A multi-element transition metal compound electrocatalyst material and preparation method thereof

By growing multivariate transition metal oxide AWO4@BxOy type electrocatalysts with abundant oxygen defects in situ on the metal oxide matrix, the scarcity of precious metal catalyst resources and the stability of non-precious metal-based electrocatalysts are solved, and high-efficiency and low-cost electrolysis is achieved Hydrogen production effect.

CN115700300BActive Publication Date: 2024-11-05ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211492775.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-11-05
Estimated Expiration
2042-11-25
Patent Text Reader

Abstract

The present invention belongs to the technical field of electrocatalyst materials, and specifically relates to a multinary transition metal compound electrocatalyst material and a preparation method thereof. The present invention uses metal oxides of various morphologies as substrates, and constructs a tungsten-based multinary metal oxide with a specific morphology and rich in oxygen defects by in-situ growth, thereby improving the conductivity and activity of current metal compound-based electrocatalysts. Under the synergistic effect of multiple components, high-efficiency electrocatalytic performance superior to that of precious metal catalysts is obtained, and the material has excellent structure and cycle stability. The present invention provides a solution to the problems of excessively high cost, insufficient structural stability and insufficient activity of current electrocatalysts. The material preparation method is simple, easy to operate, and low in cost. The prepared catalyst does not contain precious metals and can be applied on a large scale to industrial water electrolysis for hydrogen production under high current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrocatalyst materials, and in particular relates to a multi-component transition metal compound electrocatalyst material and a preparation method thereof. Background Art

[0002] The technology for producing hydrogen by electrolysis of water is already mature, and there is no pollution or carbon emissions during the hydrogen production process. It is an important part of the national hydrogen energy strategy. Therefore, the development of the technology for producing hydrogen by electrolysis of water is also receiving more and more attention.

[0003] However, the precious metal catalysts such as Pt, Pd, Ru, and Rh currently used in water electrolysis for hydrogen production are scarce and their costs remain high, becoming the main constraint on industrial water electrolysis for hydrogen production. In order to develop non-precious metal-based electrocatalysts that can match the performance of precious metal catalysts, the mainstream research direction is focused on transition metal oxides, sulfides, phosphides, etc., especially multi-metal oxide electrocatalysts such as NiWO4, which have been studied more recently, showing relatively excellent catalytic activity. However, multi-metal oxide materials still have obvious shortcomings that need to be addressed, such as structural stability problems, conductivity problems, and durability problems. These problems seriously restrict the further application of non-precious metal-based catalysts.

[0004] Therefore, in order to address these current problems, it is urgent to develop an electrocatalyst with stable structure, high conductivity and good durability. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a highly efficient non-precious metal electrocatalytic hydrogen production catalyst material with a morphology and structure that can be controlled and rich in oxygen defects, and a preparation method thereof. The present invention uses metal oxides with different morphologies and structures as a matrix, and by regulating the reaction system, finally in situ grows a highly efficient non-precious metal-based multi-element transition metal oxide AWO4@B with rich oxygen defects on the matrix. x O y The preparation process of the present invention is simple and efficient, with a short cycle and reasonable cost, and is suitable for large-scale production and application.

[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0007] The present invention provides a multi-element transition metal compound electrocatalyst material, the electrocatalyst material is composed of AWO4@B x O y ,in,

[0008] AWO4 is the main catalyst, and A is any one of Fe, Co, Ni, and Cu;

[0009] B x Oy is a substrate, comprising any one or more oxide combinations of Fe, Co, Ni, and Cu; 1≤x≤3, 1≤y≤4;

[0010] AWO4 and B x O y The mass ratio is controlled at 10:1 to 1:20;

[0011] The same elements in A and B do not appear at the same time.

[0012] Further, as mentioned above, the main catalyst AWO4 is B x O y It is grown in situ on the substrate, and the two have a strong interaction.

[0013] Furthermore, in the electrocatalyst material as described above, the substrate B x O y The metal oxide material is in the form of at least one of nanoparticles, nanowires, nanorods, nanobelts, nanosheets, nanospheres and foam network structures.

[0014] The present invention also provides a method for preparing an electrocatalyst material, comprising the following steps:

[0015] 1) Weigh an appropriate amount of B x O y Place in a pressure reaction vessel, prepare the A precursor and the tungsten source into an aqueous solution according to the A:W atomic ratio of 1:1 and transfer into the pressure reaction vessel, add an appropriate amount of ammonium fluoride to adjust the pH value of the system, then react at a temperature of 100 to 200° C. for 6 to 24 hours, and cool with the furnace to obtain a reaction product;

[0016] 2) After filtering and washing the reaction product, the reaction product is transferred to a vacuum drying oven and dried at 60 to 100° C. for 8 to 24 hours; then the reaction product is transferred to a tube furnace and heated to 300 to 600° C. at a heating rate of 1 to 10° C. / min and fully calcined for 1 to 5 hours to obtain a calcined product;

[0017] 3) Then, during the cooling process of the calcined product, a hydrogen-argon mixed gas was introduced for a certain period of time to purge and activate the product, thereby obtaining AWO4@B x O y type electrocatalyst.

[0018] Furthermore, in step 1), the A precursor includes at least one of A metal nitrate and A metal halide.

[0019] Furthermore, in step 1), the tungsten source includes at least one of ammonium metatungstate and sodium tungstate.

[0020] Furthermore, in step 1), the ammonium fluoride adjusts the pH value of the system to 3 to 6; the reaction product is in the solution system within the pH range at B x O y The morphology and structure of the AWO4 amorphous solid grown in situ on the substrate are affected by the morphology and structure of the substrate and the pH value of the solution system.

[0021] Furthermore, in step 2), the calcined product is AWO4@B having abundant oxygen defects. x O y Crystalline solid.

[0022] Furthermore, in step 3), the concentration of hydrogen in the hydrogen-argon mixed gas is controlled at 5-15%, and the purge activation time is controlled at 15-120 minutes.

[0023] The present invention also provides application of the electrocatalyst material in catalyzing the electrolysis of water to produce hydrogen in the full pH range.

[0024] The beneficial effects of the present invention are:

[0025] 1. The present invention uses non-precious metal oxides with different morphologies and structures as the matrix. On the one hand, they are widely available and low in cost, which can effectively reduce the cost of the catalyst. On the other hand, non-precious metal-based multi-metal oxides are in situ grown on the matrix, and their morphologies and structures are controllable and have excellent performance. Catalytic performance that is superior to that of precious metal catalysts can be obtained, and the preparation process is also simplified.

[0026] 2. The present invention uses a nanoscale matrix with a high specific surface area for in-situ growth, which can generate a large number of active oxygen vacancies, thereby further improving the activity of the electrocatalyst.

[0027] 3. All raw materials of the present invention are widely available, low in cost, simple in process, short in cycle, and high in yield, which can effectively reduce the cost of electrocatalysts and can be applied on a large scale to produce hydrogen by electrolysis of water.

[0028] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention uses metal oxides of various morphologies as substrates, and constructs tungsten-based multi-metal oxides with specific morphology and rich oxygen defects by in-situ growth, thereby improving the conductivity and activity of current metal compound-based electrocatalysts. Under the synergistic effect of multiple components, high-efficiency electrocatalytic performance superior to that of precious metal catalysts is obtained, and the catalyst has excellent structure and cycle stability. The present invention provides a solution to the current problems of high cost, structural stability and insufficient activity of electrocatalysts. The material preparation method is simple, easy to operate, and low in cost. The prepared catalyst does not contain precious metals and can be applied on a large scale to industrial water electrolysis to produce hydrogen under high current density.

[0031] The relevant specific embodiments of the present invention are as follows:

[0032] Example 1

[0033] Weigh 0.2 g of porous Co3O4 nanobelt powder with high specific surface area and place it in a pressure reactor, add 60 ml of mixed solution prepared with nickel nitrate and ammonium metatungstate according to the Ni:W atomic ratio of 1:1, and add the mixed solution, the total amount of nickel nitrate and ammonium metatungstate is 0.5 g, then add 0.2 g of ammonium fluoride to fully dissolve, cover the reactor tightly, transfer to a 120°C drying oven, react for 12 hours, and obtain amorphous NiWO4 / Co3O4 solid after cooling;

[0034] The mixture was filtered and washed with deionized water and ethanol until neutral, transferred to an 80°C drying oven for overnight drying, and then transferred to a muffle furnace, heated to 400°C at a heating rate of 5°C / min and fully calcined for 3h, and cooled in the furnace to obtain crystalline NiWO4 / Co3O4 powder;

[0035] The obtained crystalline NiWO4 / Co3O4 powder was transferred to a tubular furnace, the gas was evacuated, and then purged and activated for 60 minutes in a hydrogen atmosphere at 400°C to obtain a flower-like NiWO4 / Co3O4 type electrocatalyst uniformly distributed on the nanobelts.

[0036] Finally, the obtained NiWO4 / Co3O4 electrocatalyst was subjected to HER and water electrolysis performance tests in a KOH alkaline solution environment with a pH of 14. The following results were obtained: at a standard current density of 10 mA / cm 2 Under the condition of 10,000 cycles, the overpotential is 36mV, and after 10,000 cycles, the overpotential becomes 45mV; the current density of water electrolysis reaches 10mA / cm 2 The required overpotential is 1.42V.

[0037] Example 2

[0038] Weigh 0.3 g of porous CuO nanosheet powder with high specific surface area and place it in a pressure reactor, add 80 ml of mixed solution prepared with cobalt nitrate and ammonium metatungstate at a Co:W atomic ratio of 1:1, and add the mixed solution. The total amount of nickel nitrate and ammonium metatungstate is 0.45 g. Then, add 0.3 g of ammonium fluoride to fully dissolve it. Cover the reactor tightly and transfer it to a drying oven at 100°C for reaction for 12 hours. After cooling, obtain an amorphous CoWO4 / CuO solid.

[0039] The mixture was filtered and washed with deionized water and ethanol until neutral, transferred to an 80°C drying oven for overnight drying, and then transferred to a muffle furnace, heated to 500°C at a heating rate of 10°C / min and fully calcined for 2h, and cooled in the furnace to obtain crystalline CoWO4 / CuO powder;

[0040] The obtained crystalline CoWO4 / CuO powder was transferred to a tubular furnace, the gas was evacuated, and then purged and activated in a hydrogen atmosphere at 400°C for 90 minutes to obtain a clustered CoWO4 / CuO electrocatalyst uniformly distributed on the nanosheets.

[0041] Finally, the obtained CoWO4 / CuO electrocatalyst was tested for HER and water electrolysis performance in a KOH alkaline environment with a pH of 12. The following results were obtained: 2 Under the condition of 10,000 cycles, the overpotential is 55mV, and after 10,000 cycles, the overpotential becomes 66mV; the current density of water electrolysis reaches 10mA / cm 2 The required overpotential is 1.52V.

[0042] Example 3

[0043] Weigh 0.3 g of porous NiO nanorod powder with high specific surface area and place it in a pressure reactor, add 70 ml of mixed solution prepared with cobalt nitrate and sodium tungstate at a Co:W atomic ratio of 1:1, and add the solution, the total amount of nickel nitrate and ammonium metatungstate is 0.45 g, then add 0.3 g of ammonium fluoride, cover the reactor tightly, transfer to a 100°C drying oven, react for 12 h, and obtain amorphous CoWO4 / NiO solid after cooling;

[0044] The mixture was filtered and washed with deionized water and ethanol until neutral, transferred to an 80°C drying oven for overnight drying, and then transferred to a muffle furnace, heated to 500°C at a heating rate of 10°C / min and fully calcined for 2h, and cooled in the furnace to obtain crystalline CoWO4 / NiO powder;

[0045] The obtained crystalline CoWO4 / NiO powder was transferred to a tubular furnace, the gas was evacuated, and then purged and activated for 30 minutes in a hydrogen atmosphere at 500°C to obtain a flower-like CoWO4 / NiO electrocatalyst uniformly distributed on the nanorods.

[0046] Finally, the obtained CoWO4 / NiO electrocatalyst was tested for HER and water electrolysis performance in an acidic environment of sulfuric acid solution with a pH of 1. The following results were obtained: 2 Under the condition of 1000 cycles, the overpotential is 65mV, and after 5000 cycles, the overpotential becomes 70mV; the current density of water electrolysis reaches 10mA / cm 2 The required overpotential is 1.55V.

[0047] Comparative Example 1

[0048] The same high specific surface area porous Co3O4 nanobelt powder as in Example 1 was used as an electrocatalyst to conduct HER and water electrolysis performance tests in a KOH alkaline solution environment with a pH of 14. The following results were obtained: 2 Under the condition of 217mV overpotential, the performance decreased by 20% after 1000 cycles; the current density of water electrolysis reached 10mA / cm 2 The required overpotential is 1.88V.

[0049] Comparative Example 2

[0050] Compared with Example 2, in Comparative Example 2, no matrix was used, and cobalt nitrate and ammonium metatungstate were directly prepared into 80 ml of a mixed solution according to an A:W atomic ratio of 1:1, and added into a pressure reactor, the total amount of cobalt nitrate and ammonium metatungstate was 0.45 g, and then 0.3 g of ammonium fluoride was added to fully dissolve, the reactor was tightly covered, and transferred to a 100°C drying oven, reacted for 12 hours, and cooled to obtain an amorphous CoWO4 solid;

[0051] The mixture was filtered and washed with deionized water and ethanol until neutral, transferred to an 80°C drying oven for overnight drying, and then transferred to a muffle furnace, heated to 500°C at a heating rate of 10°C / min and fully calcined for 2h, and cooled in the furnace to obtain crystalline CoWO4 powder;

[0052] The obtained crystalline CoWO4 powder was transferred to a tube furnace, the gas was evacuated, and then purged and activated in a hydrogen atmosphere at 400°C for 90 minutes to obtain a CoWO4 electrocatalyst.

[0053] Finally, the obtained CoWO4 electrocatalyst was tested for HER and water electrolysis performance in a KOH alkaline environment with a pH of 12. The following results were obtained: at a standard current density of 10 mA / cm 2 Under the condition of 176mV overpotential, the performance decreased by 13% after 1000 cycles; the current density of water electrolysis reached 10mA / cm 2 The required overpotential is 1.68V.

[0054] Comparative Example 3

[0055] A 1cm×1cm carbon cloth was cut out as a substrate and placed in a pressure reactor. Cobalt nitrate and sodium tungstate were prepared into a 70ml mixed solution with a Co:W atomic ratio of 1:1 and added thereto. The total amount of cobalt nitrate and ammonium metatungstate was 0.45g. The reactor was tightly covered and transferred to a 100℃ drying oven. The reaction was carried out for 12h and the amorphous CoWO4@C solid was obtained after cooling.

[0056] The product was filtered and washed with deionized water and ethanol until neutral, transferred to an 80°C drying oven for overnight drying, and then transferred to a muffle furnace, heated to 500°C at a heating rate of 10°C / min and fully calcined for 2h, and cooled in the furnace to obtain crystalline CoWO4@C powder.

[0057] The obtained crystalline CoWO4@C powder was transferred to a tubular furnace, the gas was evacuated, and then purged and activated in a hydrogen atmosphere at 500°C for 30 minutes to obtain an array-like CoWO4@C electrocatalyst.

[0058] Finally, the obtained CoWO4@C electrocatalyst was tested for HER and water electrolysis performance in an acidic environment of sulfuric acid solution with a pH of 1. The following results were obtained: 2 Under the condition of overpotential of 130mV, the performance decreased by 12% after 5000 cycles; the current density of water electrolysis reached 10mA / cm 2 The required overpotential is 1.62V.

[0059] It can be seen from the data in Examples 1 to 3 and the corresponding Comparative Examples 1 to 3 that the non-precious metal-based multi-metal oxide electrocatalyst generated in situ with a nano-metal oxide of a specific morphological structure as a matrix has a controllable morphological structure and excellent electrocatalytic hydrogen evolution and water electrolysis performance. In contrast, the electrocatalytic activity and stability of pure nano-metal oxides are very poor, the multi-metal oxides directly synthesized without any substrate are not active and stable enough, and the multi-metal oxide electrocatalysts grown in situ directly on the matrix without adding ammonium fluoride for morphological control are not excellent enough, and are worse than the current precious metal catalysts.

[0060] Therefore, it can be seen that the selection of the matrix, the pH value of the solution reaction system and the regulation of additives have a significant impact on the morphology, catalytic activity and stability of the catalyst, which helps to further improve the hydrogen evolution and water electrolysis performance of the electrocatalyst.

[0061] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A multi-element transition metal compound electrocatalyst material, characterized in that: The electrocatalyst material is composed of AWO4@B x O y ,in, AWO4 is the main catalyst, and A is any one of Fe, Co, Ni, and Cu; B x O y is a substrate, comprising any one or more oxide combinations of Fe, Co, Ni, and Cu; 1≤x≤3, 1≤y≤4; AWO4 and B x O y The mass ratio is controlled at 10:1 to 1:20; Among them, the same elements in A and B do not appear at the same time; The main catalyst AWO4 is based on B x O y It is grown in situ on the substrate, and the two have a strong interaction; Base B x O y The metal oxide material is in the form of at least one of nanoparticles, nanowires, nanorods, nanobelts, nanosheets, nanospheres and foam network structures; The method for preparing the electrocatalyst material comprises the following steps: 1) Weigh an appropriate amount of B x O y Place in a pressure reaction vessel, prepare the A precursor and the tungsten source into an aqueous solution according to the A:W atomic ratio of 1:1 and transfer into the pressure reaction vessel, add an appropriate amount of ammonium fluoride to adjust the pH value of the system, then react at a temperature of 100 to 200° C. for 6 to 24 hours, and cool with the furnace to obtain a reaction product; 2) After filtering and washing the reaction product, the reaction product is transferred to a vacuum drying oven and dried at 60 to 100° C. for 8 to 24 hours; then the reaction product is transferred to a tube furnace and heated to 300 to 600° C. at a heating rate of 1 to 10° C. / min and fully calcined for 1 to 5 hours to obtain a calcined product; 3) Then, during the cooling process of the calcined product, a hydrogen-argon mixed gas was introduced for a certain period of time to purge and activate the product, thereby obtaining AWO4@B x O y type electrocatalyst.

2. The electrocatalyst material according to claim 1, characterized in that In step 1), the A precursor includes at least one of A metal nitrate and A metal halide.

3. The electrocatalyst material according to claim 1, characterized in that In step 1), the tungsten source includes at least one of ammonium metatungstate and sodium tungstate.

4. The electrocatalyst material according to claim 1, characterized in that In step 1), the ammonium fluoride adjusts the pH value of the system to 3-6; the reaction product is in the solution system within the pH range at B x O y The morphology and structure of the AWO4 amorphous solid grown in situ on the substrate are affected by the morphology and structure of the substrate and the pH value of the solution system.

5. The electrocatalyst material according to claim 1, characterized in that In step 2), the calcined product is AWO4@B with abundant oxygen defects. x O y Crystalline solid.

6. The electrocatalyst material according to claim 1, characterized in that In step 3), the hydrogen concentration in the hydrogen-argon mixed gas is controlled at 5-15%, and the purge activation time is controlled at 15-120 minutes.

7. Use of the electrocatalyst material according to any one of claims 1 to 3 in catalyzing the electrolysis of water to produce hydrogen in the full pH range.

Citation Information

Patent Citations

  • Preparation method of W18O49 / NiWO4 / NF self-supporting electrocatalytic material

    CN109806902A

  • 3D-structured composite hydrogen-evolving electrode and preparation method thereof

    CN109898093A

  • Metal oxide nano sheet supported carbon coated metal particle electrolysed water catalyst

    CN109939691A

  • Preparation method and application of NiO / Co3O4

    CN111195518A

  • Preparation method of water decomposition electrocatalyst Ag8W4O16 / CoWO4

    CN113774403A