Aluminum germanium silicate molecular sieve SSZ-121, its synthesis and use
By using 1,3-bis(1-adamantyl)imidazolium cation and FAU framework zeolite to form SSZ-121 molecular sieve, and removing the structure directing agent through heat treatment, the existing aluminum germanium silicate molecular sieve catalytic activity and Solving the problem of insufficient stability, it achieves efficient catalysis and compressive strength under high temperature and high pressure conditions, and is suitable for a variety of organic compound transformation reactions.
Patent Information
- Application Number
- CN202180038564.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-28
- Filing Date
- 2021-04-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-04-21
AI Technical Summary
Existing aluminum germanium silicate molecular sieves have problems with insufficient catalytic activity and stability during the conversion reaction and adsorption process of organic compounds. In particular, the catalyst is easy to decompose under high temperature and high pressure conditions, affecting industrial applications.
1,3-bis(1-adamantyl)imidazolium cation is used as the structure directing agent, and a reaction mixture is formed with FAU framework zeolite, germanium source, fluoride ion source and water, and is crystallized and heat treated to form SSZ-121 molecular sieve. And by compounding with other catalysts or materials to improve its compressive strength and catalytic performance.
The high-efficiency catalytic performance of SSZ-121 molecular sieve in the conversion reaction of organic compounds is achieved, and the structural directing agent is removed through heat treatment, which improves its stability and compressive strength under high temperature and high pressure conditions, and is suitable for a variety of commercially important organic compounds. transformation process.
Smart Images

Figure CN115667143B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of U.S. Provisional Application Serial No. 63 / 030,982, filed on May 27, 2020. Technical Field
[0003] The present disclosure relates to a novel synthetic crystalline aluminogermanosilicate molecular sieve named SSZ-121, its synthesis and its use in organic compound conversion reactions and adsorption processes. Background Art
[0004] Molecular sieves are a class of commercially important materials having distinct crystal structures with defined pore structures as shown by distinct X-ray diffraction patterns and having specific chemical compositions. The crystal structure defines cavities and pores that are unique to a particular type of molecular sieve.
[0005] According to the present disclosure, a new crystalline aluminogermanosilicate molecular sieve, designated SSZ-121 and having a unique powder X-ray diffraction pattern, has been synthesized using 1,3-bis(1-adamantyl)imidazolium cation as a structure directing agent. Summary of the invention
[0006] In a first aspect, a molecular sieve is provided which, in its as-synthesized form, has a powder X-ray diffraction pattern having at least the following 2-theta scattering angles: 6.3±0.2, 7.0±0.2, 9.5±0.2, 13.0±0.2, 16.0±0.2, 18.5±0.2, 19.8±0.2, 21.2±0.2, 24.0±0.2, 25.0±0.2, 26.5±0.2, 28.5±0.2 and 30.0±0.2 degrees 2-theta.
[0007] In their as-synthesized and anhydrous form, molecular sieves may have a chemical composition including the following molar relationships:
[0008] Widest Secondary <![CDATA[(SiO2+GeO2) / Al2O3]]> ≥30 ≥50 <![CDATA[Q / (SiO2+GeO2)]]> >0 to 0.1 >0 to 0.1
[0009] wherein Q comprises a 1,3-bis(1-adamantyl)imidazolium cation.
[0010] In a second aspect, a molecular sieve is provided, wherein in its calcined form, the powder XRD pattern has at least the following 2-θ scattering angles: 6.5±0.2, 9.5±0.2, 13.0±0.2, 18.5±0.2, 19.8±0.2, 21.2±0.2, 24.0±0.2, 25.0±0.2, 26.5±0.2, 28.5±0.2 and 30.0±0.2 degrees 2-θ.
[0011] In its calcined form, the molecular sieve may have a chemical composition comprising the following molar relationship:
[0012] Al2O3:(n)(SiO2+GeO2)
[0013] Where n≥30.
[0014] In a third aspect, a method for synthesizing the molecular sieve described herein is provided, the method comprising (1) preparing a reaction mixture comprising: (a) a FAU framework-type zeolite; (b) a germanium source; (c) a structure directing agent (Q) comprising a 1,3-bis(1-adamantyl)imidazolium cation; (d) a fluoride ion source; and (e) water; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form molecular sieve crystals.
[0015] In a fourth aspect, a process is provided for converting a feedstock comprising an organic compound to a conversion product, the process comprising contacting the feedstock with a catalyst comprising a molecular sieve described herein under organic compound conversion conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The powder X-ray diffraction (XRD) pattern of the molecular sieve as synthesized in Example 1 is shown.
[0017] Figure 2 A scanning electron microscope (SEM) image of the as-synthesized molecular sieve of Example 1 is shown.
[0018] Figure 3 The powder XRD pattern of the ozone-treated molecular sieve of Example 5 is shown. DETAILED DESCRIPTION
[0019] definition
[0020] The term "framework type" has the meaning described in "Atlas of Zeolite Framework Types" by Ch. Baerlocher, LB McCusker and DH Olsen (Elsevier, 6th revised edition, 2007).
[0021] The term "zeolite" refers to a synthetic aluminosilicate molecular sieve having a framework composed of alumina and silica (ie, repeating AlO4 and SiO4 tetrahedral units).
[0022] The term "aluminogermanosilicate" refers to a molecular sieve having a framework composed of AlO4, GeO4 and SiO4 tetrahedral units. An aluminogermanosilicate may contain only the named oxides, in which case it may be described as a "pure aluminogermanosilicate" or it may contain other oxides as well.
[0023] As used herein, the term "as synthesized" refers to the molecular sieve in its form after crystallization and prior to removal of the structure directing agent.
[0024] As used herein, the term "anhydrous" refers to a molecular sieve that is substantially free of physically adsorbed water and chemically adsorbed water.
[0025] Synthesis of molecular sieves
[0026] Molecular sieve SSZ-121 can be synthesized by: (1) preparing a reaction mixture comprising (a) a FAU framework-type zeolite; (b) a germanium source; (c) a structure directing agent (Q) comprising a 1,3-bis(1-adamantyl)imidazolium cation; (d) a fluoride ion source; and (e) water; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form molecular sieve crystals.
[0027] In terms of molar ratios, the reaction mixture may have a composition within the range listed in Table 1:
[0028] Table 1
[0029] Reactants Widest Secondary <![CDATA[(SiO2+GeO2) / Al2O3]]> 30 to 600 60 to 500 <![CDATA[Q / (SiO2+GeO2)]]> 0.10 to 1.00 0.20 to 0.70 <![CDATA[F / (SiO2+GeO2)]]> 0.10 to 1.00 0.20 to 0.70 <![CDATA[H2O / (SiO2+GeO2)]]> 2 to 10 4 to 8
[0030] wherein Q comprises a 1,3-bis(1-adamantyl)imidazolium cation.
[0031] FAU framework zeolite can be ammonium zeolite or hydrogen zeolite. The example of FAU framework zeolite includes zeolite Y (for example, CBV720, CBV760, CBV780, HSZ-HUA385 and HSZ-HUA390). Zeolite Y can have SiO2 / Al2O3 molar ratio of 30 to 500. FAU framework zeolite can include two or more zeolites. Two or more zeolites can be Y-type zeolites with different silica to alumina molar ratios. FAU framework zeolite can be the only or main source of silicon and aluminum forming the aluminum germanium silicate molecular sieve. In some aspects, a separate silicon source can be added. A separate silicon source includes colloidal silica, pyrogenic silica, precipitated silica, alkali metal silicate and tetraalkyl orthosilicate.
[0032] Suitable germanium sources include germanium oxide and germanium alkoxides (eg, germanium ethoxide, germanium isopropoxide).
[0033] Silicon and germanium may be present in the reaction mixture in a SiO2 / GeO2 molar ratio of 4 to 12 (eg, 6 to 10).
[0034] Suitable fluoride ion sources include hydrogen fluoride, ammonium fluoride and ammonium bifluoride.
[0035] The structure directing agent comprises a 1,3-bis(1-adamantyl)imidazolium cation (Q) represented by the following structure (1):
[0036]
[0037] Suitable sources of Q are hydroxides, chlorides, bromides and / or other salts of quaternary ammonium compounds.
[0038] The reaction mixture can have a Q / F molar ratio in a range of 0.80 to 1.20 (eg, 0.85 to 1.15, 0.90 to 1.10, 0.95 to 1.05, or 1 to 1).
[0039] The reaction mixture may contain seeds of a molecular sieve material, such as SSZ-121 from a previous synthesis, in an amount of 0.01 to 10,000 ppm by weight of the reaction mixture (e.g., 100 to 5000 ppm by weight). Seeding is beneficial in reducing the amount of time required for complete crystallization to occur. Additionally, seeding can result in increased purity of the product obtained by promoting nucleation and / or formation of SSZ-121 on any undesirable phase.
[0040] Note that the reaction mixture components may be provided by more than one source. In addition, one source may provide two or more reaction components. The reaction mixture may be prepared batchwise or continuously.
[0041] Crystallization and post-synthesis processing
[0042] The crystallization of the molecular sieve from the above reaction mixture can be carried out under static, tumbling or stirring conditions in a suitable reactor vessel (e.g., a polypropylene tank or a polytetrafluoroethylene liner or a stainless steel autoclave) at a temperature of 100° C. to 200° C. (e.g., 150° C. to 175° C.) for a time sufficient for crystallization to occur at the temperature used (e.g., 1 day to 14 days, or 2 days to 10 days). The hydrothermal crystallization process is usually carried out under pressure, such as in an autoclave, and preferably under autogenous pressure.
[0043] Once the molecular sieve crystals are formed, the solid product can be recovered from the reaction mixture by standard mechanical separation techniques such as centrifugation or filtration. The recovered crystals are washed with water and then dried to obtain the original synthesized molecular sieve crystals. The drying step can be carried out at an elevated temperature (e.g., 75° C. to 150° C.) for several hours (e.g., about 4 to 24 hours). The drying step can be carried out under vacuum or atmospheric pressure.
[0044] As a result of the crystallization process, the recovered crystalline molecular sieve product contains within its pore structure at least a portion of the structure directing agent used in the synthesis.
[0045] The originally synthesized molecular sieve can also be treated to remove part or all of the structure directing agent used for its synthesis. This can be conveniently achieved by heat treatment (i.e., calcination), in which the originally synthesized material is heated at a temperature of at least about 370°C for at least 1 minute and usually not more than 20 hours. Although the heat treatment can be carried out at a pressure lower than atmospheric pressure, atmospheric pressure is required for convenience. The heat treatment can be carried out at a temperature of up to about 925°C. The heat treatment can be carried out in an atmosphere selected from air, nitrogen, or a mixture thereof. For example, the heat treatment can be carried out in air at a temperature of 400°C to 600°C for a period of 3 to 8 hours. Alternatively, the structure directing agent Q can be removed by treatment with ozone. Ozone treatment can include heating the originally synthesized molecular sieve in the presence of ozone, and such heating can be carried out at a temperature of 50°C to 350°C (e.g., 100°C to 300°C, or 125°C to 250°C).
[0046] Any extra-framework metal cations in the molecular sieve may be replaced with other cations according to techniques well known in the art (e.g., by ion exchange). The replacement cations may include metal ions, hydrogen ions, hydrogen precursor (e.g., ammonium) ions, and combinations thereof.
[0047] Characterization of Molecular Sieve
[0048] In its as-synthesized and anhydrous form, molecular sieve SSZ-121 may have a chemical composition including the following molar relationships listed in Table 2:
[0049] Table 2
[0050] Widest Secondary <![CDATA[(SiO2+GeO2) / Al2O3]]> ≥30 ≥50 <![CDATA[Q / (SiO2+GeO2)]]> >0 to 0.1 >0 to 0.1
[0051] wherein Q comprises a 1,3-bis(1-adamantyl)imidazolium cation. In some aspects, the molecular sieve can have a SiO2 / GeO2 molar ratio in a range of 4 to 12 (eg, 6 to 10).
[0052] In its calcined form, molecular sieve SSZ-121 may have a chemical composition comprising the following molar relationship:
[0053] Al2O3:(n)(SiO2+GeO2)
[0054] wherein n≧30 (eg, 30 to 500, 30 to 250, 30 to 150, ≧50, 50 to 250, or 50 to 150).
[0055] In its as-synthesized form, molecular sieve SSZ-121 exhibits a powder XRD pattern having at least the following 2-theta scattering angles: 6.3±0.2, 7.0±0.2, 9.5±0.2, 13.0±0.2, 16.0±0.2, 18.5±0.2, 19.8±0.2, 21.2±0.2, 24.0±0.2, 25.0±0.2, 26.5±0.2, 28.5±0.2 and 30.0±0.2 degrees 2-theta. In its calcined form, molecular sieve SSZ-121 exhibits a powder XRD pattern having at least the following 2-theta scattering angles: 6.5±0.2, 9.5±0.2, 13.0±0.2, 18.5±0.2, 19.8±0.2, 21.2±0.2, 24.0±0.2, 25.0±0.2, 26.5±0.2, 28.5±0.2 and 30.0±0.2 degrees 2-theta.
[0056] The powder X-ray diffraction patterns presented herein were collected by standard techniques. The radiation was CuKα radiation. The peak heights and positions vary as a function of 2θ (where θ is the Bragg angle), and from the relative intensities of the peaks (adjusted for background), the interplanar spacings d corresponding to the recorded lines can be calculated.
[0057] Small changes in the diffraction pattern may be caused by changes in the molar ratio of the sample framework material due to changes in the lattice constant. In addition, disordered material and / or sufficiently small crystals will affect the shape and intensity of the peaks, resulting in significant peak broadening. Small changes in the diffraction pattern may also be caused by changes in the organic compounds used in the preparation. Calcination can also cause small changes in the XRD pattern. Despite these small perturbations, the basic lattice structure remains unchanged.
[0058] Industrial Applicability
[0059] Molecular sieve SSZ-121 (where some or all of the structure directing agent is removed) can be used as an adsorbent or catalyst to catalyze a variety of organic compound conversion processes, including many organic compound conversion processes that are currently of commercial / industrial importance. Examples of chemical conversion processes that are effectively catalyzed by SSZ-121 itself or in combination with one or more other catalytically active materials (including other crystalline catalysts) include those that require a catalyst with acid activity. Examples of organic conversion processes that can be catalyzed by SSZ-121 include aromatization, cracking, hydrocracking, disproportionation, alkylation, oligomerization, and isomerization.
[0060] As is the case with many catalysts, it may be necessary to combine SSZ-121 with another material to resist the temperature and other conditions used in organic conversion processes. Such materials include active and inactive materials and synthetic or naturally occurring zeolites and inorganic materials such as clays, silica and / or metal oxides such as alumina. The latter may be naturally occurring or in the form of a gelatinous precipitate or gel, including a mixture of silica and metal oxides. Materials used in combination with active SSZ-121 (i.e., in combination with it or present in the synthesis of new materials) tend to change the conversion rate and / or selectivity of the catalyst in certain organic conversion processes. Inactive materials appropriately act as diluents to control the amount of conversion in a given process, so that the product can be obtained in an economical and orderly manner without the need to adopt other means of controlling the reaction rate. These materials can be incorporated into naturally occurring clays (e.g., bentonite and kaolin) to increase the compressive strength of the catalyst under commercial operating conditions. These materials (i.e., clays, oxides, etc.) act as binders for the catalyst. It is necessary to provide a catalyst with good compressive strength because it is necessary to prevent the catalyst from decomposing into a powdery material in commercial applications. These clay and / or oxide binders are usually employed solely for the purpose of increasing the compressive strength of the catalyst.
[0061] Naturally occurring clays that can be compounded with SSZ-121 include montmorillonite and the kaolin family, which family includes sub-bentonite, as well as kaolins commonly known as Dixie, McNamee, Georgia and Florida clays or other kaolins in which the major mineral components are halloysite, kaolinite, dickite, perlite or bauxite. Such clays can be used in the original state as originally mined or in a state that has initially undergone calcination, acid treatment or chemical modification. Binders that can be used for compounding with SSZ-121 also include inorganic oxides such as silica, zirconium oxide, titanium dioxide, magnesium oxide, beryllium oxide, aluminum oxide and mixtures thereof.
[0062] In addition to the above materials, SSZ-121 can also be compounded with porous matrix materials such as silica-alumina, silica-magnesia, silica-zirconia, silica-thoria, silica-beryllia, silica-titania, and ternary compositions such as silica-alumina-thoria, silica-alumina-zirconia, silica-alumina-magnesia and silica-magnesia-zirconia.
[0063] The relative proportions of SSZ-121 and the inorganic oxide matrix can vary widely, with the SSZ-121 content ranging from 1 to 90 wt % (eg, 2 to 80 wt %) of the composite.
[0064] Example
[0065] The following illustrative examples are intended to be non-limiting.
[0066] Example 1
[0067] Synthesis of SSZ-121
[0068] 0.27 g of Tosoh HSZ-390HUAY-zeolite (SiO2 / Al2O3 molar ratio = 500), 0.05 g of GeO2 and 2.5 mmoles of 1,3-bis(1-adamantyl)imidazolium hydroxide aqueous solution were added to a 23 mL Parr reactor. The reactor was then placed in a fume hood and the water was allowed to evaporate to achieve a H2O / (SiO2+GeO2) molar ratio of 7 (as determined by the total mass of the suspension). Then, 2.5 mmoles of HF were added and the reactor was heated to 160°C while tumbling at 43 rpm for about 7 days. The solid product was recovered by centrifugation, washed with deionized water, and dried at 95°C.
[0069] The powder XRD of the product gives Figure 1 The pattern indicated in and shows that the product is a pure form of the new phase SSZ-121. The small crystal size was inferred from the peak broadening in the powder XRD pattern.
[0070] Figure 2 SEM images of the product are provided and show that the product comprises uniform rods.
[0071] Example 2
[0072] Calcination of SSZ-121
[0073] The as-synthesized molecular sieve of Example 1 was calcined in a muffle furnace under an air flow heated to 550° C. at a rate of 1° C. / min and maintained at 550° C. for 5 hours, cooled, and then analyzed by powder XRD.
[0074] The calcined product was analyzed by the t-curve method of nitrogen physical adsorption, which showed that the micropore volume of the sample was 0.144 cm 3 / g.
[0075] Example 3
[0076] Absorption of diisopropyl azodicarboxylate
[0077] The microporous characterization of SSZ-121 was evaluated spectrophotometrically by absorption of the chromophore diisopropyl azodicarboxylate (DIAD) according to the method described by LT. Yuen et al. (Micropor. Mater. 1997, 12, 229-249). The molecular sieve was used in its hydrogen form.
[0078] Each molecular sieve was pressed to 2000 psi in the dye and, immediately before use, the pellets were broken and sieved (24-40) and then dried in an oven at 575°F for 2-4 hours. The sample was removed, placed in a desiccator and allowed to cool. The sieved material (60 mg) was quickly weighed out and placed in a pre-calibrated spectroscopic system.
[0079] DIAD solution in spectroscopic grade isooctane (0.127 g DIAD / 70 mL isooctane) corresponding to 406 nm (λ max ) and was recirculated every 23 seconds through the zeolite holding basket in the spectroscopy system. Data were acquired continuously. The run was continued at ambient temperature for 18 hours, at which point almost all experiments reached absorption equilibrium and no further changes in absorbance were observed.
[0080] UV-Vis data were recorded using an Agilent Technologies Cary 8454 UV-Vis diode array spectrophotometer monitoring 190-500 nm. Absorbance measurements were performed using a 1 cm pathlength cuvette. Isooctane was first run as a blank since it exhibits no absorbance between 190-500 nm.
[0081] Table 3 summarizes the absorption of DIAD in SSZ-121 and several other molecular sieves of known structures.
[0082] Table 3
[0083] Molecular sieve Pore size type % DIAD removed SSZ-13(CHA) Small (3-D) none ZSM-5(MFI) Medium (3-D) 40% LZ-210(FAU) Large (3-D) 90% SSZ-121 unknown 75%
[0084] Example 4
[0085] Constraint Index
[0086] The Constraint Index is a test to determine the shape-selective catalytic properties in zeolites. It compares the reaction rates for the cracking of n-hexane and its isomer 3-methylpentane under competing conditions (see, for example, VJ Frillette et al., J. Catal. 1981, 67, 218-222).
[0087] The molecular sieve in hydrogen form of Example 2 was sphericalized at 4kpsi, crushed and granulated to 20-40 mesh. A 0.6g sample of granular material was calcined at 540°C in air for 4 hours and cooled in a dryer to ensure drying. Then, 0.47g of material was loaded into a 1 / 4 inch stainless steel tube with corundum on both sides of the molecular sieve bed. A furnace (Applied TestSystems, Inc.) was used to heat the reactor tube. Nitrogen was introduced into the reactor tube at 9.4mL / min and at atmospheric pressure. The reactor was heated to about 800°F (427°C), and 50 / 50 n-hexane and 3-methylpentane feeds were introduced into the reactor at a rate of 8μL / min. The feed was delivered by an ISCO pump. Direct injection into the GC began 15 minutes after the feed was introduced. The test data results after running for 136 minutes (800°F) are listed in Table 4.
[0088] Table 4 Constraint index test
[0089] n-Hexane conversion, % 2.8 3-Methylpentane conversion, % 4.9 Feed conversion, % 3.9 Constraint Index (excluding 2-methylpentane) 0.56 Constraint Index (including 2-methylpentane) 0.56
[0090] Example 5
[0091] Example 1 was repeated except that Zeolyst CBV780 Y-zeolite (SiO2 / Al2O3 molar ratio = 80) was used as the FAU source. Powder XRD showed the product to be SSZ-121.
[0092] The as-synthesized molecular sieve was exposed to ozone at 150°C for 6 hours.
[0093] The powder XRD of the ozone treated product gives Figure 3 The graphic indicated in .
[0094] Example 6
[0095] Example 1 was repeated except that Zeolyst CBV760 Y-zeolite (SiO2 / Al2O3 molar ratio = 60) was used as the FAU source. The recovered raw synthesis product was calcined as described in Example 2. Powder XRD showed that the calcined product was SSZ-121.
[0096] Analysis of the calcined product by the t-curve method of nitrogen physical adsorption showed that the sample had a 0.18 cm 3 / g micropore volume and greater than 300m 2 A high surface area indicates that the material consists of very small crystals.
[0097] Example 7
[0098] Example 1 was repeated except that Zeolyst CBV720 Y-zeolite (SiO2 / Al2O3 molar ratio = 30) was used as the FAU source. Powder XRD showed the product to be SSZ-121.
[0099] The recovered raw synthesis product was calcined as described in Example 2.
[0100] The calcined product was analyzed by the t-curve method of nitrogen physical adsorption, which showed that the micropore volume of the sample was 0.22 cm 3 / g.
[0101] Example 8
[0102] Bronsted acidity ( Acidity
[0103] The Bronsted acidity of the molecular sieve of Example 6 in its calcined form was determined by n-propylamine temperature programmed desorption (TPD) adapted from the description published by TJ Gricus Kofke et al. (J. Catal. 1988, 114, 34-45); TJ Gricus Kofke et al. (J. Catal. 1989, 115, 265-272); and JG Tittensor et al. (J. Catal. 1992, 138, 714-720). The sample was pretreated in flowing dry H2 at 400°C-500°C for 1 hour. The dehydrated sample was then cooled to 120°C in flowing dry helium and held at 120°C for 30 minutes in flowing helium saturated with n-propylamine for adsorption. The n-propylamine saturated sample was then heated to 500°C in flowing dry helium at a rate of 10°C / min. The Bronsted acidity was calculated by thermogravimetric analysis (TGA) and mass spectrometry of the effluent NH3 and propylene based on the weight loss versus temperature. The Bronsted acidity of the sample was 295.63 μmol / g, indicating that aluminum sites were incorporated into the framework of the molecular sieve.
Claims
1. A molecular sieve having, in its calcined form, a powder X-ray diffraction pattern having at least the following 2-theta scattering angles: 6.5 ± 0.2, 9.5 ± 0.2, 13.0 ± 0.2, 18.5 ± 0.2, 19.8 ± 0.2, 21.2 ± 0.2, 24.0 ± 0.2, 25.0 ± 0.2, 26.5 ± 0.2, 28.5 ± 0.2 and 30.0 ± 0.2 degrees 2-theta, in, The composition of the molecular sieve includes the following molar relationship: Where n≥30.
2. The molecular sieve according to claim 1, wherein the composition comprises the following molar relationship: Where n≥50.
3. A molecular sieve having, in its as-synthesized form, a powder X-ray diffraction pattern having at least the following 2-theta scattering angles: 6.3±0.2, 7.0±0.2, 9.5±0.2, 13.0±0.2, 16.0±0.2, 18.5±0.2, 19.8±0.2, 21.2±0.2, 24±0.2, 25.0±0.2, 26.5±0.2, 28.5±0.2 and 30.0±0.2 degrees 2-theta, The chemical composition of the molecular sieve includes the following molar relationship: wherein Q comprises a 1,3-bis(1-adamantyl)imidazolium cation.
4. The molecular sieve according to claim 3, wherein the chemical composition comprises the following molar relationship: wherein Q comprises a 1,3-bis(1-adamantyl)imidazolium cation.
5. A method for synthesizing the molecular sieve according to claim 3, the method comprising: (1) preparing a reaction mixture, which comprises: (a) FAU framework zeolite; (b) Germanium source; (c) a structure directing agent Q comprising a 1,3-bis(1-adamantyl)imidazolium cation; (d) a source of fluoride ions; and (e) water; and (2) subjecting the reaction mixture to crystallization conditions sufficient to form crystals of the molecular sieve.
6. The process according to claim 5, wherein the reaction mixture has the following composition in molar ratio:
7. The process according to claim 5, wherein the reaction mixture has the following composition in molar ratio:
8. The method of claim 5, wherein the FAU framework-type zeolite is zeolite Y.
9. The method of claim 5, wherein the crystallization conditions include a temperature of 100°C to 200°C.
10. The method of claim 5, wherein the reaction mixture has a Q / F in the range of 0.8 to 1.2 - Molar ratio.
11. A process for converting a feedstock comprising an organic compound into a conversion product, the process comprising contacting the feedstock with a catalyst comprising the molecular sieve according to claim 1 under organic compound conversion conditions.