A high-transparency and high-toughness polyamide material and preparation method thereof
By performing oscillatory shearing and temperature control during the preparation process of polyamide materials, γ crystalline materials are produced, which solves the contradiction between transparency and toughness in the existing technology, achieves efficient preparation of polyamide materials, and has good Mechanical properties and light transmittance.
Patent Information
- Application Number
- CN202211446560.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-18
AI Technical Summary
When improving the transparency of existing polyamide materials, the toughness and processing properties are often affected, and common methods have compatibility issues and increased costs.
By performing oscillatory shear treatment during the preparation process of polyamide materials, controlling temperature and post-polymerization reaction, polyamide materials with stable γ crystal form are produced, and their mechanical properties and light transmittance are improved.
The elongation at break and toughness of the polyamide material are significantly improved, while high transparency is achieved. The method is simple to operate, environmentally friendly, does not require additives, and is suitable for promotion and use.
Smart Images

Figure CN115678003B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyamide material preparation, and in particular relates to a high-transparency and high-toughness polyamide material and a preparation method thereof. Background Art
[0002] Ordinary polyamide has strong hydrogen bonds between molecular chains due to the presence of amide groups, and the molecules are easily arranged in a regular pattern, so it has a high degree of crystallinity, and the crystal size is large, larger than the wavelength of visible light, so this type of polyamide generally appears white, milky white or yellow and other opaque states under the macroscopic view. If suitable monomers are introduced into polyamide to inhibit crystallization behavior or the crystal size is controlled by certain means to make it smaller than the wavelength of visible light (400-700nm), and there is no chromophore in the molecular structure, macroscopically transparent polyamide materials can be obtained while ensuring that the refractive index of the crystalline region and the amorphous region is consistent. The key to obtaining transparent polyamide is to hinder crystallization or reduce the crystal size. The common methods are mainly the following three:
[0003] 1. Introducing large steric hindrance monomers
[0004] Introducing large steric hindrance branching, alicyclic or aromatic ring structures into the polyamide main chain can greatly reduce the regularity of the polyamide chain segments by hindering the movement of the molecular chain. Its crystallization ability shows a significant decrease, making the material present a microcrystalline or amorphous state, thus showing transparency.
[0005] The Chinese invention patent with application number CN201510660451.2 discloses a semi-aromatic transparent polyamide material PA6I and a preparation method thereof, wherein isophthalic acid and hexamethylenediamine are melt-polycondensed in an aqueous solvent to obtain a PA6I material with high transparency and excellent mechanical properties.
[0006] Chinese patent application number CN201510992965.8 discloses a method for preparing semi-aromatic transparent polyamide, which uses aromatic dicarboxylic acid and alicyclic diamine to carry out acid-base neutralization reaction in a polar aprotic solvent to obtain a mixed solution containing polyamide salt, and then polymerizes to obtain a high molecular weight semi-aromatic transparent polyamide.
[0007] The Chinese patent application number CN202010322055.X discloses a transparent polyamide T21 material and its preparation method, which uses hexamethylenediamine, isophthalic acid and terephthalic acid to carry out melt polycondensation or solid phase polycondensation in an aqueous solvent, combining the high rigidity of the benzene ring and the transparency of the semi-aromatic polyamide to obtain a polyamide material T21 with good rigidity and transparency, which fully meets the requirements for oil cups and industrial glasses in motor vehicles. However, these large steric hindrance monomers often have high rigidity, which greatly reduces their elongation at break and toughness, resulting in performance degradation; at the same time, after the introduction of such monomers, their glass transition temperature and melting point are greatly increased, making their processing performance very poor, and requiring high processing equipment and very harsh process conditions.
[0008] 2. Copolymerization or blending
[0009] Different monomers are introduced into the main chain of polyamide for random copolymerization modification, thereby destroying the regularity of the molecular chain arrangement and reducing the density of hydrogen bonds that can be formed, so that the material has higher transparency.
[0010] Chinese patent application number CN201210592812.0 discloses a transparent polyamide and a preparation method thereof. By utilizing the copolymerization method and the structural characteristics of aliphatic diacid monomers and alicyclic diamine monomers, a transparent polyamide material having a light transmittance of more than 80% in the visible light wavelength range is prepared by copolymerizing aliphatic diacids and alicyclic diamines with amide salts.
[0011] The Chinese patent application number CN201510861348.4 discloses a method for synthesizing a highly fluid transparent polyamide, wherein a transparent polyamide is first prepared by melt copolymerization of alicyclic diamine, aromatic diacid, aliphatic long carbon chain diacid, and polyamine, and then blended with a long carbon chain semi-crystalline polyamide. On the premise of ensuring the transmittance, the rigidity and toughness of the blended polyamide can be maintained and the fluidity can be improved. However, due to the destruction of crystallization, other properties (such as mechanical properties, thermal properties, etc.) will be greatly lost.
[0012] 3. Introduce fillers
[0013] By adding a suitable nucleating agent to cause crystal fragmentation, a transparent product can be obtained. For example, by adding 0.1% of a nucleating agent (such as colloidal silica) to the melt of PA66 or PA6, crystal particles with very small grain size can be obtained, thereby producing a transparent product.
[0014] Chinese patent application number CN201210247411.1 discloses a method for preparing a highly transparent polyamide composite film, in which polypropylene or polypropylene elastomer is added to a polyamide resin as a material for improving transparency, thereby preparing a highly transparent polyamide co-extruded composite film.
[0015] The Chinese patent application number CN202011489942.2 discloses a highly infrared transparent nylon and a preparation method thereof, using a prepolymer prepared by a long carbon chain diamine and an aliphatic long carbon chain dibasic acid in a molar ratio of 1:1, and a prepolymer prepared by a para-aromatic diamine and an aromatic dibasic acid in a molar ratio of 1:1, adding an antioxidant and a nucleating agent, wherein the nucleating agent helps to form a fine and uniform crystal structure, which can improve infrared transmittance. However, due to the very fast crystallization rate of polyamide, crystallization is difficult to control, and the transparency of the product obtained using this method is limited.
[0016] In summary, the current methods for making polyamides highly transparent are mainly concentrated on the above three methods. However, all three methods have some shortcomings: for example, while the method of introducing large steric hindrance monomers improves transparency, these large steric hindrance monomers often have high rigidity, which greatly reduces their elongation at break and toughness, resulting in performance degradation; at the same time, after the introduction of such monomers, their glass transition temperature and melting point are greatly increased, making their processing performance very poor, and requiring high processing equipment and harsh process conditions. In addition, the key factor that determines the performance of polymer composites is the compatibility issue. The method of adding small molecule fillers or second polymers often faces poor interactions between fillers or second polymers and matrix polymers, resulting in agglomeration or phase separation in the matrix, while adding a third component as a compatibilizer increases the cost and the complexity of the system.
[0017] In view of this, the present invention is proposed. Summary of the invention
[0018] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a highly transparent and highly tough polyamide material and a preparation method thereof, wherein a polyamide material having a stable γ crystal form is prepared by subjecting the raw material mixture to an oscillating shearing treatment during the preparation of the polyamide material and controlling the temperature during the preparation of the polyamide material; or adjusting the post-polymerization temperature during the post-polymerization of the polyamide material; or controlling the cooling rate during the heat treatment of the polyamide material. On the other hand, the present invention provides a highly transparent and highly tough polyamide material, which has a γ crystal form and contains less extended chain structure in the γ crystal than in the α crystal, so that the Young's modulus of the γ crystal is lower but the toughness is higher, which greatly improves the mechanical properties of the polyamide, and at the same time, the polyamide having a γ crystal form prepared by the preparation method of the present invention has the characteristic of high light transmittance.
[0019] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a highly transparent and high-toughness polyamide material, comprising the following steps:
[0020] S1, a dibasic acid, a diamine, deionized water, a catalyst and an antioxidant are mixed to obtain a raw material mixture;
[0021] S2, heating the raw material mixture to a first preset temperature under a preset pressure condition to allow the raw material mixture to undergo a polycondensation reaction, and performing an oscillation shearing treatment on the raw material mixture during the heating process;
[0022] S3, after the polycondensation reaction is completed, the material is cooled and discharged to obtain a polyamide material having a γ crystal structure;
[0023] The dibasic acid and diamine in the raw material mixture are dibasic acids and diamines having an even number of carbon atoms in the main chain;
[0024] Preferably, the antioxidant is a mixture of one or more of a phenolic antioxidant, an ester antioxidant, a metal ion passivator, or a peroxide decomposer;
[0025] More preferably, the phenolic antioxidant is antioxidant 1010, antioxidant 1098, antioxidant 1035, antioxidant 1093; the amine antioxidant is antioxidant DNP, antioxidant 4010; the metal ion passivator is copper acetate / potassium iodide; the peroxide decomposer is antioxidant 168;
[0026] Preferably, the catalyst is sodium hypophosphite.
[0027] Specifically, step S3 is to continue heating for a period of time after depressurizing and draining, and then cool and discharge the material to obtain a polyamide material with a γ crystal form.
[0028] The above scheme limits the temperature and pressure of the polycondensation reaction and the types of dibasic acid and diamine in the raw material mixture, and adds an oscillation shear process during the polycondensation reaction. The oscillation shear process and the reaction regulation are coordinated to achieve the control of the crystal structure of the polyamide material, thereby obtaining a polyamide material with a stable γ crystal structure.
[0029] Furthermore, in step S2, the temperature of the condensation reaction is raised from room temperature to a first preset temperature, and the first preset temperature is between 80°C below the melting temperature of the polyamide material with a γ crystal form and the starting thermal decomposition temperature. After the temperature reaches the melting temperature of the polyamide material with a γ crystal form, the raw material mixture is subjected to an oscillation shearing treatment.
[0030] In the above scheme, it is specified that the oscillation shearing treatment starts when the condensation reaction temperature reaches the melting temperature of the polyamide material with the γ crystal form. At this time, part of the solid inside the raw material mixture has melted into liquid and can be better processed by oscillation shearing; if the oscillation shearing is started at a temperature lower than the melting temperature of the polyamide material with the γ crystal form, part of the raw material is still in a solid state and cannot be affected by the oscillation shearing.
[0031] Preferably, the first preset temperature is between 20° C. below the melting temperature of the polyamide material having the γ crystal phase and 30° C. above the melting temperature.
[0032] In the above preferred embodiment, if the first preset temperature is higher than the starting thermal decomposition temperature, the raw material mixture will decompose while polymerizing, resulting in a decrease in the reaction yield and the possible generation of by-products that affect the purity of the product.
[0033] Furthermore, in step S2, the reaction temperature is raised to a first preset temperature by a staged heating method, wherein the temperature of at least one heating stage is higher than the melting temperature of the polyamide material having the γ crystal form.
[0034] In the above scheme, the accuracy of temperature control is improved by means of staged heating, wherein the temperature of at least one heating stage is higher than the melting temperature of the polyamide material with γ crystal form, thereby ensuring that the raw material mixture can be subjected to oscillatory shearing and matching the temperature of the oscillatory shearing and polycondensation reaction, thereby improving the control accuracy.
[0035] Furthermore, the duration of each heating stage ranges from 1 to 5 hours; preferably, the duration ranges from 2 to 3 hours.
[0036] Furthermore, the staged heating process includes at least two heating stages above the melting temperature of the polyamide material having the γ crystal phase, wherein at least one of the heating stages is subjected to an oscillating shearing treatment.
[0037] The above scheme defines that the heating process includes at least two heating stages that are higher than the melting temperature of the polyamide material with the γ crystal form, and at least one of the heating stages is subjected to oscillation shearing treatment. The duration of the oscillation shearing can be controlled according to actual needs to adjust the proportion of the γ crystal form.
[0038] Preferably, the last heating stage is subjected to an oscillating shearing treatment.
[0039] The above preferred scheme is a more preferred scheme obtained by technicians based on a large number of calculations and experiments. Controlling the last heating stage to perform oscillation shearing treatment can ensure that the reaction system is in a sheared state before the end of the polycondensation reaction, which is beneficial to improving the performance of the prepared polyamide material.
[0040] Furthermore, the heating stage includes a first heating stage, a second heating stage and a third heating stage in which the temperature is increased successively, and both the second heating stage and the third heating stage are subjected to oscillation shearing treatment, wherein the duration of the oscillation shearing treatment in the third heating stage is shorter than the duration of the oscillation shearing treatment in the second heating stage.
[0041] Furthermore, the duration of the oscillating shearing treatment does not exceed 2 hours; and the amplitude range of the oscillating shearing treatment is 3-30%.
[0042] Preferably, the duration of the oscillating shearing treatment is 0.5-1 h; the amplitude range of the oscillating shearing treatment is 3-10%.
[0043] Since long oscillation shearing time will lead to product degradation, after a lot of calculations and research, it was found that controlling the oscillation shearing time to no more than two hours can ensure the stable production of γ crystals while avoiding product degradation; preferably, oscillation shearing is started after the temperature of the heating stage corresponding to the need for oscillation shearing is stabilized.
[0044] At the same time, the amplitude of the above-mentioned oscillatory shearing treatment is the preferred range obtained by technicians based on a large number of studies and experiments. If it is less than this range, the amplitude of the oscillatory shearing is small, and the polyamide material with a γ crystal form cannot be successfully obtained; if the amplitude is too large, it may promote the degradation of the product, resulting in the inability to obtain a polyamide material with a stable γ crystal form.
[0045] Furthermore, in step S2, before heating, the air is replaced by an inert gas, and a portion of the inert gas is reserved to reach a preset pressure, and then the temperature is raised to carry out a polycondensation reaction, and the preset pressure range is 0.05-1.0 MPa.
[0046] Furthermore, in step S3, heating is continued for a period of time after pressure relief and drainage, the heating temperature is between the melting temperature and 30° C. above the melting temperature, and the heating time does not exceed 2 hours.
[0047] Preferably, the heating temperature is between the melting temperature and 10° C. above the melting temperature, and the heating time does not exceed 1 hour.
[0048] In the above scheme, the pressure relief process is to remove a large amount of water molecules produced during the polymerization process, so that the reaction proceeds in the forward direction to obtain a high molecular weight polyamide material. At the same time, the heating temperature in the pressure relief and drainage stage is between the melting temperature and 10°C above the melting temperature, and the heating time does not exceed 1 hour, so as to ensure that the influence of the oscillating shear treatment in the previous heating stage is not eliminated while increasing the molecular weight of the material.
[0049] The present invention also provides a method for preparing a highly transparent and high-toughness polyamide material, wherein a post-polymerization reaction is performed on the polyamide material in a solid phase viscosity increasing device, and the molecular weight and distribution of the polyamide material are adjusted by adjusting the temperature of the post-polymerization reaction, thereby achieving regulation of the crystal form to obtain a polyamide material with a γ crystal form, wherein the temperature during the post-polymerization reaction is between the glass transition temperature and the melting temperature of the polyamide material.
[0050] Preferably, the duration of the post-polymerization reaction is 1-14 hours.
[0051] More preferably, the duration of the post-polymerization reaction is 2-8 hours.
[0052] Furthermore, the polyamide material with γ crystal structure prepared by the previous preparation method is placed in a solid phase viscosity increasing device for post-polymerization reaction.
[0053] The above scheme can improve the γ crystal form inside the amide by further performing a post-polymerization reaction on the polyamide material that already has the γ crystal form, thereby further improving the mechanical properties and light transmittance of the polyamide material with the γ crystal form.
[0054] The present invention also provides a method for preparing a highly transparent and high-toughness polyamide material, which comprises the following steps: after the polyamide material is completely dehydrated, the temperature is raised to above the melting point in an inert atmosphere to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain the inert atmosphere; and then the temperature is lowered to 40° C. below the melting point of the polyamide material at a rate of not less than 5° C. / min to obtain a polyamide material having a γ crystal form;
[0055] Alternatively, after the polyamide material is completely dehydrated, the temperature is raised to a second preset temperature under an inert atmosphere, and then the polyamide material is heat treated by keeping the temperature, and then the temperature is lowered to 40° C. below the melting point of the polyamide material at a rate of not less than 5° C. / min to obtain a polyamide material having a γ crystal structure;
[0056] The inert atmosphere is high-purity helium, high-purity nitrogen or high-purity argon, and the vacuum degree under the inert atmosphere is maintained at -0.1-1 MPa.
[0057] Preferably, the inert atmosphere is high-purity helium or high-purity nitrogen;
[0058] Preferably, the temperature is lowered to room temperature at a rate of not less than 5° C. / min to obtain a polyamide material having a γ crystal structure.
[0059] It should be noted that the complete dehydration of the polyamide material means that the weight of the polyamide material measured by the constant weight method no longer changes, and at this time, the moisture content of the polyamide material is determined to be 0%.
[0060] In the above scheme, after completely eliminating the thermal history, the hydrogen bonds in the melt are disordered, and in the subsequent cooling process, the hydrogen bonds will be reorganized into ordered hydrogen bonds. By changing the cooling rate, the order of the subsequent hydrogen bonds can be controlled, thereby obtaining a γ crystal with disordered hydrogen bonds.
[0061] Furthermore, the second preset temperature is between the melting temperature of the polyamide material and 30° C. above the melting temperature, and the heat treatment time is 5-30 minutes.
[0062] Furthermore, the polyamide material with γ crystal structure prepared by the above method is one of PA66, PA610, PA612, or a polyamide in which the number of methylene groups between adjacent amide groups on the main chain is not less than 10.
[0063] More preferably, the prepared polyamide material is one of PA1010, PA1012, PA1210, PA1212 or PA1214.
[0064] The second aspect of the present invention provides a high-transparency and high-toughness polyamide material prepared by the above method.
[0065] Specifically, the prepared polyamide material with γ crystal form has an elongation at break of 101-210% of that of conventional polyamide materials, a toughness of 101-200% of that of conventional polyamide materials, and a light transmittance of 80%-100%.
[0066] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0067] 1. The preparation method of the highly transparent and high-toughness polyamide provided by the present invention is to obtain a polyamide with a γ crystal structure by subjecting the raw material mixture to an oscillating shearing treatment during the polycondensation reaction; or adjusting the post-polymerization temperature during the post-polymerization of the polyamide material; or controlling the cooling rate during the heat treatment of the polyamide material. The formation of the γ crystal structure can significantly improve the elongation at break and toughness of the polyamide. At the same time, due to the appearance of the γ crystal structure, the polyamide changes from the original opaque to highly transparent.
[0068] 2. The preparation method of high-transparency and high-toughness polyamide provided by the present invention is a physical method, which is simple and direct to operate and does not require other additives or chemical methods to improve its toughness and transparency; and the whole process is environmentally friendly and pollution-free, and is suitable for promotion and use.
[0069] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 This is a comparison of one-dimensional WAXD curves of a highly transparent and high-toughness polyamide material prepared according to the preparation method of Example 15 of the present invention;
[0071] Figure 2 It is the result of peak separation of the one-dimensional WAXD curves corresponding to the α-crystalline form and the γ-crystalline form;
[0072] Figure 3 The stress-strain comparison curves of the high-transparency and high-toughness polyamide material prepared according to the preparation method of Example 15 of the present invention are compared;
[0073] Figure 4 This is a transparency comparison display diagram of the high-transparency and high-toughness polyamide material prepared according to the preparation method of Example 15 of the present invention. DETAILED DESCRIPTION
[0074] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention but are not used to limit the scope of the present invention.
[0075] It should be noted that, in the present invention, the testing conditions for the melting onset temperature and the melting point temperature are measured using a differential scanning calorimeter in a nitrogen atmosphere from room temperature to 250°C at a rate of 10°C / min, and the starting thermal decomposition temperature is measured using a thermogravimetric analyzer in a nitrogen atmosphere from 50°C to 700°C at a rate of 10°C / min.
[0076] The crystal form was tested by using an X-ray diffractometer (Xeuss 2.0) from Xenocs, France. The instrument used a copper target Cu Kα light source (GeniX3D Cu ULD) with a wavelength of In order to obtain a result with a good signal-to-noise ratio, the exposure time used was 300s. The distance from the sample to the detector in the experiment was 134mm. The corresponding two-dimensional WAXD pattern was collected with a semiconductor detector (Pilatus300k, DECTRIS). The resolution of the two-dimensional image was 487×619 pixels, and the size of each pixel was 172×172μm2. The obtained two-dimensional WAXD pattern was corrected for detector noise, air scattering and sample absorption, and then integrated to obtain a one-dimensional WAXD curve.
[0077] Mechanical testing The tensile properties of the samples were tested using a tensile testing machine (Instron 3365) at a temperature of 25° C., a relative humidity of 30% RH, and a tensile speed of 20 mm / min. The above test was repeated at least 10 times for each sample.
[0078] The light transmittance is measured by a light transmittance / haze meter.
[0079] Oscillatory shearing means that the sample is oscillated by applying periodic rotational shearing to the sample, and the amplitude of the oscillatory shearing is controlled within a range of 3-30% by controlling the frequency of the rotational shearing.
[0080] The present invention is further described in detail below with reference to specific embodiments.
[0081] Embodiment 1
[0082] As an embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material. The prepared polyamide material is PA66, the melting temperature of PA66 is 257° C., and the initial thermal decomposition temperature is 437° C., and the method specifically comprises the following steps:
[0083] S1, mixing adipic acid, hexamethylenediamine, antioxidant 1098, sodium hypophosphite and deionized water in a mass ratio of 1:1.2:0.005:0.005:0.3 to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0084] S2. Replace the air inside the autoclave with an inert gas, and reserve 1 MPa of inert gas after repeating three times. Rise the temperature to 280°C for polycondensation reaction in three stages, wherein the first stage is from room temperature to 200°C; the second stage is from 200°C to 240°C; the third stage is from 240°C to 280°C, and each stage is heated to the target temperature and kept isothermal for 2 hours; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 10%;
[0085] S3. After depressurizing the reactor, maintain heating at 260° C. for 1 hour, and then cool and discharge the material to obtain a PA66 material with a γ-crystal structure.
[0086] It should be noted that, since water is generated during the reaction, the water continues to evaporate in a high temperature environment, causing the pressure in the reactor to increase.
[0087] Embodiment 2
[0088] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, wherein the prepared polyamide material is PA1214, the melting temperature of PA1214 is 184° C., and the thermal decomposition temperature is 400° C., and the method specifically comprises the following steps:
[0089] S1, mixing tetradecanedioic acid, dodecanediamine, antioxidant 1010, sodium hypophosphite and deionized water in a mass ratio of 1:1.1:0.007:0.005:0.2 to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0090] S2. Replace the air inside the autoclave with an inert gas, and reserve 0.05 MPa of inert gas after repeating three times. Raise the temperature to 200°C for polycondensation reaction in three stages, wherein the first stage is from room temperature to 160°C; the second stage is from 160°C to 180°C; the third stage is from 180°C to 200°C, and each stage is heated to the target temperature and kept isothermal for 3 hours; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 5%;
[0091] S3. After depressurizing the reactor, maintain heating at 184° C. for 2 h, and then cool and discharge the material to obtain a PA1214 material with a γ-crystal structure.
[0092] Embodiment 3
[0093] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, wherein the prepared polyamide material is PA1012, the melting temperature of PA1012 is 189° C., and the thermal decomposition temperature is 406° C., and the method specifically comprises the following steps:
[0094] S1, mixing dodecanedioic acid, decanediamine, antioxidant 168, sodium hypophosphite and deionized water in a mass ratio of 1:1.3:0.005:0.007:0.5 to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0095] S2. Replace the air inside the autoclave with an inert gas, and reserve 0.8 MPa of inert gas after repeating three times. Rise the temperature to 230°C for polycondensation reaction in three stages, wherein the first stage is from room temperature to 190°C; the second stage is from 190°C to 210°C; the third stage is from 210°C to 230°C, and each stage is heated to the target temperature and kept isothermal for 1 hour; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 15%;
[0096] S3. After depressurizing the reactor, maintain heating at 190° C. for 2 h, and then cool and discharge the material to obtain a PA1012 material with a γ crystal structure.
[0097] Embodiment 4
[0098] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, wherein the prepared polyamide material is PA1012, the melting temperature of PA1012 is 189° C., and the thermal decomposition temperature is 406° C., and the method specifically comprises the following steps:
[0099] S1, mixing dodecanedioic acid, decanediamine, antioxidant 4010, sodium hypophosphite and deionized water in a mass ratio of 1:1.2:0.005:0.005:0.5 to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0100] S2. Replace the air inside the autoclave with an inert gas, repeat three times and reserve 0.1 MPa of inert gas, and heat the mixture to 220°C for polycondensation reaction in three stages, wherein the first stage is from room temperature to 180°C; the second stage is from 180°C to 200°C; the third stage is from 200°C to 220°C, and each stage is heated to the target temperature and kept isothermal for 2 hours; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 8%;
[0101] S3. After depressurizing the reactor, maintain heating at 200° C. for 2 h, and then cool and discharge the material to obtain a PA1012 material with a γ crystal structure.
[0102] Embodiment 5
[0103] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, wherein the prepared polyamide material is PA610, the melting temperature of PA610 is 222° C., and the thermal decomposition temperature is 420° C., and the method specifically comprises the following steps:
[0104] S1, mixing sebacic acid, hexamethylenediamine, antioxidant DNP, sodium hypophosphite and deionized water in a mass ratio of 1:1.1:0.002:0.01:0.5 to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0105] S2. Replace the air inside the autoclave with an inert gas, and reserve 1 MPa of inert gas after repeating three times. Raise the temperature to 240°C for polycondensation reaction in three stages, wherein the first stage is from room temperature to 200°C; the second stage is from 200°C to 220°C; the third stage is from 220°C to 240°C, and each stage is heated to the target temperature and kept isothermal for 3 hours; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 10%;
[0106] S3. After the reactor is depressurized, the temperature is maintained at 230° C. for 1 hour, and then the material is cooled and discharged to obtain a PA610 material having a γ crystal structure.
[0107] Embodiment 6
[0108] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, wherein the prepared polyamide material is PA610, the melting temperature of PA610 is 222° C., and the thermal decomposition temperature is 420° C., and the method specifically comprises the following steps:
[0109] S1, mixing sebacic acid, hexamethylenediamine, antioxidant 1035, sodium hypophosphite and deionized water in a mass ratio of 1:1.3:0.002:0.007:0.3 to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0110] S2. Replace the air inside the autoclave with an inert gas, and reserve 0.8 MPa of inert gas after repeating three times. Rise the temperature to 240°C in three stages for polycondensation reaction, wherein the first stage is from room temperature to 200°C; the second stage is from 200°C to 220°C; the third stage is from 220°C to 240°C, and each stage is heated to the target temperature and kept isothermal for 2 hours; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 20%;
[0111] S3. After the reactor is depressurized, the temperature is maintained at 230° C. for 2 h, and then the material is cooled and discharged to obtain a PA610 material having a γ-crystal structure.
[0112] Embodiment 7
[0113] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0114] The polyamide material PA1212 was placed in a vacuum oven and dried at 75°C for 20 hours. The constant weight method test confirmed that the weight of PA1212 no longer changed. PA1212 was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 185°C. During the post-polymerization process, the solid phase viscosity increasing device was maintained in a high-purity nitrogen atmosphere. The post-polymerization time was 8 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0115] Embodiment 8
[0116] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0117] The polyamide material PA610 was placed in a vacuum oven and dried at 105°C for 11 hours. The constant weight method test confirmed that the weight of PA610 no longer changed. PA610 was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 225°C. The solid phase viscosity increasing device was maintained in a vacuum state during the post-polymerization process. The post-polymerization time was 6 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0118] Embodiment 9
[0119] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0120] The polyamide material PA612 was placed in a vacuum oven and dried at 100°C for 18 hours. The constant weight method test confirmed that the weight of PA612 no longer changed. PA612 was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 215°C. The solid phase viscosity increasing device was maintained in a vacuum state during the post-polymerization process. The post-polymerization time was 7 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0121] Embodiment 10
[0122] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0123] A composite of polyamide material PA1212 and a nucleating agent is placed in a vacuum oven, wherein the amount of the nucleating agent is 0.5wt% of PA1212, and dried at 105°C for 10 hours. The constant weight method test confirms that the weight of the composite no longer changes. The composite is taken out and placed in a solid phase viscosity increasing device, and post-polymerized at 160°C. During the post-polymerization, the solid phase viscosity increasing device is maintained in a vacuum state. The post-polymerization time is 5 hours. After the post-polymerization, it is cooled to room temperature to obtain a polyamide material with a γ crystal structure.
[0124] Embodiment 11
[0125] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0126] The polyamide material PA1212 / PP alloy was placed in a vacuum oven and dried at 100°C for 24 hours. The constant weight method test confirmed that the weight of the PA1212 / PP alloy no longer changed. The PA1212 / PP alloy was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 189°C. The solid phase viscosity increasing device was maintained in a vacuum state during the post-polymerization process. The post-polymerization time was 6 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0127] Embodiment 12
[0128] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0129] The polyamide material PA1010 / glass fiber composite material was placed in a vacuum oven and dried at 100°C for 24 hours. The constant weight method test confirmed that the weight of the PA1010 / glass fiber composite material no longer changed. The PA1010 / glass fiber composite material was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 200°C. During the post-polymerization, the solid phase viscosity increasing device was maintained in a vacuum state. The post-polymerization time was 3 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0130] Embodiment 13
[0131] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0132] The polyamide material PA1214 was placed in a vacuum oven and dried at 100°C for 18 hours. The constant weight method test confirmed that the weight of PA1214 no longer changed. PA1214 was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 165°C. The solid phase viscosity increasing device was maintained in a vacuum state during the post-polymerization process. The post-polymerization time was 3 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0133] Embodiment 14
[0134] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0135] The polyamide material PA612 was placed in a vacuum oven and dried at 95°C for 20 hours. The constant weight method test confirmed that the weight of PA612 no longer changed. PA612 was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 200°C. The solid phase viscosity increasing device was maintained in a vacuum state during the post-polymerization process. The post-polymerization time was 10 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0136] Embodiment 15
[0137] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0138] First, the polyamide material PA1012 is placed in a vacuum oven and dried at 95°C for 24 hours. The constant weight method test confirms that the weight of PA1012 no longer changes. Then, the PA1012 is heated to 230°C to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reaches 230°C, it is cooled to 120°C at a cooling rate of 60°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0139] The crystal structure of the polyamide material with γ crystal structure obtained in Example 15 was characterized by WAXD. The characterization results are as follows: Figure 1 and Figure 2 As shown, Figure 2 Figure a in the figure is the WAXD characterization result of the polyamide material with γ crystal structure prepared in this embodiment, and Figure b is the WAXD characterization result of the polyamide material obtained by conventional heat treatment using the same polyamide material as in this embodiment. It can be seen from the figure that the crystal structure of the polyamide material prepared by the method in Example 15 has changed from α crystal to γ crystal. Figure 2 The interplanar spacing of different crystal faces corresponding to the α and γ crystal forms is processed to obtain the average grain size of each crystal form as follows:
[0140]
[0141] It can be seen that the average grain size of γ crystal is much smaller than that of α crystal, which further indicates that the light transmittance of polyamide material with γ crystal form is higher and the material is transparent as a whole.
[0142] Furthermore, the mechanical properties of the polyamide material before and after being treated by the method of Example 15 were tested, and the results were as follows:
[0143]
[0144] It should be noted that in the above table, "after treatment" refers to the polyamide material prepared according to the embodiment scheme, and "before treatment" refers to the sample that has been cooled to room temperature at a slow rate (2°C / min) after the thermal history has been eliminated under the same conditions.
[0145] From the table and Figure 3 It can be seen that the elastic modulus and yield strength of the polyamide material treated by the method described in Example 15 are reduced while the elongation at break and toughness are improved compared with those before treatment, indicating that the generation of the γ crystal form significantly improves the deformation ability and toughness of the material.
[0146] Embodiment 16
[0147] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0148] First, the polyamide material PA1012 is placed in a vacuum oven and dried at 85°C for 24 hours. The constant weight method test confirms that the weight of PA1012 no longer changes. Then, the PA1012 is heated to 240°C to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reaches 240°C, it is cooled to 100°C at a cooling rate of 60°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0149] Embodiment 17
[0150] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0151] Firstly, the polyamide material PA610 was placed in a vacuum oven and dried at 105°C for 8 hours. The constant weight method test confirmed that the weight of PA610 no longer changed. Then, the PA610 was heated to 250°C to eliminate the thermal history, and the air was continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reached 250°C, it was cooled to room temperature by quenching to obtain a polyamide material with a γ crystal form.
[0152] Embodiment 18
[0153] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0154] First, the polyamide material PA612 is placed in a vacuum oven and dried at 100°C for 12 hours. The constant weight method test confirms that the weight of PA612 no longer changes. Then, the PA612 is heated to 250°C to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reaches 250°C, it is cooled to 130°C at a cooling rate of 80°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0155] Embodiment 19
[0156] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0157] First, a composite of polyamide material PA612 and a chain extender is placed in a vacuum oven and dried at a temperature of 100°C for 12 hours. The constant weight method test confirms that the weight of the composite of PA612 and the chain extender no longer changes, wherein the chain extender accounts for 0.5wt% of PA612; then the composite of PA612 and the chain extender is heated to 250°C to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reaches 250°C, it is cooled to 80°C at a cooling rate of 100°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0158] Embodiment 20
[0159] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0160] First, the polyamide material PA1210 is placed in a vacuum oven and dried at 90°C for 24 hours. The constant weight method test confirms that the weight of PA1210 no longer changes. Then, the PA1210 is heated to 230°C to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reaches 230°C, it is cooled to 100°C at a cooling rate of 100°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0161] Embodiment 21
[0162] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0163] First, the polyamide material PA1212 is placed in a vacuum oven and dried at 90°C for 24 hours. The constant weight method test confirms that the weight of PA1212 no longer changes. Then, the PA1212 is heated to 220°C to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reaches 220°C, it is cooled to 50°C at a cooling rate of 100°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0164] Embodiment 22
[0165] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0166] Firstly, the polyamide material PA1214 was placed in a vacuum oven and dried at 100°C for 18 hours. The constant weight method test confirmed that the weight of PA1214 no longer changed. Then, the PA1214 was heated to 220°C to eliminate the thermal history, and the air was continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reached 220°C, it was cooled to 130°C at a cooling rate of 60°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0167] Embodiment 23
[0168] As another embodiment of the present invention, this embodiment provides a method for preparing a highly transparent and high-toughness polyamide material, which is specifically as follows.
[0169] First, the polyamide material PA66 is placed in a vacuum oven and dried at 100°C for 24 hours. The constant weight method test confirms that the weight of PA66 no longer changes. Then, the PA66 is heated to 290°C to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain an inert atmosphere. After the temperature reaches 290°C, it is cooled to 150°C at a cooling rate of 100°C / min, and then naturally cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0170] Embodiment 24
[0171] This comparative example adopts the same preparation method as that of Example 7, and the only difference from Example 7 is that the polyamide material with γ crystal structure prepared in Example 1 is subjected to post-polymerization reaction.
[0172] S1, mixing adipic acid, hexamethylenediamine, antioxidant 1098, sodium hypophosphite and deionized water (mass ratio 1:1.2:0.005:0.005:0.3) to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0173] S2. Replace the air inside the autoclave with an inert gas, and reserve 1 MPa of inert gas after repeating three times. Rise the temperature to 280°C for polycondensation reaction in three stages, wherein the first stage is from room temperature to 200°C; the second stage is from 200°C to 240°C; the third stage is from 240°C to 280°C, and each stage is heated to the target temperature and kept isothermal for 2 hours; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 10%;
[0174] S3. After depressurizing the reactor, maintain heating at 260°C for 1 hour, then cool and discharge the material to obtain the raw material of PA66.
[0175] The polyamide material PA66 was placed in a vacuum oven and dried at 75°C for 20 hours. The constant weight method test confirmed that the weight of PA66 no longer changed. PA66 was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 200°C. During the post-polymerization process, the solid phase viscosity increasing device was maintained in a high-purity nitrogen atmosphere. The post-polymerization time was 8 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal structure.
[0176] Embodiment 25
[0177] This comparative example adopts the same preparation method as that of Example 8, and the only difference from Example 8 is that the polyamide material with γ crystal structure prepared in Example 4 is subjected to post-polymerization reaction.
[0178] S1, mixing dodecanedioic acid, decanediamine, antioxidant 4010, sodium hypophosphite and deionized water (mass ratio 1:1.2:0.005:0.005:0.5) to obtain a raw material mixture, and adding the raw material mixture into a high-pressure reactor;
[0179] S2. Replace the air inside the autoclave with an inert gas, repeat three times and reserve 0.1 MPa of inert gas, and heat the mixture to 220°C for polycondensation reaction in three stages, wherein the first stage is from room temperature to 180°C; the second stage is from 180°C to 200°C; the third stage is from 200°C to 220°C, and each stage is heated to the target temperature and kept isothermal for 2 hours; at the same time, in the third stage, oscillating shear is applied to the raw material mixture, and the amplitude of the oscillating shear is 8%;
[0180] S3. After depressurizing the reactor, maintain heating at 200°C for 2 hours, and then cool and discharge the material to obtain the raw material of PA1012.
[0181] The polyamide material PA1012 was placed in a vacuum oven and dried at 100°C for 9 hours. The constant weight method test confirmed that the weight of PA1012 no longer changed. PA1012 was taken out and placed in a solid phase viscosity increasing device for post-polymerization at 145°C. The solid phase viscosity increasing device was maintained in a vacuum state during the post-polymerization process. The post-polymerization time was 3 hours. After the post-polymerization, it was cooled to room temperature to obtain a polyamide material with a γ crystal form.
[0182] The mechanical properties of the polyamide materials with γ crystal structure prepared in the above embodiments are tested, and the results are shown in the following table. It should be noted that the elongation at break and toughness in the table refer to the performance of the polyamide materials prepared under the same preparation process without oscillating shearing treatment as the benchmark, and the performance improvement ratio is as follows:
[0183]
[0184]
[0185] Next, various experimental examples are used for further analysis and explanation. It should be noted that the elongation at break and toughness in the following tables refer to the performance improvement ratio compared with the performance of polyamide materials obtained under the same preparation process without oscillating shear treatment.
[0186] Experimental Example 1
[0187] This experimental example is based on Example 1, and only the amplitude during the preparation process is changed to obtain different polyamide materials. The specific amplitude during the preparation of each polyamide material and the properties of the obtained polyamide materials are shown in the following table:
[0188] amplitude Increase rate of elongation at break Toughness improvement rate Transmittance % 10% 60% 60% 80% 20% 105% 90% 90% 30% 80% 80% 80% 35% 70% 70% 60% 1% 10% 5% 50% 0% 0% 0% 40%
[0189] From the above comparison results, it can be seen that the polyamide material with γ crystal form can be controlled by oscillating shearing treatment, and its tensile strength and toughness are significantly improved compared with the polyamide material obtained without oscillating shearing treatment; and it has a higher light transmittance; and it can be further seen that the amplitude applied during the polycondensation reaction is too small to play a role in regulating the crystal form, so the improvements in elongation at break, toughness and transmittance are limited; at the same time, it can also be seen that the larger the amplitude, the better. With the increase of the amplitude, the elongation at break, toughness and transmittance show an overall trend of first increasing and then decreasing, indicating that an amplitude applied that is too large can cause the product to degrade and will also affect the final performance of the polyamide material.
[0190] Experimental Example 2
[0191] This experimental example is based on Example 1, and only the temperature of each heating stage in the preparation process is changed to obtain different polyamide materials. The specific amplitudes in the preparation process of each polyamide material and the properties of the obtained polyamide materials are shown in the following table:
[0192]
[0193] From the above comparison results, it can be seen that within the range of 260-280°C, the formation of the γ crystal can be promoted by increasing the temperature, thereby improving the performance of the polyamide material, while the performance decreases when the temperature reaches 290°C. Combined with the polyamide material prepared in Example 1, which is PA66 and has a melting temperature of 257°C, it can be seen that when the temperature of the polycondensation reaction is between 20°C below the melting temperature and 30°C above the melting temperature, it can significantly affect the generation of the γ crystal. Outside this temperature range, although the γ crystal is also generated, it may decompose due to excessively high temperature, or the temperature is too low to affect the effect of oscillating shear, resulting in a decrease in material performance.
[0194] At the same time, it can be seen that the three-stage heating method is more conducive to the smooth production of the γ crystal form, and the performance of the polyamide material prepared by one-time heating is significantly reduced.
[0195] Experimental Example 3
[0196] This experimental example is based on Example 1, and only changes the duration of each heating stage in the preparation process to obtain different polyamide materials. The specific amplitudes in the preparation process of each polyamide material and the properties of the obtained polyamide materials are shown in the following table:
[0197]
[0198] From the above comparison results, we can see that:
[0199] When applying oscillatory shearing to the raw material mixture in the second and third temperature rising stages, excessively long oscillatory shearing time may lead to degradation of the product.
[0200] Experimental Example 4
[0201] This experimental example is based on Example 1, except that the number of heating stages and the number of heating stages for oscillating shearing treatment are changed to obtain different polyamide materials. The specific amplitudes in the preparation process of each polyamide material and the properties of the obtained polyamide materials are shown in the following table:
[0202]
[0203]
[0204] From the above comparison results, it can be seen that the γ crystal form can be formed in the polyamide material through the oscillation shearing treatment, thereby improving the mechanical properties and transmittance of the polyamide material, and it can also be seen that when the oscillation shearing time is constant, the performance of the polyamide material can be significantly affected by changing the distribution of the oscillation shearing time; if the oscillation shearing is concentrated in the second heating stage, it cannot be guaranteed that the system in the reactor is in a sheared state before the end of the polycondensation reaction, and thus a stable γ crystal form cannot be produced; it can also be seen that the same oscillation shearing time is divided into two parts, and the oscillation shearing is performed in the second heating stage and the third heating stage respectively, and the performance of the polyamide material can be further improved by reasonably allocating the oscillation shearing time in the two heating stages; among them, a longer time is allocated to the second heating stage, and a shorter oscillation shearing time is allocated to the third heating stage. Since the temperature in the third heating stage is higher, the short-term oscillation shearing promotes the formation of γ crystals while avoiding the product degradation caused by long-term oscillation shearing, thereby obtaining a polyamide material with better performance.
[0205] Experimental Example 5
[0206] This experimental example is based on the preparation method of Example 7, and only changes the temperature of the post-polymerization reaction to obtain different polyamide materials. The specific temperature during the post-polymerization reaction and the properties of the obtained polyamide materials are shown in the following table:
[0207]
[0208]
[0209] From the above comparison results, it can be seen that the post-polymerization temperature has a significant effect on the formation of the γ crystal form. The higher the post-polymerization temperature, the more conducive it is to perfecting the γ crystal form inside the amide, and further improving the mechanical properties and transmittance of the material.
[0210] Experimental Example 6
[0211] This experimental example is based on the preparation method of Example 15, and different polyamide materials are obtained by only changing the cooling rate. The specific cooling rate and the properties of the obtained polyamide materials are shown in the following table:
[0212] Cooling rate (% / min) Increase rate of elongation at break Toughness improvement rate Transmittance % 60 103% 60% 95% 100 110% 100% 90% Liquid nitrogen quenching 110% 100% 95% 20 40% 30% 50% 40 60% 50% 60% 5 0% 0% 20%
[0213] From the above comparison results, it can be seen that the cooling rate will also have a great influence on the formation of γ crystal form. This is because changing the cooling rate can control the order of subsequent hydrogen bonds. It can be further seen that the faster the cooling rate, the better the performance of the polyamide material.
[0214] Experimental Example 7
[0215] This experimental example is based on the preparation method of Example 15, and different polyamide materials are obtained by only changing the target temperature of cooling. The specific target temperature of cooling and the properties of the obtained polyamide materials are shown in the following table:
[0216]
[0217] From the above comparison results, it can be seen that different target temperatures at a specific cooling rate will also affect the performance of the material. The lower the target temperature, the better the performance of the polyamide material, indicating that more γ crystals are generated inside.
[0218] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A method for preparing a highly transparent and high-toughness polyamide material, characterized in that: The following steps are included: S1, mixing a dibasic acid, a diamine, deionized water, a catalyst and an antioxidant to obtain a raw material mixture; S2, heating the raw material mixture to a first preset temperature under a preset pressure condition to allow the raw material mixture to undergo a polycondensation reaction, and performing an oscillation shearing treatment on the raw material mixture during the heating process; S3, after the polycondensation reaction is completed, the material is cooled and discharged to obtain a polyamide material having a γ crystal structure; The dibasic acid and diamine in the raw material mixture are dibasic acids and diamines having an even number of carbon atoms in the main chain; In step S2, the temperature of the polycondensation reaction is raised from room temperature to a first preset temperature, the first preset temperature being between 80° C. below the melting temperature of the polyamide material having a γ-crystal form and the starting thermal decomposition temperature, and after the temperature of the polycondensation reaction reaches the melting temperature of the polyamide material having a γ-crystal form, the raw material mixture is subjected to an oscillating shearing treatment; the amplitude range of the oscillating shearing treatment is 3-30%; The prepared polyamide material with gamma crystal form is one of PA66, PA610 and PA612, or a polyamide in which the number of methylene groups between adjacent amide groups on the main chain is not less than 10.
2. The method for preparing a highly transparent and high-toughness polyamide material according to claim 1, characterized in that: The antioxidant is a mixture of one or more of a phenolic antioxidant, an amine antioxidant, a metal ion passivator, or a peroxide decomposer.
3. The method for preparing a highly transparent and high-toughness polyamide material according to claim 2, characterized in that: The phenolic antioxidant is antioxidant 1010, antioxidant 1098, antioxidant 1035 or antioxidant 1093; the amine antioxidant is antioxidant DNP or antioxidant 4010; the metal ion passivator is copper acetate / potassium iodide; and the peroxide decomposer is antioxidant 168.
4. The method for preparing a highly transparent and high-toughness polyamide material according to claim 1, characterized in that: The catalyst is sodium hypophosphite.
5. The method for preparing a highly transparent and high-toughness polyamide material according to claim 1, characterized in that: The first preset temperature is between 20° C. below the melting temperature of the polyamide material having the γ crystalline phase and 30° C. above the melting temperature.
6. The method for preparing a highly transparent and high-toughness polyamide material according to any one of claims 1 to 5, characterized in that: In step S2, during the polycondensation reaction, the polycondensation reaction temperature is raised to a first preset temperature by a staged heating method, wherein the temperature of at least one heating stage is higher than the melting temperature of the polyamide material having the γ crystal form.
7. The method for preparing a highly transparent and high-toughness polyamide material according to claim 6, characterized in that: The segmented heating process includes at least two heating stages above the melting temperature of the polyamide material with γ crystal form, and at least one of the heating stages is subjected to oscillating shearing treatment.
8. The method for preparing a highly transparent and high-toughness polyamide material according to claim 7, characterized in that: The last heating stage is an oscillating shearing treatment.
9. The method for preparing a highly transparent and high-toughness polyamide material according to claim 7, characterized in that: The heating stage includes the first heating stage, the second heating stage and the third heating stage in which the temperature is increased successively. The second heating stage and the third heating stage are both subjected to oscillation shearing treatment, wherein the duration of oscillation shearing treatment in the third heating stage is shorter than that in the second heating stage.
10. The method for preparing a highly transparent and high-toughness polyamide material according to claim 6, characterized in that: The duration of each heating stage ranges from 1 to 5 hours; the total duration of the oscillation shearing treatment does not exceed 2 hours.
11. The method for preparing a highly transparent and high-toughness polyamide material according to claim 10, characterized in that: The duration of each heating stage ranges from 2 to 3 hours; the total duration of the oscillating shearing treatment is from 0.5 to 1 hour; and the amplitude range of the oscillating shearing treatment is 20%.
12. The method for preparing the high-transparency and high-toughness polyamide material according to any one of claims 1 to 5, characterized in that: In step S2, before heating, the air is replaced by an inert gas, and a portion of the inert gas is reserved to reach a preset pressure, and then the temperature is raised to carry out a polycondensation reaction, and the preset pressure range is 0.05-1.0 MPa.
13. The preparation method according to any one of claims 1 to 5, characterized in that: The prepared polyamide material with γ crystal form is one of PA1010, PA1012, PA1210, PA1212 or PA1214.
14. A method for preparing a highly transparent and high-toughness polyamide material, characterized in that: The polyamide material prepared by any preparation method as described in any one of claims 1 to 13 is placed in a solid phase viscosity enhancement device for post-polymerization reaction; a polyamide material with a γ crystal structure is obtained by adjusting the temperature of the post-polymerization reaction, wherein the temperature during the post-polymerization reaction is between the glass transition temperature and the melting temperature of the polyamide material.
15. The preparation method according to claim 14, characterized in that: The duration of the post-polymerization reaction is 1-14 hours.
16. The preparation method according to claim 15, characterized in that: The duration of the post-polymerization reaction is 2-8h.
17. A method for preparing a highly transparent and high-toughness polyamide material, characterized in that: After the polyamide material is completely dehydrated, the temperature is raised to above the melting point in an inert atmosphere to eliminate the thermal history, and the air is continuously replaced before and during the heating process to maintain the inert atmosphere; then the temperature is lowered at a rate of not less than 60°C / min to below 40°C below the melting point of the polyamide material to obtain a polyamide material with a γ crystal form; Alternatively, after the polyamide material is completely dehydrated, the temperature is raised to a second preset temperature under an inert atmosphere, and then the polyamide material is heat treated by keeping the temperature, and then the temperature is lowered to 40° C. below the melting point of the polyamide material at a rate of not less than 60° C. / min to obtain a polyamide material with a γ crystal structure; the inert atmosphere is high-purity helium, high-purity nitrogen or high-purity argon; The prepared polyamide material with gamma crystal form is one of PA66, PA610 and PA612, or a polyamide in which the number of methylene groups between adjacent amide groups on the main chain is not less than 10.
18. The preparation method according to claim 17, characterized in that: The inert atmosphere is high-purity helium or high-purity nitrogen.
19. The preparation method according to claim 18, characterized in that: The temperature is lowered to room temperature at a rate of not less than 60°C / min to obtain a polyamide material with a γ crystal structure.
20. The method for preparing a highly transparent and high-toughness polyamide material according to claim 17, characterized in that: The second preset temperature is between the melting temperature of the polyamide material and 30° C. above the melting temperature, and the heat treatment time is 5-30 minutes.
21. The preparation method according to claim 17, characterized in that: The prepared polyamide material with γ crystal form is one of PA1010, PA1012, PA1210, PA1212 or PA1214.
22. A highly transparent and high-toughness polyamide material prepared by the preparation method according to any one of claims 1 to 21, characterized in that: The elongation at break of the polyamide material with the γ crystal form is 101-210% of that of the conventional polyamide material, the toughness is 101-200% of that of the conventional polyamide material, and the light transmittance is 80%-100%.