A tool, TiB x Coating and its preparation method and application

Through high-power pulse magnetron sputtering and ion source-assisted deposition, the stoichiometric ratio of the TiBx coating is adjusted to solve the problems of high residual stress and poor toughness of the existing TiB2 coating, and a nanostructure with high hardness and high toughness is prepared. TiBx coating, suitable for metal surface treatment and processing.

CN115612996BActive Publication Date: 2024-10-18XIAMEN GOLDEN EGRET SPECIAL ALLOY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211153811.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2024-10-18
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

The existing TiB2 coating deposited by magnetron sputtering often exhibits a columnar crystal structure and exceeds the stoichiometric ratio, resulting in problems of large residual stress and poor toughness.

Method used

Using high-power pulse magnetron sputtering TiB2 target and turning on the ion source to assist deposition, adjusting the stoichiometric ratio of the TiBx coating, and controlling the deposition conditions in an Ar atmosphere, a nanostructured TiBx coating was prepared.

Benefits of technology

The TiBx coating has excellent properties of dense structure, high hardness, high toughness and low stress, making it suitable for metal surface treatment and metal processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115612996B_ABST
    Figure CN115612996B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of tool coatings, and in particular to a tool, a TiBx coating, and a preparation method and application thereof. x The coating preparation method comprises the following steps: depositing TiB on the substrate x Coating: In Ar atmosphere, high power pulse magnetron sputtering TiB2 target material, while turning on ion source to assist deposition, TiB x The coating is deposited on the substrate surface to prepare TiB x The TiB x The coating preparation method is to use high power pulsed magnetron sputtering TiB2 target material, while Ar + Ion source assisted deposition of TiB x TiB coating can be achieved through simple process and operation x The atomic ratio of B / Ti in the coating can be controlled to obtain TiB x The coating has excellent properties of dense structure, high hardness, high toughness and low stress, making the TiB x Coatings can be widely used in metal surface treatment or metal processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of tool coatings, and in particular to a tool, a TiBx coating, and a preparation method and application thereof. Background Art

[0002] Titanium diboride (TiB2) is one of the hard coatings applied to the surface of cutting tools, and it has broad application prospects in improving the functionality and service life of cutting tools. TiB2 coating has excellent mechanical and chemical properties such as high melting point (about 3100℃), good thermal conductivity and electrical conductivity, high hardness, high wear resistance and corrosion resistance.

[0003] Among the existing coating deposition methods, magnetron sputtering is often used to sputter TiB2 targets in an Ar gas environment to prepare TiB2 coatings due to its high film surface quality and wide target material applicability. However, in the existing magnetron sputtering TiB2 coating deposition process, TiB2 often presents a columnar crystal structure and is overstoichiometric, and the excess B is easily segregated at the grain boundaries, resulting in the TiB2 coating having the disadvantages of large residual stress and poor toughness. Summary of the invention

[0004] To solve the shortcomings of the existing solutions mentioned in the background technology: magnetron sputtering deposited TiB2 coatings often present a columnar crystal structure, and the excess B is easily segregated at the grain boundaries, resulting in large residual stress and poor toughness of the TiB2 coating. x Coating preparation method, the preparation method can controllably adjust TiB x The coating stoichiometry comprises the following steps:

[0005] Deposition of TiB on substrate x Coating: In Ar atmosphere, high power pulse magnetron sputtering (HiPIMS) TiB2 target material is used, and ion source is turned on to assist deposition, so that TiB x The coating is deposited on the substrate surface to prepare TiB x coating.

[0006] In one embodiment, during the high-power pulsed magnetron sputtering of the TiB2 target, the target peak current density of the TiB2 target is greater than or equal to 0.5 A / cm 2 And less than or equal to 0.8A / cm 2 .

[0007] In one embodiment, during the high-power pulsed magnetron sputtering of the TiB2 target, the average sputtering power of the TiB2 target is greater than or equal to 5 W / cm 2And less than or equal to 10W / cm 2 , and its deposition bias is greater than or equal to -30V and less than or equal to -150V;

[0008] The operating current of the ion source is greater than 0A and less than or equal to 20A.

[0009] In one embodiment, the pressure of the Ar atmosphere is greater than or equal to 0.2Pa and less than or equal to 0.8Pa.

[0010] In one embodiment, it is characterized in that: TiB is deposited on the substrate x Before the coating step, a substrate pretreatment step is performed; the substrate pretreatment step includes at least one of mechanical grinding, polishing, and cleaning.

[0011] In one embodiment, the cleaning includes at least one of solvent cleaning, glow cleaning, and ion etching cleaning.

[0012] The present application provides a TiB x coating, the TiB x The coating is a nanostructured coating, the grain size of which is greater than or equal to 5 nm and less than or equal to 30 nm, and the TiB x The atomic ratio of the B element to the Ti element in the coating is greater than or equal to 1.8 and less than or equal to 2.5, that is, the TiB x The coating component content atomic ratio B / Ti is greater than or equal to 1.8 and less than or equal to 2.3.

[0013] In one embodiment, the TiB x The hardness of the coating is greater than or equal to 32 GPa and less than or equal to 36 GPa, and the elastic modulus is greater than or equal to 370 GPa and less than or equal to 475 GPa. x The residual compressive stress of the coating is greater than or equal to -2.5 GPa and less than or equal to -3.3 GPa.

[0014] The present application also provides a TiB x Application of coating in metal surface treatment or metal processing; the TiB x The coating is TiB as described above x coating or TiB as above x TiB prepared by the coating preparation method x coating.

[0015] The present application also provides a tool, wherein TiB is deposited on the surface of the tool. x coating; the TiB x The coating is TiB as described above x coating or TiB as abovex TiB prepared by the coating preparation method x coating.

[0016] A TiB provided by this application x Compared with the existing technology, the coating preparation method has the following beneficial effects:

[0017] The TiB provided in this application x Coating preparation method, which can controllably adjust TiB x The coating stoichiometric ratio is obtained by high power pulsed magnetron sputtering of TiB2 target and Ar + Ion source assisted deposition of TiB x TiB coating can be achieved through simple process and operation x The atomic ratio of B / Ti in the coating can be controlled to obtain TiB x The coating has excellent properties of dense structure, high hardness, high toughness and low stress, making the TiB x Coatings can be widely used in metal surface treatment or metal processing.

[0018] Other features and beneficial effects of the present application will be described in the subsequent description, and partly become apparent from the description, or be understood by practicing the present application. The purpose and other beneficial effects of the present application can be realized and obtained by the structures and / or components indicated in the description. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the existing solutions, the drawings required for use in the description of the embodiments or the existing solutions will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0020] Figure 1 Preparation of TiB for ion-assisted deposition x Schematic diagram of the coating scheme and the schematic diagram of the Booster ion source structure;

[0021] Figure 2 TiB prepared in Comparative Example 1 and Examples 1-5 under different ion source currents x Coating component content B / Ti atomic ratio;

[0022] Figure 3 TiB prepared in Comparative Example 1 and Examples 1-5 x Coating XRD (X-ray diffraction) pattern;

[0023] Figure 4 TiB prepared in Comparative Example 1 and Examples 1-4 x SEM (scanning electron microscope) surface and cross-sectional morphology of the coating;

[0024] Figure 5 TiB prepared in Comparative Example 1 and Examples 1-5 x Nanohardness data of coating;

[0025] Figure 6 TiB prepared in Comparative Example 1 and Examples 1-5 x Coating elastic modulus data graph;

[0026] Figure 7 TiB prepared in Comparative Example 1 and Examples 1-5 x Coating residual stress data graph.

[0027] Reference numerals:

[0028] DETAILED DESCRIPTION

[0029] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0030] The present application provides a TiB x The coating preparation method comprises the following steps:

[0031] (1) TiB is deposited on the substrate 50 x Before the coating step, a pretreatment step of the substrate 50 is performed; wherein the pretreatment step of the substrate 50 can be selected from at least one of mechanical grinding, polishing, and cleaning. Furthermore, the cleaning can be selected from at least one of solvent cleaning, glow cleaning, and ion etching cleaning.

[0032] (2) Depositing TiB on the substrate 50 x Coating: In Ar atmosphere, high power pulse magnetron sputtering TiB2 target 40, while turning on ion source 10 to assist deposition, TiB x The coating is deposited on the surface of the substrate 50 to prepare TiB x coating.

[0033] Specific operations such as Figure 1As shown, TiB was prepared in pure Ar atmosphere. x coating:

[0034] During the coating deposition process, when Ar is introduced into the vacuum chamber 30, the pressure of the deposition chamber is adjusted to be greater than or equal to 0.2 Pa and less than or equal to 0.8 Pa; the substrate 50 is mounted on the sample rotating rack 20, and then the TiB2 target 40 is sputtered by high-power pulsed magnetron sputtering, and the average sputtering power of the TiB2 target 40 is greater than or equal to 5 W / cm 2 And less than or equal to 10W / cm 2 The target peak current density of the TiB2 target material 40 is greater than or equal to 0.5A / cm 2 And less than or equal to 0.8A / cm 2 , and its deposition bias voltage is greater than or equal to -30V and less than or equal to -150V, and the ion source 10 is turned on, and its working current is set to be greater than 0A and less than or equal to 20A, in TiB x During the coating deposition, the sample holder drives the substrate 50 to rotate and revolve, so that TiB is deposited on the surface of the substrate 50. x coating.

[0035] Among them, the ion source 10 used in the present application scheme can be used as follows Figure 1 The Booster ion source 10 shown includes components such as a copper cover 11, a tantalum tube 12 and an air pipe 13. The ion source 10 is an existing device, and the structural structure, connection relationship and working principle of its various components are no longer repeated here. According to the concept of this application, technical personnel in this field can make adaptive selections in the existing Booster ion source 10 according to needs.

[0036] The TiB provided by the present application as described above x The coating preparation method includes at least the following design principles and inventive concepts:

[0037] In the existing TiB x In the coating preparation scheme, magnetron sputtering deposited TiB2 coating often presents a columnar crystal structure and is an overstoichiometric ratio. Excess B is easily segregated at the grain boundaries, resulting in the TiB2 coating having the disadvantages of large residual stress and poor toughness. The study found that the B content in the coating can be reduced by increasing the working distance between the substrate 50 and the target 40 or increasing the deposition pressure, but it will cause problems such as a reduced coating deposition rate and reduced coating density. A reduced coating deposition rate will lead to a reduced coating thickness, and a reduced coating density will lead to a reduced coating toughness and high-temperature oxidation resistance. All three of these factors reduce the wear resistance of the coating. In addition, the existing solution research also proposes: by applying an external magnetic field between the substrate 50 and the target 40 to reduce the TiB xThe stoichiometric ratio method, however, involves equipment magnetic field modification, plasma motion simulation, etc., and its practical application is relatively complex and difficult, and its application is limited;

[0038] Based on this, this application provides the TiB x The coating preparation method comprises the following steps: a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, and an Ar + Ion source 10 assisted deposition of TiB x TiB coating can be achieved through simple process and operation x The atomic ratio of B / Ti in the coating can be controlled to obtain TiB x The coating has excellent properties of dense structure, high hardness, high toughness and low stress, thus solving the problem of TiB x The coating has problems such as large residual stress, poor toughness and poor density, and its process operation is simple and easy to achieve.

[0039] The present invention adopts high power pulse magnetron sputtering to form a TiB2 target 40. + Ion source 10 assisted deposition of TiB x The mechanism of coating to achieve the desired effect is as follows: 1) Ar + Ion source 10 assisted deposition can improve the density of the prepared coating; 2) Ar + Ion bombardment can preferentially sputter and remove B+ in the coating deposition particle source, thereby reducing the B content in the coating. + The size of the ion beam current (ion source 10 current) can achieve the TiB x The controllable adjustment of the coating stoichiometric ratio can produce TiB with dense structure, high hardness, high toughness and low stress. x coating.

[0040] In addition, the present application also provides the following examples and comparative examples to verify the beneficial effects of the present application:

[0041] Comparative Example 1

[0042] In this example, TiB x The steps for preparing the coating are as follows:

[0043] 1. Substrate 50 pretreatment

[0044] (1) First, the substrate 50 is mechanically ground with sandpaper, then the surface of the substrate 50 is polished with a polishing liquid, and finally cleaned; wherein the substrate 50 is specifically a cemented carbide.

[0045] (2) Solvent cleaning: First use deionized water for ultrasonic cleaning for 30 minutes, and then use 98% alcohol solution for ultrasonic cleaning for 15 minutes.

[0046] (3) Glow cleaning treatment: The substrate 50 is cleaned for 20 minutes by glow discharge in an Ar atmosphere, with a working pressure of 0.35 Pa; the bias voltage of the substrate 50 is -650 V, and the frequency is 240 kHz.

[0047] (4) Ion etching treatment: cleaning for 20 minutes, ambient pressure is 0.32Pa; substrate bias is -200V.

[0048] 2. High power pulsed magnetron sputtering of TiB2 target 40, while turning on the Booster ion source 10 to assist in the preparation of TiB x coating:

[0049] Preparation of TiB in pure Ar atmosphere x During the coating deposition process, when Ar is introduced, the pressure of the deposition chamber, i.e., the vacuum chamber 30, is adjusted to 0.4 Pa, and a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, with an average sputtering power of 5 W / cm 2 、TiB2 target 40 target peak current density 0.5A / cm 2 , deposition bias -60V; at the same time, turn on the Booster ion source 10, set the current to 0A, the sample holder drives the substrate 50 to rotate and revolve (rotation speed 2rpm (rpm: rounds per minute, revolutions per minute), revolution speed 1.5 rpm, deposition time 2h (i.e., high-power pulsed magnetron sputtering TiB2 target 40 and Booster ion source 10 working time, unit hour), and deposit TiB x coating.

[0050] Example 1

[0051] In this example, TiB x The steps for preparing the coating are as follows:

[0052] 1. Pretreatment of substrate 50: The pretreatment steps of substrate 50 are the same as those in Comparative Example 1.

[0053] 2. High power pulsed magnetron sputtering of TiB2 target 40, while turning on the Booster ion source 10 to assist in the preparation of TiB x coating:

[0054] Preparation of TiB in pure Ar atmosphere x During the coating deposition process, when Ar is introduced, the pressure of the deposition chamber, i.e., the vacuum chamber 30, is adjusted to 0.4 Pa, and a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, with an average sputtering power of 5 W / cm 2 、TiB2 target 40 target peak current density 0.5A / cm 2, deposition bias voltage -60V; at the same time, turn on the Booster ion source 10, set the current to 2A, the sample holder drives the substrate 50 to rotate and revolve (rotation speed 2rpm (rpm: rounds per minute, revolutions per minute), revolution speed 1.5 rpm, deposition time 2h (i.e., high-power pulsed magnetron sputtering TiB2 target 40 and Booster ion source 10 working time, unit hour), deposited TiB x coating.

[0055] Example 2

[0056] In this example, TiB x The steps for preparing the coating are as follows:

[0057] 1. Pretreatment of substrate 50: The pretreatment steps of substrate 50 are the same as those in Example 1.

[0058] 2. High power pulsed magnetron sputtering of TiB2 target 40, while turning on the Booster ion source 10 to assist in the preparation of TiB x coating:

[0059] Preparation of TiB in pure Ar atmosphere x During the coating deposition process, when Ar is introduced, the pressure of the deposition chamber, i.e., the vacuum chamber 30, is adjusted to 0.4 Pa, and a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, with an average sputtering power of 5 W / cm 2 、TiB2 target 40 target peak current density 0.5A / cm 2 , deposition bias -60V; at the same time, turn on the Booster ion source 10, set the current to 5A, the sample holder drives the substrate 50 to rotate and revolve (rotation speed 2rpm (rpm: rounds per minute, revolutions per minute), revolution speed 1.5 rpm, deposition time 2h (i.e., high-power pulsed magnetron sputtering TiB2 target 40 and Booster ion source 10 working time, unit hour), deposited TiB x coating.

[0060] Example 3

[0061] In this example, TiB x The steps for preparing the coating are as follows:

[0062] 1. Pretreatment of substrate 50: The pretreatment steps of substrate 50 are the same as those in Example 1.

[0063] 2. High power pulsed magnetron sputtering of TiB2 target 40, while turning on the Booster ion source 10 to assist in the preparation of TiB x coating:

[0064] Preparation of TiB in pure Ar atmosphere x During the coating deposition process, when Ar is introduced, the pressure of the deposition chamber, i.e., the vacuum chamber 30, is adjusted to 0.4 Pa, and a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, with an average sputtering power of 5 W / cm 2 、TiB2 target 40 target peak current density 0.5A / cm 2 , deposition bias -60V; at the same time, turn on the Booster ion source 10, set the current to 10A, the sample holder drives the substrate 50 to rotate and revolve (rotation speed 2rpm (rpm: rounds per minute, revolutions per minute), revolution speed 1.5 rpm, deposition time 2h (i.e., high-power pulsed magnetron sputtering TiB2 target 40 and Booster ion source 10 working time, unit hour), deposited TiB x coating.

[0065] Example 4

[0066] In this example, TiB x The steps for preparing the coating are as follows:

[0067] 1. Pretreatment of substrate 50: The pretreatment steps of substrate 50 are the same as those in Example 1.

[0068] 2. High power pulsed magnetron sputtering of TiB2 target 40, while turning on the Booster ion source 10 to assist in the preparation of TiB x coating:

[0069] Preparation of TiB in pure Ar atmosphere x During the coating deposition process, when Ar is introduced, the pressure of the deposition chamber, i.e., the vacuum chamber 30, is adjusted to 0.4 Pa, and a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, with an average sputtering power of 5 W / cm 2 、TiB2 target 40 target peak current density 0.5A / cm 2 , deposition bias -60V; at the same time, turn on the Booster ion source 10, set the current to 15A, the sample holder drives the substrate 50 to rotate and revolve (rotation speed 2rpm (rpm: rounds per minute, revolutions per minute), revolution speed 1.5 rpm, deposition time 2h (i.e., high-power pulsed magnetron sputtering TiB2 target 40 and Booster ion source 10 working time, unit hour), deposited TiB x coating.

[0070] Example 5

[0071] In this example, TiB xThe steps for preparing the coating are as follows:

[0072] 1. Pretreatment of substrate 50: The pretreatment steps of substrate 50 are the same as those in Example 1.

[0073] 2. High power pulsed magnetron sputtering of TiB2 target 40, while turning on the Booster ion source 10 to assist in the preparation of TiB x coating:

[0074] Preparation of TiB in pure Ar atmosphere x During the coating deposition process, when Ar is introduced, the pressure of the deposition chamber, i.e., the vacuum chamber 30, is adjusted to 0.4 Pa, and a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, with an average sputtering power of 5 W / cm 2 、TiB2 target 40 target peak current density 0.5A / cm 2 , deposition bias -60V; at the same time, turn on the Booster ion source 10, set the current to 20A, the sample holder drives the substrate 50 to rotate and revolve (rotation speed 2rpm (rpm: rounds per minute, revolutions per minute), revolution speed 1.5 rpm, deposition time 2h (i.e., high-power pulsed magnetron sputtering TiB2 target 40 and Booster ion source 10 working time, unit hour), deposited TiB x coating.

[0075] The coatings prepared in the examples and comparative examples were tested for performance, and the specific performance data are shown in Table 1 below:

[0076] Table 1

[0077]

[0078] Combined with the contents of Table 1 and Figure 2-6 The content shows:

[0079] 1. TiB x Coating element content and mechanical properties test

[0080] XPS is used to test the content of coating elements. Figure 2 TiB prepared in Comparative Example 1 and Examples 1-5 x Coating component content diagram, TiB of Comparative Example 1 x The atomic ratio of the coating components B / Ti is 2.5. The TiB x The atomic ratio of coating components B / Ti is 1.8-2.3. Figure 4 It can be seen that TiB in Examples 1-4 x The average grain size in the coating is greater than or equal to 5 nm and less than or equal to 30 nm. Figure 4 The cross section of the coating shows that the compactness of the coating of Comparative Example 1 is significantly poorer than that of the embodiment. The hardness and elastic modulus of the coating are characterized by a nanoindenter. The test method and steps are performed according to the international standard ISO-14577. Figure 5 TiB prepared in Comparative Example 1 and Examples 1-5 x Coating hardness diagram, Figure 5 The TiB of Comparative Example 1 is shown x The coating hardness is 37.8 GPa, and the TiB x The coating hardness ranges from 33.1 to 35.5 GPa, indicating that the TiB prepared in the embodiment x The coating has high hardness and good mechanical properties and can meet the requirements of use.

[0081] Figure 6 TiB prepared in Comparative Example 1 and Examples 1-5 x Coating elastic modulus diagram, Figure 6 The TiB of Comparative Example 1 is shown x The elastic modulus of the coating is 483 GPa. x The elastic modulus of the coating is in the range of 372 to 475 GPa. Compared with the embodiment, the elastic modulus of the coating of comparative example 1 is larger, indicating that it is brittle. The brittleness of the coating has an adverse effect on the cutting performance of the tool coated with the coating. It can be seen that the TiB prepared in this application x The coating has good toughness and excellent mechanical properties.

[0082] A thin film stress meter is used to characterize the residual stress of the coating, and the test substrate used is a stainless steel stress sheet. Figure 7 TiB prepared in Comparative Example 1 and Examples 1-5 x Coating residual stress diagram, Figure 7 The residual compressive stress of the coating in Comparative Example 1 is -3.8 GPa, and the residual compressive stress of the coating in Examples 1-5 is -3.8 GPa. x The residual compressive stress of the coating ranges from -2.5 to -3.3 GPa, and the residual stress is relatively low (the absolute value is relatively small); compared with the embodiment, the residual stress of comparative example 1 is relatively large (the absolute value is relatively large), which will also have an adverse effect on the cutting performance of the tool coated with the coating.

[0083] In summary, compared with the embodiment, although the coating prepared in comparative example 1 has a higher hardness, it is brittle, the structural density of the coating is poor, and the residual stress is large (the absolute value is large), which affects its performance during application.

[0084] 2. Analysis of the test results of the embodiment shows that:

[0085] Figure 2TiB prepared in Comparative Example 1 and Examples 1-5 under different ion source currents x The atomic ratio of the coating component content is B / Ti. It can be seen from the figure that increasing the ion source current by 10 can reduce the coating stoichiometric ratio, that is, the atomic ratio B / Ti.

[0086] Figure 3 TiB prepared in Comparative Example 1 and Examples 1-5 x The XRD spectrum of the coating shows that increasing the ion source current by 10 can reduce the stoichiometric ratio of the coating, resulting in TiB x The characteristic diffraction peak shifts to the right, TiB x The right shift of the characteristic diffraction peak indicates that the out-of-plane interplanar spacing of the coating is reduced, and the out-of-plane lattice constant of the crystal is smaller than that of TiB2. x It is characterized by a substoichiometric ratio, that is, x is less than 2.

[0087] In summary:

[0088] TiB provided by this application x The coating preparation method comprises the following steps: a TiB2 target material 40 is sputtered by high-power pulsed magnetron sputtering, and an Ar + Ion source 10 assisted deposition of TiB x TiB coating can be achieved through simple process and operation x The TiB x The coating is a nanostructured coating, the grain size of which is greater than or equal to 5 nm and less than or equal to 30 nm, and the TiB x The atomic ratio of the B element to the Ti element in the coating is greater than or equal to 1.8 and less than or equal to 2.3;

[0089] TiB prepared by the present application scheme x The coating has excellent properties of dense structure, high hardness, high toughness and low stress. x The hardness of the coating is greater than or equal to 32 GPa and less than or equal to 36 GPa, and the elastic modulus is greater than or equal to 370 GPa and less than or equal to 475 GPa. x The residual compressive stress of the coating is greater than or equal to -2.5 GPa and less than or equal to -3.3 GPa, so that the TiB x Coatings can be widely used in metal surface treatment or metal processing.

[0090] It should be noted that:

[0091] In this article, “~” is used to indicate a numerical range, and the range indicated by this expression includes two endpoint values.

[0092] The substrate 50 material used in the embodiment and the comparative example is cemented carbide. According to the above design concept, the TiB provided in this application x TiB prepared by coating preparation method x The coating can be applied to metal surface treatment and metal processing, including metal tool surface protection, etc. Therefore, it is not only applicable to the substrate 50 material in the embodiment, but also applicable to various metal substrates 50 materials, such as substrates 50 materials such as cemented carbide, steel, titanium alloy, etc., including but not limited to the embodiment scheme.

[0093] In the embodiments provided in this application, Figure 1 The ion source 10 shown in the figure assists the deposition of TiB x The coating device is prepared. According to the above-mentioned inventive concept, during the actual implementation, the arrangement of the ion source 10, the number and position of the TiB2 target material 40, the number of workstations of the substrate 50 in the sample holder, the revolution speed and rotation speed of the sample holder can all be adaptively adjusted according to actual needs, including but not limited to the embodiment scheme.

[0094] “Booster ion source 10 ” is a common expression for a booster ion source 10 or an auxiliary ion source 10 in the art.

[0095] In summary, the specific parameters or some commonly used reagents or raw materials in the above embodiments are specific embodiments or preferred embodiments of the present application, but are not intended to limit the present application. Those skilled in the art may make adaptive adjustments within the scope of the present application.

[0096] In addition, unless otherwise specified, the raw materials used may also be conventional commercial products in the art, or prepared by conventional methods in the art; that is, the reagents and instruments used in this embodiment are not indicated with information such as the manufacturer, and are all conventional products that can be purchased on the market.

[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A TiB x The coating preparation method is characterized in that: The following steps are involved: Deposition of TiB on substrate x Coating: In Ar atmosphere, high-power pulsed magnetron sputtering of TiB2 target material, while Booster-type ion source assisted deposition, makes TiB x The coating is deposited on the substrate surface to prepare TiB x Coating; During the high-power pulsed magnetron sputtering of the TiB2 target, the target peak current density of the TiB2 target is greater than or equal to 0.5A / cm 2 And less than or equal to 0.8A / cm 2 The average sputtering power of the TiB2 target is greater than or equal to 5W / cm 2 And less than or equal to 10W / cm 2 , and its deposition bias is greater than or equal to -30V and less than or equal to -150V; The operating current of the ion source is greater than 0A and less than or equal to 20A.

2. The TiB according to claim 1 x The coating preparation method is characterized by: The pressure of the Ar atmosphere is greater than or equal to 0.2 Pa and less than or equal to 0.8 Pa.

3. The TiB according to claim 1 x The coating preparation method is characterized by: TiB is deposited on the substrate x Before the coating step, a substrate pretreatment step is performed; the substrate pretreatment step includes at least one of mechanical grinding, polishing, and cleaning.

4. TiB according to claim 3 x The coating preparation method is characterized by: The cleaning includes at least one of solvent cleaning, glow cleaning, and ion etching cleaning.

5. A TiB x The coating is characterized in that :TiB x The coating is a nanostructured coating, the grain size of which is greater than or equal to 5 nm and less than or equal to 30 nm, and the TiB x The atomic ratio of the B element to the Ti element in the coating is greater than or equal to 1.8 and less than or equal to 2.3; The TiB x The coating is prepared by the preparation method according to any one of claims 1 to 4.

6. TiB according to claim 5 x A coating, characterized in that: The TiB x The hardness of the coating is greater than or equal to 32 GPa and less than or equal to 36 GPa, and the elastic modulus is greater than or equal to 370 GPa and less than or equal to 475 GPa. x The residual compressive stress of the coating is greater than or equal to -2.5 GPa and less than or equal to -3.3 GPa.

7. A TiB x Application of coating in metal surface treatment or metal processing; its characteristics are: The TiB x The coating adopts TiB as described in any one of claims 5-6 x Coating or TiB according to any one of claims 1 to 4 x TiB prepared by the coating preparation method x coating.

8. A cutting tool, characterized in that: TiB is deposited on the surface of the tool x coating; The TiB x The coating adopts TiB as described in any one of claims 5-6 x Coating or TiB according to any one of claims 1 to 4 x TiB prepared by the coating preparation method x coating.