen-bonded cross-linked high-performance polyarylene imine ether nitrile (4-PIEN) obtained in Example 1;

[0027] Figure 4 This is the H NMR spectrum of the hydrogen-bonded cross-linked high-performance polyarylene imine ether nitrile (3-PIEN) obtained in Example 2;

[0028] Figure 5 The Fourier transform infrared spectrum of the hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile obtained in Example 1-2;

[0029] Figure 6 The thermogravimetric curve of the hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile obtained in Example 1-2;

[0030] Figure 7 The differential scanning calorimetry curves of the polymers obtained in Examples 1-2 and Comparative Example 1 are shown;

[0031] Figure 8 This is a comparison chart of the mechanical properties of the polymers obtained in Examples 1-2 and Comparative Example 1 after being formed into thin films. DETAILED DESCRIPTION

[0032] Example 1

[0033] A hydrogen-bond cross-linked high-performance polyarylene imine ether nitrile, the preparation method of which comprises the following steps:

[0034] (1) Under nitrogen protection, 12 g of potassium carbonate catalyst was added to 6 g of 4,4'-dihydroxydiphenylamine and 4.1 g of 2,6'-difluorobenzonitrile monomer in a reactor to obtain a mixture; the molar ratio of 4,4'-dihydroxydiphenylamine, 2,6'-difluorobenzonitrile monomer and potassium carbonate was 1:1:3; 100 mL of N-methylpyrrolidone and 20 mL of toluene were added to the reactor and mixed with the mixture to obtain a mixed solution;

[0035] (2) heating the mixed solution obtained in step (1) to 140° C., distilling off toluene, then heating to 190° C. and reacting for 10 h, cooling to room temperature and slowly adding to 500 mL of distilled water, filtering to obtain a solid;

[0036] (3) The solid obtained in step (2) is crushed, boiled and washed twice with distilled water, extracted with 250 mL of methanol for 20-24 h, and dried at 65° C. to obtain a hydrogen-bonded cross-linked high-performance poly (aryl imine ether nitrile) (4-PIEN).

[0037] And the chemical reaction equation involved in the above preparation process is:

[0038]

[0039] The above 4,4'-dihydroxydiphenylamine is prepared by the following method:

[0040] Under nitrogen protection, 4,4'-dimethoxydiphenylamine is prepared into a dichloromethane solution of 4,4'-dimethoxydiphenylamine with a concentration of 0.4 mol / L, boron tribromide is prepared into a dichloromethane solution of boron tribromide with a concentration of 2 mol / L, the dichloromethane solution of boron tribromide is slowly added dropwise into the dichloromethane solution of 4,4'-dimethoxydiphenylamine, and the mixture is reacted at -80°C for 24 hours; the obtained crude product is extracted with distilled water, and after standing and stratification, the upper aqueous solution is collected, the pH of the aqueous solution is adjusted to precipitate 4,4'-dihydroxydiphenylamine monomer, and after filtration, the 4,4'-dihydroxydiphenylamine monomer is collected, and the 4,4'-dihydroxydiphenylamine monomer is recrystallized with toluene to obtain 4,4'-dihydroxydiphenylamine.

[0041] The NMR hydrogen spectra of 4,4'-dihydroxydiphenylamine and hydrogen-bonded cross-linked high-performance polyarylene imine ether nitrile (4-PIEN) prepared in this example are shown as follows: Figure 1-2 As shown in the figure, the schematic diagram of hydrogen bonding in hydrogen bond cross-linked high-performance poly (4-PIEN) is as follows Figure 3 shown.

[0042] Depend on Figure 1 It can be seen that the hydrogen atoms in each chemical environment of the compound correspond well to their chemical shifts, and their number is consistent with the peak area. From the analysis of the NMR spectrum, it can be seen that the target product 4,4'-dihydroxydiphenylamine can be obtained according to the experimental method of the present invention.

[0043] Depend on Figure 2It can be seen that the single peak between 8.4-8.5ppm is the characteristic peak of the imine group, the double peak between 7.4-7.5ppm is the characteristic absorption peak of the meta-position H atom on the benzene ring connected to the cyano group, the single peak between 6.4-6.5ppm is the characteristic absorption peak of the para-position H atom on the benzene ring connected to the cyano group, the double peak between 7.2-7.3ppm is the characteristic absorption peak of the four H atoms on the benzene ring connected to the imine group, and the double peak between 7.1-7.2ppm is the characteristic absorption peak of the four H atoms on the benzene ring connected to the ether bond, indicating that the structure of the prepared polymer is consistent with the theory. The present invention successfully prepares high-performance polyarylene imine ether nitrile (4-PIEN) cross-linked by hydrogen bonds.

[0044] Example 2

[0045] A hydrogen-bond cross-linked high-performance polyarylene imine ether nitrile, the preparation method of which comprises the following steps:

[0046] (1) Under nitrogen protection, 12 g of potassium carbonate catalyst was added to 6 g of 3,3'-dihydroxydiphenylamine and 4.1 g of 2,6'-difluorobenzonitrile monomer in a reactor to obtain a mixture; the molar ratio of 3,3'-dihydroxydiphenylamine, 2,6'-difluorobenzonitrile monomer and potassium carbonate was 1:1:3; 100 mL of N-methylpyrrolidone and 20 mL of toluene were added to the reactor and mixed with the mixture to obtain a mixed solution;

[0047] (2) heating the mixed solution obtained in step (1) to 140° C., distilling off toluene, then heating to 190° C. and reacting for 10 h, cooling to room temperature and slowly adding to 500 mL of distilled water, filtering to obtain a solid;

[0048] (3) The solid obtained in step (2) is crushed and washed twice with distilled water, then extracted with 250 mL of methanol for 20-24 h, and dried at 65° C. to obtain a hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile (3-PIEN).

[0049] And the chemical reaction equation involved in the above preparation process is:

[0050]

[0051] The hydrogen-bond cross-linked high-performance poly (arylene imine ether nitrile) (3-PIEN) prepared in this example has the following nuclear magnetic hydrogen spectra: Figure 4 shown.

[0052] Depend on Figure 4It can be seen that the single peak between 8.5-8.6ppm is the characteristic peak of the imine group, the single peak between 7.6-7.5ppm is the characteristic absorption peak of the para-position H atom on the benzene ring connected to the cyano group, the double peak between 7.4-7.2ppm is the characteristic absorption peak of the meta-position H atom on the benzene ring connected to the cyano group, the single peak between 7.1-7.0ppm is the characteristic absorption peak of the No. 1 H atom on the benzene ring connected to the imine group, the single peak between 6.8-6.7ppm is the characteristic absorption peak of the No. 4 H atom on the benzene ring connected to the imine group, the double peak between 6.7-6.6ppm is the characteristic absorption peak of the No. 3 H atom on the benzene ring connected to the imine group, and the double peak between 6.6-6.5ppm is the characteristic absorption peak of the No. 5 H atom on the benzene ring connected to the imine group, indicating that the structure of the prepared polymer is consistent with the theory. The present invention successfully prepares hydrogen-bonded cross-linked high-performance polyarylene imine ether nitrile (4-PIEN).

[0053] Comparative Example 1

[0054] Preparation of poly(arylene ether nitrile) polymers containing no imine groups:

[0055] According to the preparation method of Example 1, 4,4'-dihydroxydiphenylamine is replaced by 4,4'-dimethoxydiphenylamine, and other factors remain unchanged. The chemical reaction equation of the obtained polyarylethernitrile polymer (4-PEN) is:

[0056]

[0057] Experimental example

[0058] The Fourier transform infrared spectra and thermogravimetric curves of the hydrogen bond cross-linked high-performance poly (aryl imide ether nitrile) prepared in Examples 1 and 2 were obtained, and the results were as follows: Figure 5-6 shown.

[0059] Depend on Figure 5 It can be seen that at 3410cm -1 The peak at 2240cm is the characteristic peak of the skeleton vibration of the imine group -NH; -1 The peak at 1245cm is the characteristic peak of the skeleton vibration of cyano-CN; -1 and 853cm -1 The peak at is the stretching vibration peak of the ether bond COC, indicating that the main chain structure of the polymer synthesized in the present invention is consistent with the theory.

[0060] Depend on Figure 6 It can be seen that the thermal decomposition temperature of the polymer (T d 5%)>390℃, indicating that the polymer has a higher thermal decomposition temperature.

[0061] The polymers obtained in Examples 1-2 and Comparative Example 1 were used to prepare films respectively, and the specific steps were as follows: the polymer material was dissolved in N-methylpyrrolidone to prepare a polymer solution with a concentration of 5%, and impurities were removed by filtration, and then the solution was cast on a clean and flat glass plate, and dried in an oven at 80°C for 12 hours, and then vacuum dried at 80°C for 24 hours to obtain a polyarylethernitrile film. It can be seen that the polyarylethernitrile polymers obtained in Examples 1-2 all have excellent film-forming properties.

[0062] The performance parameters of the polymers obtained in Examples 1-2 and Comparative Example 1 are shown in Table 1. The differential scanning calorimetry curves of the polymers obtained in Examples 1-2 and Comparative Example 1 and the mechanical properties comparison diagrams after film formation are shown in Table 1. Figure 7-8 shown.

[0063] Table 1 Performance parameters of the polymers obtained in Examples 1-2 and Comparative Example 1

[0064] Example 1 Example 2 Comparative Example 1 Tensile strength(MPa) 135 110 84 Elongation at break (%) 31 22 10 Glass transition temperature(℃) 203 198 153

[0065] Depend on Figure 7 It can be seen that the glass transition temperature (Tg) of the polyarylethernitrile polymer obtained in Example 1-2 is greater than 190°C, which is better than the glass transition temperature of 150°C of the polyarylethernitrile polymer obtained in Comparative Example 1, indicating that the polymer has a higher glass transition temperature and meets the high temperature processing requirements.

[0066] Depend on Figure 8 It can be seen that the polyarylethernitrile film obtained in Example 1-2 has good mechanical properties, with a tensile strength of >110 MPa and an elongation at break of >20%. Its strength and toughness are better than the polyarylethernitrile film obtained in Comparative Example 1.

[0067] From Table 1 and Figure 7-8 It can be seen that compared with polyarylethernitrile polymers, hydrogen bonds in polyimine ether nitrile polymers with hydrogen bond interactions make the polymer molecular chains more tightly entangled, making the movement of the molecular chains more difficult, resulting in the glass transition temperature of polyarylethernitrile being higher than that of polymethylene arylethernitrile; the breaking of hydrogen bonds under the action of external forces will also dissipate a portion of energy accordingly, and compared with polyarylethernitrile, polyarylethernitrile has higher tensile strength and fracture toughness. In summary, the polyimine arylethernitrile prepared by the present invention has excellent mechanical properties and thermal properties.

[0068] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A high-performance hydrogen-bonded cross-linked polyarylene imide ether nitrile, characterized in that: Its structural formula is: ; in, ; The preparation method of the hydrogen-bond cross-linked high-performance polyarylene imine ether nitrile comprises the following steps: (1) adding a potassium carbonate catalyst to dihydroxydiphenylamine and 2,6'-difluorobenzonitrile monomers in a reactor to obtain a mixture; adding an organic solvent and toluene in a volume ratio of 10:1 to the reactor and mixing the mixture to obtain a mixed solution; the molar ratio of dihydroxydiphenylamine, 2,6'-difluorobenzonitrile monomer and potassium carbonate is 1:1:2-4; the dihydroxydiphenylamine is 4,4'-dihydroxydiphenylamine; (2) heating the mixed solution obtained in step (1) to 140°C, distilling off toluene, then heating to 180-190°C for reaction for 8-10 hours, cooling to room temperature, adding to 500 mL of distilled water, filtering, and obtaining a solid; (3) The solid obtained in step (2) is crushed, boiled and washed with distilled water for 2-3 times, extracted with 250 mL of methanol for 20-24 h, and dried to obtain a hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile.

2. The hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile according to claim 1, characterized in that: In step (1), the molar ratio of dihydroxydiphenylamine, 2,6'-difluorobenzonitrile monomer and potassium carbonate is 1:1:

3.

3. The hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile according to claim 1, characterized in that: In step (1), the solid-liquid mass ratio of the mixture to the organic solvent is 1:7-9.

4. The hydrogen-bonded cross-linked high-performance polyarylimine ether nitrile according to claim 1 or 3, characterized in that: In step (1), the solid-liquid mass ratio of the mixture to the organic solvent is 1:

8.

5. The hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile according to claim 1, characterized in that: The organic solvent is N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide or sulfolane.

6. The hydrogen-bonded cross-linked high-performance polyarylene imide ether nitrile according to claim 1, characterized in that: In step (3), vacuum drying is performed at 100° C. and 0.1 MPa for 10 h, or drying is performed at 100-150° C. for 24 h.

Citation Information

Patent Citations

  • Aromatic polyether and method for producing the same

    JP1993310914A