A device and method for regenerating metal by vacuum electroslag-rotational segregation
Through the combination of vacuum electroslag refining and rotational segregation purification units, the problems of process complexity and insufficient purity in the existing electroslag remelting process are solved, and efficient regeneration of multi-form metal scraps and high-purity metal preparation are achieved.
Patent Information
- Application Number
- CN202110947361.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-18
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-08-18
AI Technical Summary
The existing electroslag remelting process requires metal materials to be made into electrode rods, which increases process steps and processing costs. It also has low adaptability to metal materials that are difficult to make into electrode rods and cannot effectively remove segregated impurities in the ingot. Resulting in insufficient purity of the ingot.
Using a vacuum electroslag-rotating segregation regenerated metal device, the vacuum electroslag refining unit realizes rapid smelting and electroslag refining of polymorphic metal scraps. Combined with the rotating segregation purification unit, the segregation-type impurities are efficiently removed to achieve the preparation of high-purity regenerated metal.
The short-range, efficient, continuous and stable regeneration of high-value metals from metal scraps with multiple forms and different properties has been achieved, and high-purity recycled metal with a purity of ≥99.99% has been obtained, simplifying the process and improving purity.
Smart Images

Figure CN115707786B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of recycling secondary metal resources, and in particular to a device and method for regenerating metal by vacuum electroslag-rotational segregation. Background Art
[0002] As the foundation of social development, the energy industry has received extensive attention from all walks of life in recent years. Metallurgical methods have the advantages of low energy consumption and low investment, and have great potential in reducing costs, simplifying processes, and energy conservation and environmental protection.
[0003] Slag is a product of the pyrometallurgical process. It is a multi-component melt with oxides as the main components, among which acidic oxides (such as SiO2), alkaline oxides (such as CaO) and amphoteric oxides (Al2O3) are the main oxides. The main difference between various oxides is the different binding ability to oxygen ions, among which acidic oxides have the strongest binding ability to oxygen ions and alkaline oxides have the weakest binding ability. These oxides can also combine with each other to form various compounds, solid solutions and eutectic mixtures. According to the role played in the pyrometallurgical process, slag can be divided into: smelting slag, refining slag and enriched slag, etc.; according to the different composition of slag, it can be divided into binary slag, ternary slag, etc. At present, slag refining has become one of the main methods to improve metal quality.
[0004] CN112359216A discloses a multi-electrode electroslag remelting device and electroslag remelting process for high-nitrogen austenitic stainless steel. The process uses nitrided alloys, low-carbon steel, manganese steel and other alloy materials with different elements and contents, and combines the calculation of the composition ratio and mass fraction of the electroslag ingot to prepare multiple electrode rods of the same length and different diameters to carry out electroslag remelting of the high-nitrogen austenitic stainless steel, thereby solving the technical problems of expensive electroslag remelting equipment and complicated operating process for high-nitrogen austenitic stainless steel.
[0005] CN111440956A discloses an electroslag remelting process method, which first smelts alloy raw materials and casts them into a master alloy rod as an electrode rod for electroslag remelting, and removes oxide scale from the surface of the electrode rod; then prepares an aluminum powder mixture of water glass and industrial aluminum powder and applies it to the electrode rod; after the aluminum powder mixture applied to the electrode rod is naturally dried, it is baked at a temperature of 100-250°C for 1-3 hours; electroslag remelting slag is prepared according to the elements and contents in the alloy rod; inert gas is continuously introduced during the electroslag remelting process, and 0.1-0.3% aluminum particles of the mass percentage of the electrode rod are added until the electroslag remelting is completed; and the aluminum content of the entire alloy electroslag remelting ingot is uniform.
[0006] Both of the above-mentioned two electroslag remelting processes require that the raw materials be made into electrode rods before electroslag remelting can be performed, which increases the process operation steps and increases the processing cost. In addition, some metal materials that are not easy to be made into electrode rods cannot be processed, and the adaptability to raw materials is low.
[0007] CN110358930A discloses an electroslag remelting slag and an electroslag remelting method that can retain sulfur, which solves the problem of high desulfurization rate of the existing electroslag remelting method. The electroslag remelting slag is prepared by weight from 5 to 9 parts of CaO, 26 to 35 parts of Al2O3, 50 to 65 parts of CaF2 and 1 to 3 parts of SiO2. Method: weigh metallurgical lime block, white corundum powder, fluorite powder and quartz powder as raw materials and dry them, first add fluorite powder into the crystallizer to start the arc, then add white corundum powder and quartz powder, and finally add metallurgical lime block; weld the consumable electrode to the dummy electrode, power on for electroslag remelting, and use a step-by-step current reduction method to feed the shrinkage after the electroslag remelting is completed. After the feeding is completed and the power is turned off, the shrinkage is cooled and demolded. The process is more stable and conducive to sulfur retention, avoiding excessive desulfurization rate, and the prepared ingot has good molding effect and smooth surface. However, this method cannot effectively remove segregation impurities in the ingot, and the purity of the obtained ingot needs to be further improved.
[0008] Based on the above analysis, there is an urgent need to develop an electroslag remelting process that can process metal waste of various forms and different properties to obtain high-purity recycled metal. Summary of the invention
[0009] In view of the problems existing in the prior art, the present invention provides a device and method for vacuum electroslag-rotary segregation metal regeneration. The device adopts a vacuum electroslag refining unit to realize slag washing countercurrent efficient smelting and electroslag refining of polymorphic metal waste, and further couples the rotary segregation purification unit to efficiently remove segregation impurities through the rotary solidification segregation process, so as to achieve the purpose of short-range, efficient, continuous and stable preparation of high-value recycled metal from polymorphic metal waste.
[0010] To achieve this object, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a device for regenerating metal by vacuum electroslag-rotary segregation, the device comprising a vacuum electroslag refining unit, a rotary segregation purification unit and a transport unit; the vacuum electroslag refining unit and the rotary segregation purification unit are independently connected to the transport unit.
[0012] The vacuum electroslag-rotating segregation metal regeneration device of the present invention can directly electroslag refine metal wastes of various forms (powder, sphere, square or irregular shape, etc.) and different properties (not easy to make into ingots and can be made into ingots) through the vacuum electroslag refining unit, and quickly separate volatile, easily oxidizable and inclusion impurities, and can achieve rapid and efficient removal of segregation impurities through the rotating segregation purification unit. The device of the present invention overcomes the defect of the prior art that the metal material must be made into ingots before electroslag refining, shortens the steps of metal waste regeneration and purification, and the device of the present invention adopts rotating segregation purification, which has high purification efficiency for metal waste, less time consumption, and high purity of the regenerated metal compared with the existing directional solidification purification.
[0013] Preferably, the vacuum electroslag refining unit comprises a vacuum chamber.
[0014] Preferably, the vacuum electroslag refining unit comprises a non-consumable electrode, a voltage control device and an automatic feeding device.
[0015] The present invention adopts non-consumable electrodes to carry out electroslag refining, thereby realizing rapid smelting of polymorphic metal solid waste.
[0016] Preferably, the automatic feeding device is arranged on one side of the upper part of the vacuum chamber.
[0017] Preferably, the non-consumable electrode and the voltage control device form an electrical circulation loop with the containing container.
[0018] In the present invention, a containing container is first placed in a vacuum chamber, a non-consumable electrode is inserted into the bottom of the containing container to start an arc, and then solid electroslag is added to the bottom of the non-consumable electrode, so that the non-consumable electrode and the voltage control device form an electric circulation loop with the containing container to melt the solid electroslag into an electroslag melt.
[0019] Preferably, the ratio of the outer diameter of the non-consumable electrode to the inner diameter of the container is 1 / 10 to 1 / 2, for example, it can be 1 / 10, 1 / 9, 1 / 8, 1 / 7, 1 / 6, 1 / 5, 1 / 4, 1 / 3 or 1 / 2, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the ratio of the length of the non-consumable electrode to the inner height of the container is 1 / 2 to 2 / 1, for example, it can be 1 / 2, 3 / 5, 7 / 10, 4 / 5, 1 / 1, 6 / 5, 3 / 2 or 2 / 1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the rotary segregation purification unit comprises an atmosphere protection furnace.
[0022] Preferably, the atmosphere protection furnace comprises a heating chamber and a non-heating chamber.
[0023] Preferably, the heating chamber is located below the non-heating chamber.
[0024] The atmosphere protection furnace of the present invention is divided into two parts, the lower part is a heating chamber, and the upper part is a non-heating chamber. The heating chamber is used to keep the temperature of the molten metal always above the melting point of the metal, and the non-heating chamber is used to provide sufficient space for the rotary segregation purification operation of the rotary crystallizer.
[0025] Preferably, heating devices are arranged around the heating chamber.
[0026] Preferably, central axes of the heating chamber and the non-heating chamber overlap.
[0027] Preferably, a rotary crystallization device is arranged on the central axis of the heating chamber and the non-heating chamber.
[0028] The rotary crystallization device of the present invention can move up and down along the central axis in the vertical direction inside the heating chamber and the non-heating chamber.
[0029] Preferably, the rotary crystallization device is a shell-type structure, including a central layer for inputting cooling medium and an outer shell layer for outputting cooling medium.
[0030] Preferably, a double-layer sealing valve is provided between the heating chamber and the non-heating chamber.
[0031] The invention discloses that a transition chamber is provided inside the double-layer sealing valve.
[0032] The sealing valves described in the present invention are opened or closed in sequence during the startup process to ensure the air tightness inside the heating chamber.
[0033] Preferably, the transport unit comprises an atmosphere protection chamber.
[0034] Preferably, the atmosphere protection chamber is provided with a containing container, a lifting transport device, a closed-circuit transport track, an electroslag recovery device and a metal melt residual material recovery device.
[0035] The present invention can remove the container containing high-temperature molten metal and liquid electroslag from the vacuum chamber of the vacuum electroslag refining unit through a double-layer sealing valve by lowering the lifting and transporting device. After the liquid electroslag is dumped and removed, the lifting and transporting device transports the high-temperature molten metal to the rotary segregation purification unit, and the lifting and transporting device is adjusted to rise to place it into the atmosphere protection furnace.
[0036] Preferably, the lifting and transporting device moves cyclically along a closed-circuit transport track.
[0037] The lifting and transporting device of the present invention circulates along the closed-circuit transport track, and the lifting and transporting device can transport the emptied containing container to the vacuum chamber of the vacuum electroslag refining unit to continue the next electroslag remelting and refining.
[0038] Preferably, the vacuum electroslag refining unit and the rotary segregation purification unit are independently connected to the transport unit via a double-layer sealing valve at the furnace mouth.
[0039] The vacuum electroslag refining unit and the rotary segregation purification unit in the present invention are independently connected to the transport unit through the double-layer sealing valve at the furnace mouth to ensure the airtightness of the vacuum chamber and the atmosphere protection furnace.
[0040] Preferably, the furnace mouth double-layer sealing valves are independently controlled by a furnace mouth valve control device.
[0041] In a second aspect, the present invention provides a method for regenerating metal by vacuum electroslag-rotational segregation, wherein the method is carried out using the device for regenerating metal by vacuum electroslag-rotational segregation described in the first aspect.
[0042] The method of the present invention utilizes the high-efficiency countercurrent smelting of polymorphic metal waste slag washing and the dynamic interface impurity removal process of rotary segregation to achieve the synchronous removal of multiple impurities in metal waste, wherein the rotary segregation unit utilizes the high-speed rotation of the crystallization device to cause the solute diffusion layer formed near the solid-liquid interface to be effectively stirred and mixed with other main liquid phase parts, and the impurities in the diffusion layer are dispersed into the entire liquid phase, thereby greatly reducing the thickness of the diffusion layer, reducing the effective segregation coefficient of impurities, and improving the segregation efficiency of impurities. At the same time, the boundary layer of the temperature distribution on the liquid phase side is also thinned, thereby increasing the temperature gradient of the liquid phase region near the liquid-solid interface, and synergistically achieving rapid crystal growth and impurity segregation removal.
[0043] Preferably, the method comprises the following steps:
[0044] (1) After the solid electroslag is melted into an electroslag melt in a vacuum electroslag refining unit, metal waste is added for refining treatment to obtain a metal melt and liquid electroslag;
[0045] (2) After removing the liquid electroslag, the metal melt is transported to a rotary segregation purification unit via a transport unit for rotary segregation purification to obtain high-purity recycled metal.
[0046] Preferably, the solid electroslag in step (1) comprises any one or a combination of at least two of CaO, SiO2, Al2O3, MgO, FeO, CaF2, NaF, Na3AlF6, BaO, BaF2, TiO2, Cr2O3, B2O3, K2O, ZrO2, ZnO, Li2O, SrO, Ce2O3, PbO, CaCl2, NaCl or KCl, wherein typical but non-limiting combinations include a combination of CaO and SiO2, a combination of MgO and FeO, a combination of CaF2 and NaF, a combination of Na3AlF6 and BaO, a combination of BaF2 and TiO2, a combination of B2O3 and K2O, a combination of ZrO2 and ZnO, a combination of Ce2O3 and PbO or a combination of CaCl2 and NaCl.
[0047] Preferably, the metal scrap comprises any one or a combination of at least two of iron, chromium, manganese, aluminum, copper, magnesium, potassium, sodium, calcium, strontium, barium, lead, zinc, tin, cobalt, nickel, antimony, cadmium, bismuth, gold, silver, platinum, ruthenium, palladium, lithium, beryllium, titanium, zirconium, vanadium, gallium, indium, thallium, germanium, lanthanum, cerium, neodymium, scandium or silicon, wherein typical but non-limiting combinations include a combination of iron and chromium, a combination of manganese and aluminum, a combination of copper and lead, a combination of zinc and tin, a combination of cobalt and nickel, a combination of titanium and zirconium, a combination of magnesium and calcium, a combination of strontium and barium, a combination of antimony and cadmium, a combination of bismuth and gold, a combination of silver and platinum, a combination of ruthenium and palladium, a combination of lanthanum and cerium, or a combination of neodymium and scandium.
[0048] Preferably, the shape of the metal scrap includes any one of powder, sphere, cube, cone, prism or irregular shape, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of powder and sphere, a combination of sphere and cube, a combination of cone and prism, or a combination of cube and irregular shape.
[0049] Preferably, the size of the metal scrap is 0.001 mm to 50 mm, for example, 0.0001 mm, 0.001 mm, 0.01 mm, 0.1 mm, 1 mm, 5 mm, 20 mm or 50 mm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0050] Preferably, the absolute vacuum degree of the vacuum electroslag refining unit is 10 -3 Pa~10 -1 Pa, for example, can be 10 - 3 Pa, 5×10 -3 Pa, 8×10 -3 Pa, 10 -2 Pa, 3×10 -2 Pa, 5×10 -2Pa or 10 -1 Pa, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0051] Preferably, the ratio of the thickness of the electroslag melt in step (1) to the inner height of the containing container is 1 / 10 to 1 / 2, for example, it can be 1 / 10, 1 / 9, 1 / 8, 1 / 7, 1 / 6, 1 / 5, 1 / 4, 1 / 3 or 1 / 2, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0052] Preferably, the ratio of the thickness of the solid electroslag to the inner height of the container is 1 / 10 to 1 / 2, for example, it can be 1 / 10, 1 / 9, 1 / 8, 1 / 7, 1 / 6, 1 / 5, 1 / 4, 1 / 3 or 1 / 2, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] Preferably, the depth of immersion of the non-consumable electrode in the solid electroslag is 1 / 10 to 9 / 10 of the thickness of the solid electroslag, for example, it can be 1 / 10, 2 / 10, 3 / 10, 4 / 10, 5 / 10, 6 / 10, 7 / 10, 8 / 10 or 9 / 10, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] Preferably, the density of the electroslag melt is less than 0.5 g / cm3 of the density of the metal melt. 3 ~5.0g / cm 3 , for example, it can be 0.5 g / cm 3 , 1.0g / cm 3 , 1.5g / cm 3 , 2.0g / cm 3 、3.0g / cm 3 , 4.0g / cm 3 or 5.0g / cm 3 , but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0055] The density of the electroslag melt in the present invention is less than the density of the metal melt by 0.5 g / cm 3 ~5.0g / cm 3 Therefore, the electroslag melt is above the liquid surface of the molten metal. On the one hand, it is necessary to ensure that the non-consumable electrode does not contact the molten metal, ensure the resistance heating effect of the electroslag, and meet the smelting and refining effects of the metal waste slag washing process. On the other hand, it is convenient to dump and remove the electroslag melt before entering the rotary segregation purification unit to improve the purity of the recycled metal.
[0056] Preferably, the melting point of the solid electroslag is 50°C to 200°C lower than the melting point of the molten metal, for example, it can be 50°C, 80°C, 100°C, 120°C, 150°C, 170°C or 200°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0057] Preferably, the temperature of the refining treatment is 50°C to 200°C higher than the melting point of the metal scrap, for example, it can be 50°C, 80°C, 100°C, 120°C, 150°C, 170°C or 200°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0058] Preferably, the electrical conductivity of the material of the container is greater than 200s / cm, for example, it can be 200s / cm, 220s / cm, 250s / cm, 300s / cm, 500s / cm or 650s / cm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0059] Preferably, the melting point of the material of the container is more than 200°C greater than the melting point of the metal waste, for example, it can be 200°C, 230°C, 250°C, 300°C or 400°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0060] Preferably, the depth of immersion of the rotating crystallization device in step (2) into the metal melt is 1 / 5 to 1 / 1 of the depth of the metal melt, for example, it can be 1 / 5, 1 / 4, 1 / 3, 2 / 5, 1 / 2, 3 / 5, 4 / 5 or 1 / 1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0061] Preferably, the rotational speed of the rotary crystallization device is 1 r / min to 500 r / min, for example, it can be 1 r / min, 5 r / min, 10 r / min, 30 r / min, 50 r / min, 100 r / min, 300 r / min or 500 r / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0062] Preferably, the wall temperature of the rotary crystallization device is reduced from the temperature of the metal melt to 50°C to 200°C below the melting point of the metal scrap within 10 to 60 minutes, for example, it can be 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, 45 minutes, 50 minutes, 55 minutes or 60 minutes, for example, it can be 50°C, 80°C, 100°C, 120°C, 150°C, 170°C or 200°C, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0063] Preferably, the temperature of the molten metal is 50°C to 200°C higher than the melting point of the metal scrap, for example, it may be 50°C, 80°C, 100°C, 120°C, 150°C, 170°C or 200°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0064] Preferably, the purity of the high-purity recycled metal is ≥99.99%, for example, it may be 99.99%, 99.993%, 99.995%, 99.997%, 99.9991% or 99.99992%.
[0065] Preferably, step (1) and step (2) are each independently carried out under the protection of an inert atmosphere.
[0066] Preferably, the inert atmosphere comprises any one of a nitrogen atmosphere, an argon atmosphere or a helium atmosphere, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of a nitrogen atmosphere and an argon atmosphere, a combination of an argon atmosphere and a helium atmosphere, a combination of a nitrogen atmosphere and a helium atmosphere, or a combination of a nitrogen atmosphere, an argon atmosphere and a helium atmosphere.
[0067] As a preferred technical solution of the present invention, the method comprises the following steps:
[0068] (1) Solid electroslag is heated in the vacuum electroslag refining unit at an absolute vacuum of 10 -3 Pa~10 -1 Pa, and then add metal scraps with a size of 0.001 mm to 50 mm for refining to obtain metal melt and liquid electroslag; the ratio of the thickness of the electroslag melt to the inner height of the container is 1 / 10 to 1 / 2; the ratio of the thickness of the solid electroslag to the inner height of the container is 1 / 10 to 1 / 2; the depth of the non-consumable electrode immersed in the solid electroslag is 1 / 10 to 9 / 10 of the thickness of the solid electroslag; the density of the electroslag melt is less than the density of the metal melt by 0.5 to 5.0 g / cm 3; The melting point of the solid electroslag is 50°C to 200°C lower than the melting point of the metal melt; the temperature of the refining treatment is 50°C to 200°C higher than the melting point of the metal waste; the electrical conductivity of the material of the container is greater than 200s / cm; the melting point of the material of the container is more than 200°C higher than the melting point of the metal waste;
[0069] (2) After removing the liquid electroslag, the molten metal is transported to a rotary segregation purification unit via a transport unit, and rotary segregation purification is performed under an inert atmosphere to obtain a high-purity recycled metal with a purity of ≥99.99%; the depth of the rotary crystallization device immersed in the molten metal is 1 / 5 to 1 / 1 of the depth of the molten metal; the rotation speed of the rotary crystallization device is 1 to 500 r / min; the wall temperature of the rotary crystallization device is reduced from the temperature of the molten metal to 50°C to 200°C below the melting point of the metal waste within 10 to 60 minutes; the temperature of the molten metal is 50°C to 200°C higher than the melting point of the metal waste.
[0070] Compared with the prior art, the present invention has at least the following beneficial effects:
[0071] (1) The vacuum electroslag-rotating segregation metal regeneration device provided by the present invention overcomes the technical difficulties of high-efficiency countercurrent smelting of multi-form metal solid waste slag washing, and linking electroslag refining with rotary solidification segregation process. By coupling the vacuum electroslag refining unit with the rotary segregation purification unit, the short-range, high-efficiency, continuous and stable regeneration of high-value metals from multi-form and different-property metal waste is achieved;
[0072] (2) The vacuum electroslag-rotational segregation metal regeneration method provided by the present invention adopts slag washing countercurrent high-efficiency smelting and rotational segregation dynamic interface impurity removal, thereby achieving the simultaneous removal of multiple impurities in metal waste and obtaining high-purity recycled metal with a purity of ≥99.99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0073] Figure 1 It is a longitudinal section of the device for vacuum electroslag-rotational segregation metal regeneration provided by the present invention;
[0074] Figure 2 It is a top view of the device for vacuum electroslag-rotational segregation metal regeneration provided by the present invention.
[0075] Among them: 1-metal waste; 2-automatic feeding device; 3-non-consumable electrode; 4-voltage control device; 5-furnace mouth valve control device; 6-solid electroslag; 7-metal melt; 8-furnace mouth double-layer sealing valve; 9-carrying container; 10-lifting and lowering transport device; 11-electroslag recovery device; 12-heating device; 13-double-layer sealing valve; 14-rotating crystallization device; 15-center layer; 16-atmosphere protection furnace; 17-metal melt residue; 18-metal melt residue recovery device; 19-atmosphere protection chamber; 20-vacuum chamber; 21-closed-loop transport track. DETAILED DESCRIPTION
[0076] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0077] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0078] As a specific embodiment of the present invention, a vacuum electroslag-rotation segregation device for regenerating metal is provided, and a longitudinal section of the device is as follows: Figure 1 As shown, the top view of the device is as shown Figure 2 The device comprises a vacuum electroslag refining unit, a rotary segregation purification unit and a transport unit; the vacuum electroslag refining unit and the rotary segregation purification unit are independently connected to the transport unit.
[0079] The vacuum electroslag refining unit is a vacuum chamber 20; the electroslag refining unit includes a non-consumable electrode 3, a voltage control device 4 and an automatic feeding device 2; the non-consumable electrode 3 and the voltage control device 4 form an electrical circulation loop with the containing container 9; the ratio of the outer diameter of the non-consumable electrode 3 to the inner diameter of the containing container 9 is 1 / 10 to 1 / 2, and the height ratio is 1 / 2 to 2 / 1, and the automatic feeding device 2 is arranged on the upper side of the vacuum chamber 20.
[0080] The rotary segregation purification unit is an atmosphere protection furnace 16; the atmosphere protection furnace 16 includes a heating chamber and a non-heating chamber; the heating chamber is at the lower part of the non-heating chamber; a heating device 12 is arranged around the heating chamber; a double-layer sealing valve 13 is arranged between the heating chamber and the non-heating chamber; a transition chamber is arranged inside the double-layer sealing valve 13; a rotary crystallization device 14 is arranged on the axis of the heating chamber and the non-heating chamber, and the rotary crystallization device 14 is a shell-type structure, including a central layer 15 for inputting cooling medium and an outer shell layer for outputting cooling medium.
[0081] The transport unit is an atmosphere protection chamber 19; the transport unit includes a container 9, a lifting carrier 10, a closed-circuit carrier track 21 (see Figure 2 ), an electroslag recovery device 11 and a metal melt residual material recovery device 18; the vacuum electroslag refining unit and the rotary segregation purification unit are independently connected to the transportation unit through a furnace mouth double-layer sealing valve 8, and the furnace mouth double-layer sealing valve 8 is independently controlled by a furnace mouth valve control device 5.
[0082] The following examples and comparative examples are carried out using the above-mentioned vacuum electroslag-rotational segregation metal regeneration device.
[0083] Example 1
[0084] This embodiment provides a method for regenerating metal by vacuum electroslag-rotational segregation, the method comprising the following steps:
[0085] (1) placing a container 9 inside a vacuum chamber 20, inserting a non-consumable electrode 3 to the bottom of the container 9 to start an arc, wherein the ratio of the outer diameter of the non-consumable electrode 3 to the inner diameter of the container 9 is 1 / 5, and the ratio of the height is 1 / 2; adding solid electroslag 6 to the bottom of the non-consumable electrode 3 through the gap between the non-consumable electrode 3 and the container 9 by an automatic feeding device 2, heating and melting the solid electroslag 6 into an electroslag melt and keeping the temperature at 1200° C., wherein the ratio of the thickness of the solid electroslag 6 to the inner height of the container 9 is 1 / 10; during the melting and continuous increase of the solid electroslag 6, the depth of the non-consumable electrode 3 inserted into the solid electroslag 6 is maintained at 1 / 10 of the thickness of the solid electroslag 6, and the vacuum degree of the vacuum chamber 20 is 10 -1 pa; the composition of the solid electroslag is CaO-Al2O3-CaF2-CuO, and the melting point of the solid electroslag is 950°C;
[0086] (2) Adding powdered copper waste 1 with a size of 1 to 10 mm into liquid electroslag through an automatic feeding device 2, and obtaining a refined molten copper material 7 after passing through the liquid electroslag, the added amount of the powdered copper waste 1 is 300 kg; the material conductivity of the container 9 containing the liquid electroslag and the refined molten copper material 7 is 300 s / cm, and the melting point of the material of the container 9 is 1400° C.; the melting point of the powdered copper waste 1 is 1050° C., the purity of the powdered copper waste 1 is 99.95%, and the impurities include Fe, Al, H2, Cu2O, etc.; the density of the electroslag melt is less than the density of the refined molten copper material 7 by 1.0 g / cm 3 ;
[0087] (3) The container 9 containing the liquid electroslag and the refined molten copper material 7 is moved out of the vacuum chamber 20 to the lifting and transporting device 10, and the liquid electroslag is poured into the electroslag recovery device 11. The molten copper material after slag pouring is transported to the bottom of the atmosphere protection furnace 16 and raised to the furnace body by the lifting and transporting device 10, and argon gas is continuously introduced into the furnace, and the pressure in the furnace is maintained at 60000 Pa and the temperature in the furnace is maintained at 1200°C;
[0088] (4) The rotary crystallization device 14 is immersed in the molten copper material after slag pouring, and the depth of the rotary crystallization device 14 immersed in the molten copper material is 1 / 5 of the total depth of the molten copper material. Liquid argon is continuously introduced into the central layer 15 of the rotary crystallization device 14 while maintaining a rotating state, and the rotation speed is 100 rpm. The wall temperature of the rotary crystallization device 14 is reduced from the temperature of the molten copper material to 1000° C. within 30 minutes, and the temperature of the molten copper material is 1200° C.;
[0089] (5) After the copper on the outer layer of the rotary crystallization device 14 is solidified, it is lifted to the outside of the atmosphere protection furnace 16 at a rate of 10 mm / min, and high-purity copper S1 is obtained after separation. The rotary crystallization device 14 is then returned to the inside of the atmosphere protection furnace 16, and the operation of step (4) is repeated. During this process, the internal temperature and pressure of the atmosphere protection furnace 16 remain unchanged;
[0090] (6) Repeat steps (4) and (5) for a total of 3 times to obtain high-purity recycled copper S2-S4 with a weight of 30 kg each, lower the molten metal residue 17 out of the atmosphere protection furnace 16 and transport it to the molten metal residue recovery device 18 for recovery, and then transport the emptied container 9 to the bottom of the vacuum chamber 20 for the next electroslag remelting refining.
[0091] Example 2
[0092] This embodiment provides a method for regenerating metal by vacuum electroslag-rotational segregation, the method comprising the following steps:
[0093] (1) The containing container 9 is placed inside the vacuum chamber 20, and the non-consumable electrode 3 is inserted to the bottom of the containing container 9 to start the arc. The ratio of the outer diameter of the non-consumable electrode 3 to the inner diameter of the containing container 9 is 1 / 6, and the height ratio is 1 / 2; the solid electroslag 6 is added to the bottom of the non-consumable electrode 3 through the gap between the non-consumable electrode 3 and the containing container 9 by the automatic feeding device 2, and the solid electroslag 6 is heated and melted into electroslag melt and kept at 1400°C. The ratio of the thickness of the solid electroslag 6 to the inner height of the containing container 9 is 1 / 8; during the melting and continuous increase of the solid electroslag 6, the depth of the non-consumable electrode 3 inserted into the solid electroslag 6 is maintained at 1 / 5 of the thickness of the solid electroslag 6, and the vacuum degree of the vacuum chamber 20 is 10 -1pa; the composition of the solid electroslag is CaO-Al2O3-CaF2-MnO, and the melting point of the solid electroslag is 950°C;
[0094] (2) adding a powdered manganese waste material 1 having a size of 1 to 10 mm into liquid electroslag through an automatic feeding device 2, and obtaining a refined manganese melt 7 after passing through the liquid electroslag, wherein the amount of the powdered manganese waste material 1 added is 300 kg; the material conductivity of a container 9 containing liquid electroslag and refined manganese melt 7 is 300 s / cm, and the material melting point of the container 9 is 1600° C.; the melting point of the powdered manganese waste material 1 is 1250° C., the purity of the powdered manganese waste material 1 is 99.99%, and the impurities thereof include Fe, S, Al2O3, etc.; the density of the electroslag melt is less than the density of the refined molten manganese material 7 by 5.0 g / cm 3 ;
[0095] (3) moving the container 9 containing the liquid electroslag and the refined manganese melt 7 out of the vacuum chamber 20 onto the lifting and transporting device 10, pouring the liquid electroslag into the electroslag recovery device 11, and transporting the molten manganese material after pouring the slag to the bottom of the atmosphere protection furnace 16 and raising it to the furnace body through the lifting and transporting device 10, continuously introducing argon gas into the furnace, and maintaining the pressure in the furnace at 40000 Pa and the temperature in the furnace at 1400°C;
[0096] (4) immersing the rotary crystallization device 14 into the molten manganese material after slag pouring, the depth of the rotary crystallization device 14 immersed in the molten manganese material is 1 / 5 of the total depth of the molten manganese material, while continuously introducing liquid argon into the central layer 15 of the rotary crystallization device 14 and maintaining a rotating state, and the rotation speed is 200 rpm, and the wall temperature of the rotary crystallization device 14 is reduced from the temperature of the molten manganese material to 1200° C. within 30 minutes, and the temperature of the molten manganese material is 1400° C.;
[0097] (5) After the manganese in the outer layer of the rotary crystallization device 14 is solidified, it is lifted to the outside of the atmosphere protection furnace 16 at a rate of 10 mm / min, and high-purity regenerated manganese S1 is obtained after separation. Then, the rotary crystallization device 14 is returned to the inside of the atmosphere protection furnace 16, and the operation of step (4) is repeated. During this process, the internal temperature and pressure of the atmosphere protection furnace 16 remain unchanged;
[0098] (6) Repeat steps (4) and (5) for a total of 4 times to obtain high-purity regenerated manganese S2-S5 with a weight of 30 kg each, and lower the molten metal residue 17 out of the atmosphere protection furnace 16 and transport it to the molten metal residue recovery device 18 for recovery, and then transport the emptied container 9 to the bottom of the vacuum chamber 20 for the next electroslag remelting refining.
[0099] Example 3
[0100] This embodiment provides a method for regenerating metal by vacuum electroslag-rotational segregation, the method comprising the following steps:
[0101] (1) The containing container 9 is placed inside the vacuum chamber 20, and the non-consumable electrode 3 is inserted to the bottom of the containing container 9 to start the arc. The ratio of the outer diameter of the non-consumable electrode 3 to the inner diameter of the containing container 9 is 1 / 5, and the height ratio is 1 / 2; the solid electroslag 6 is added to the bottom of the non-consumable electrode 3 through the gap between the non-consumable electrode 3 and the containing container 9 by the automatic feeding device 2, and the solid electroslag 6 is heated and melted into an electroslag melt and kept at 1600°C. The ratio of the thickness of the solid electroslag 6 to the inner height of the containing container 9 is 1 / 6; during the melting and continuous increase of the solid electroslag 6, the depth of the non-consumable electrode 3 inserted into the solid electroslag 6 is maintained at 1 / 5 of the thickness of the solid electroslag 6, and the vacuum degree of the vacuum chamber 20 is 10 -2 pa; the composition of the solid electroslag is CaO-SiO2-Al2O3-CaF2, and the melting point of the solid electroslag is 1300°C;
[0102] (2) adding irregular silicon waste block 1 with a size of 5 to 20 mm into liquid electroslag through an automatic feeding device 2, and obtaining refined molten silicon material 7 after passing through the liquid electroslag, wherein the addition amount of the irregular silicon waste block 1 is 100 kg; the material conductivity of the container 9 containing the liquid electroslag and the refined molten silicon material 7 is 650 s / cm, and the melting point of the material of the container 9 is 1800° C.; the melting point of the irregular silicon waste block 1 is 1420° C., the purity of the irregular silicon waste block 1 is 99.995%, wherein the impurities include Fe, Al, Ti, B and P; the density of the electroslag melt is less than the density of the refined molten silicon material 7 by 4.0 g / cm 3 ;
[0103] (3) The container 9 containing the liquid electroslag and the refined molten silicon material 7 is moved out of the vacuum chamber 20 to the lifting and transporting device 10, and the liquid electroslag is poured into the electroslag recovery device 11. The molten silicon material after slag pouring is transported to the bottom of the atmosphere protection furnace 16 and raised to the furnace body by the lifting and transporting device 10, and argon gas is continuously introduced into the furnace, and the pressure in the furnace is maintained at 40000 Pa and the temperature in the furnace is maintained at 1400°C;
[0104] (4) The rotary crystallization device 14 is immersed in the molten silicon material after the slag is poured. The depth of the rotary crystallization device 14 immersed in the molten silicon material is 1 / 5 of the total depth of the molten silicon material. Liquid argon is continuously introduced into the central layer 15 of the rotary crystallization device 14 while the device is kept rotating at a speed of 200 rpm. The wall temperature of the rotary crystallization device 14 is reduced from the temperature of the molten silicon material to 1200° C. within 30 minutes, and the temperature of the molten silicon material is 1400° C.;
[0105] (5) After the silicon on the outer layer of the rotary crystallization device 14 is solidified, it is lifted to the outside of the atmosphere protection furnace 16 at a rate of 10 mm / min, and high-purity silicon S1 is obtained after separation. The rotary crystallization device 14 is then returned to the inside of the atmosphere protection furnace 16, and the operation of step (4) is repeated. During this process, the internal temperature and pressure of the atmosphere protection furnace 16 remain unchanged;
[0106] (6) Repeat steps (4) and (5) for a total of 6 times to obtain high-purity regenerated silicon S2-S7 with a weight of 10 kg each, lower the metal melt residue 17 out of the atmosphere protection furnace 16 and transport it to the metal melt residue recovery device 18 for recovery, and then transport the emptied container 9 to the bottom of the vacuum chamber 20 for the next electroslag remelting refining.
[0107] Example 4
[0108] This embodiment provides a method for regenerating metal by vacuum electroslag-rotational segregation, the method comprising the following steps:
[0109] (1) The containing container 9 is placed inside the vacuum chamber 20, and the non-consumable electrode 3 is inserted to the bottom of the containing container 9 to start the arc. The ratio of the outer diameter of the non-consumable electrode 3 to the inner diameter of the containing container 9 is 1 / 5, and the height ratio is 1 / 2; the solid electroslag 6 is added to the bottom of the non-consumable electrode 3 through the gap between the non-consumable electrode 3 and the containing container 9 by the automatic feeding device 2, and the solid electroslag 6 is heated and melted into an electroslag melt and kept at 800°C. The ratio of the thickness of the solid electroslag 6 to the inner height of the containing container 9 is 1 / 8; during the melting and continuous increase of the solid electroslag 6, the depth of the non-consumable electrode 3 inserted into the solid electroslag 6 is maintained at 1 / 5 of the thickness of the solid electroslag 6, and the vacuum degree of the vacuum chamber 20 is 10 -3 pa; the composition of the solid electroslag is CaO-Al2O3-NaF-Na3AlF6-NaCl, and the melting point of the solid electroslag is 600°C;
[0110] (2) A square block of aluminum scrap 1 with a size of 10 to 15 mm is added to the liquid electroslag through an automatic feeding device 2, and a refined aluminum melt 7 is obtained after passing through the liquid electroslag. The amount of the square block of aluminum scrap 1 added is 100 kg; the material conductivity of the container 9 containing the liquid electroslag and the refined aluminum melt 7 is 250 s / cm, and the melting point of the material of the container 9 is 950°C; the melting point of the square block of aluminum scrap 1 is 660°C, and the purity of the square block of aluminum scrap 1 is 99.99%, wherein the impurities include Fe, Si, O, Al2O3, etc.; the density of the electroslag melt is less than the density of the refined aluminum melt 7 by 3.0 g / cm 3 ;
[0111] (3) The container 9 containing the liquid electroslag and the refined aluminum melt 7 is moved out of the vacuum chamber 20 to the lifting and transporting device 10, and the liquid electroslag is poured into the electroslag recovery device 11. The molten aluminum material after the slag is transported to the bottom of the atmosphere protection furnace 16 and raised to the furnace body by the lifting and transporting device 10, and argon gas is continuously introduced into the furnace, and the pressure in the furnace is maintained at 10000 Pa and the temperature in the furnace is maintained at 750°C;
[0112] (4) The rotary crystallization device 14 is immersed in the molten aluminum material after slag pouring, and the depth of the rotary crystallization device 14 immersed in the molten aluminum material is 1 / 5 of the total depth of the molten aluminum material. Liquid argon is continuously introduced into the central layer 15 of the rotary crystallization device 14 while maintaining a rotating state, and the rotation speed is 200 rpm. The wall temperature of the rotary crystallization device 14 is reduced from the temperature of the molten aluminum material to 1200° C. within 30 minutes, and the temperature of the molten aluminum material is 1400° C.;
[0113] (5) After the aluminum of the outer layer of the rotary crystallization device 14 is solidified, it is lifted to the outside of the atmosphere protection furnace 16 at a rate of 10 mm / min, and high-purity regenerated aluminum S1 is obtained after separation. Then, the rotary crystallization device 14 is returned to the inside of the atmosphere protection furnace 16, and the operation of step (4) is repeated. During this process, the internal temperature and pressure of the atmosphere protection furnace 16 remain unchanged;
[0114] (6) Repeat steps (4) and (5) for a total of 5 times to obtain high-purity recycled aluminum S2-S6 with a weight of 15 kg each, lower the molten metal residue 17 out of the atmosphere protection furnace 16 and transport it to the molten metal residue recovery device 18 for recovery, and then transport the emptied container 9 to the bottom of the vacuum chamber 20 for the next electroslag remelting refining.
[0115] Example 5
[0116] This embodiment provides a method for regenerating metal by vacuum electroslag-rotational segregation, the method comprising the following steps:
[0117] (1) The containing container 9 is placed inside the vacuum chamber 20, and the non-consumable electrode 3 is inserted to the bottom of the containing container 9 to start the arc. The ratio of the outer diameter of the non-consumable electrode 3 to the inner diameter of the containing container 9 is 1 / 5, and the height ratio is 1 / 2; the solid electroslag 6 is added to the bottom of the non-consumable electrode 3 through the gap between the non-consumable electrode 3 and the containing container 9 by the automatic feeding device 2, and the solid electroslag 6 is heated and melted into electroslag melt and kept at 1600°C. The ratio of the thickness of the solid electroslag 6 to the inner height of the containing container 9 is 1 / 8; during the melting and continuous increase of the solid electroslag 6, the depth of the non-consumable electrode 3 inserted into the solid electroslag 6 is maintained at 1 / 5 of the thickness of the solid electroslag 6, and the vacuum degree of the vacuum chamber 20 is 10 -3pa; the composition of the solid electroslag is CaO-SiO2-Al2O3-TiO2-K2O-CaF2, and the melting point of the solid electroslag is 1350°C;
[0118] (2) Irregular titanium-silicon alloy scrap 1 with a size of 1 to 10 mm is added to liquid electroslag through an automatic feeding device 2, and a refined molten titanium-silicon alloy material 7 is obtained after passing through the liquid electroslag. The amount of irregular titanium-silicon alloy scrap 1 added is 250 kg; the material conductivity of the container 9 containing liquid electroslag and the refined molten titanium-silicon alloy material 7 is 650 s / cm, and the melting point of the material of the container 9 is 1700°C; the melting point of the irregular titanium-silicon alloy scrap 1 is 1500°C, and the purity of the irregular titanium-silicon alloy scrap 1 is 99.95%, wherein the impurities include Fe, Al, O, Al2O3, etc.; the density of the electroslag melt is less than the density of the refined molten titanium-silicon alloy material 7 by 0.5 g / cm 3 ;
[0119] (3) The container 9 containing the liquid electroslag and the refined molten titanium-silicon alloy material 7 is moved out of the vacuum chamber 20 to the lifting and transporting device 10, and the liquid electroslag is poured into the electroslag recovery device 11. The molten titanium-silicon alloy material after slag pouring is transported to the bottom of the atmosphere protection furnace 16 and raised to the furnace body by the lifting and transporting device 10, and argon gas is continuously introduced into the furnace, and the pressure in the furnace is maintained at 20000 Pa and the temperature in the furnace is maintained at 1600°C;
[0120] (4) The rotary crystallization device 14 is immersed in the molten titanium-silicon alloy material after slag pouring, and the depth of the rotary crystallization device 14 immersed in the molten titanium-silicon alloy material is 1 / 5 of the total depth of the molten titanium-silicon alloy material. Liquid argon is continuously introduced into the central layer 15 of the rotary crystallization device 14 while maintaining a rotating state, and the rotation speed is 200 rpm. The wall temperature of the rotary crystallization device 14 is reduced from the temperature of the molten titanium-silicon alloy material to 1200° C. within 30 minutes, and the temperature of the molten titanium-silicon alloy material is 1400° C.;
[0121] (5) After the titanium-silicon alloy of the outer layer of the rotary crystallization device 14 is solidified, it is lifted to the outside of the atmosphere protection furnace 16 at a rate of 10 mm / min, and high-purity regenerated titanium-silicon alloy S1 is obtained after separation. Then, the rotary crystallization device 14 is returned to the inside of the atmosphere protection furnace 16, and the operation of step (4) is repeated. During this process, the internal temperature and pressure of the atmosphere protection furnace 16 remain unchanged;
[0122] (6) Repeat steps (4) and (5) for a total of 3 times to obtain high-purity regenerated titanium silicon alloys S2-S4 with a weight of 25 kg each, lower the molten metal residue 17 out of the atmosphere protection furnace 16 and transport it to the molten metal residue recovery device 18 for recovery, and then transport the emptied container 9 to the bottom of the vacuum chamber 20 for the next electroslag remelting refining.
[0123] The purity of the high-purity recycled metals obtained in Examples 1 to 5 above is shown in Table 1.
[0124] Table 1
[0125] Heat Example 1 Example 2 Example 3 Example 4 Example 5 S1 99.999% 99.999% 99.99992% 99.9996% 99.995% S2 99.997% 99.998% 99.99991% 99.995% 99.993% S3 99.996% 99.997% 99.9999% 99.994% 99.991% S4 99.994% 99.995% 99.9998% 99.993% 99.99% S5 / 99.993% 99.9997% 99.991% / S6 / / 99.9996% 99.99% / S7 / / 99.9993% / /
[0126] In Table 1, “ / ” means no data.
[0127] It can be seen from Examples 1 to 5 that the vacuum electroslag-rotational segregation method for metal regeneration provided by the present invention can regenerate and purify single metal waste or alloy waste of different forms and properties, and the purity of the obtained recycled metal can reach more than 99.99%, which has a prospect for large-scale industrial application.
[0128] Example 6
[0129] This embodiment provides a method for regenerating metal by vacuum electroslag-rotational segregation. The density of the electroslag melt is greater than the density of the refined copper melt by 0.5 g / cm 3 Except for this, the rest are the same as in Example 1.
[0130] The density of the electroslag melt in this embodiment is 0.5 g / cm greater than the density of the refined copper melt. 3 , resulting in the electroslag melt being above the liquid level of the refined molten copper material, causing the non-consumable electrode to come into contact with the molten metal, and the current failing to pass through the electroslag, rendering the resistance heating effect of the electroslag ineffective. Moreover, the electroslag melt cannot be removed by dumping before entering the rotary segregation purification unit, further resulting in a significant reduction in the purity of the recycled metal.
[0131] Comparative Example 1
[0132] This comparative example provides an electroslag remelting process method, which is carried out by the method disclosed in Example 1 of CN111440956A.
[0133] Compared with Example 2, this comparative example must first melt the smelted raw materials into master alloy rods before electroslag remelting, and cannot directly process manganese waste that is brittle and difficult to make into rods. In addition, the purity of the alloy electroslag remelting ingot prepared in Comparative Example 1 is not significantly improved compared with the raw materials, and high-purity recycled metal cannot be obtained.
[0134] It can be seen that the device for vacuum electroslag-rotary segregation metal regeneration provided by the present invention adopts a vacuum electroslag refining unit coupled with a rotary segregation purification unit, thereby realizing the short-range, efficient, continuous and stable regeneration of high-value metals from metal wastes with multiple forms and different properties; the method for vacuum electroslag-rotary segregation metal regeneration provided by the present invention adopts slag washing countercurrent efficient smelting and rotary segregation dynamic interface impurity removal, thereby realizing the simultaneous removal of multiple impurities in metal wastes, and obtaining high-purity recycled metal with a purity ≥99.99%.
[0135] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for regenerating metal by vacuum electroslag-rotational segregation, characterized in that: The method is carried out using the following vacuum electroslag-rotational segregation metal regeneration device; The device comprises a vacuum electroslag refining unit, a rotary segregation purification unit and a transport unit; the vacuum electroslag refining unit and the rotary segregation purification unit are independently connected to the transport unit; The method comprises the following steps: (1) After the solid electroslag is melted into an electroslag melt in a vacuum electroslag refining unit, metal waste is added for refining treatment to obtain a metal melt and liquid electroslag; The density of the electroslag melt is less than 0.5 g / cm3 of the metal melt. 3 ~5.0g / cm 3 ; The melting point of the solid electroslag is 50°C to 200°C lower than the melting point of the molten metal; the temperature of the refining treatment is 50°C to 200°C higher than the melting point of the metal waste; (2) After removing the liquid electroslag, the metal melt is transported to a rotary segregation purification unit via a transport unit for rotary segregation purification to obtain high-purity recycled metal.
2. The method according to claim 1, characterized in that The vacuum electroslag refining unit includes a vacuum chamber.
3. The method according to claim 1, characterized in that The vacuum electroslag refining unit comprises a non-consumable electrode, a voltage control device and an automatic feeding device.
4. The method according to claim 3, characterized in that The automatic feeding device is arranged on one side of the upper part of the vacuum chamber.
5. The method according to claim 3, characterized in that: The non-consumable electrode and the voltage control device form an electric circulation loop with the containing container.
6. The method according to claim 3, characterized in that The ratio of the outer diameter of the non-consumable electrode to the inner diameter of the containing container is 1 / 10 to 1 / 2.
7. The method according to claim 3, characterized in that The ratio of the length of the non-consumable electrode to the inner height of the containing container is 1 / 2 to 2 / 1.
8. The method according to claim 1, characterized in that The rotary segregation purification unit includes an atmosphere protection furnace.
9. The method according to claim 8, characterized in that The atmosphere protection furnace comprises a heating chamber and a non-heating chamber.
10. The method according to claim 9, characterized in that The heating chamber is located at the lower part of the non-heating chamber.
11. The method according to claim 10, characterized in that The central axes of the heating chamber and the non-heating chamber overlap.
12. The method according to claim 11, characterized in that A rotating crystallization device is arranged on the central axis of the heating chamber and the non-heating chamber.
13. The method according to claim 12, characterized in that A double-layer sealing valve is arranged between the heating chamber and the non-heating chamber.
14. The method according to claim 13, characterized in that A transition chamber is arranged inside the double-layer sealing valve.
15. The method according to claim 1, characterized in that The transport unit includes an atmosphere protection chamber.
16. The method according to claim 15, characterized in that The atmosphere protection chamber is provided with a containing container, a lifting transport device, a closed-circuit transport track, an electroslag recovery device and a metal melt residual material recovery device.
17. The method according to claim 16, characterized in that The lifting and lowering transport device circulates along the closed-circuit transport track.
18. The method according to claim 1, characterized in that The vacuum electroslag refining unit and the rotary segregation purification unit are independently connected to the transport unit through the double-layer sealing valve at the furnace mouth.
19. The method according to claim 1, characterized in that The solid electroslag in step (1) includes any one of CaO, SiO2, Al2O3, MgO, FeO, CaF2, NaF, Na3AlF6, BaO, BaF2, TiO2, Cr2O3, B2O3, K2O, ZrO2, ZnO, Li2O, SrO, Ce2O3, PbO, CaCl2, NaCl or KCl, or a combination of at least two thereof.
20. The method according to claim 1, characterized in that The metal waste includes any one of iron, chromium, manganese, aluminum, copper, magnesium, potassium, sodium, calcium, strontium, barium, lead, zinc, tin, cobalt, nickel, antimony, cadmium, bismuth, gold, silver, platinum, ruthenium, palladium, lithium, beryllium, titanium, zirconium, vanadium, gallium, indium, thallium, germanium, lanthanum, cerium, neodymium, scandium or silicon, or a combination of at least two thereof.
21. The method according to claim 1, characterized in that The shape of the metal scrap includes any one of powder, sphere, cube, cone, prism or irregular shape or a combination of at least two of them.
22. The method according to claim 1, characterized in that The size of the metal scrap is 0.001 mm to 50 mm.
23. The method according to claim 1, characterized in that The absolute vacuum degree of the vacuum electroslag refining unit is 10 -3 Pa~10 -1 Pa.
24. The method according to claim 1, characterized in that In step (1), the ratio of the thickness of the electroslag melt to the inner height of the containing container is 1 / 10 to 1 / 2.
25. The method according to claim 1, characterized in that The ratio of the thickness of the solid electroslag to the inner height of the containing container is 1 / 10 to 1 / 2.
26. The method according to claim 3, characterized in that The depth of the non-consumable electrode immersed in the solid electroslag is 1 / 10 to 9 / 10 of the thickness of the solid electroslag.
27. The method according to claim 5, characterized in that The electrical conductivity of the material of the containing container is greater than 200 s / cm.
28. The method according to claim 5, characterized in that The melting point of the material of the containing container is greater than the melting point of the metal waste by more than 200°C.
29. The method according to claim 12, characterized in that In step (2), the depth of immersion of the rotary crystallization device in the metal melt is 1 / 5 to 1 / 1 of the depth of the metal melt.
30. The method according to claim 12, characterized in that The rotation speed of the rotary crystallization device is 1 r / min to 500 r / min.
31. The method according to claim 12, characterized in that The wall temperature of the rotary crystallization device is reduced from the temperature of the metal melt to 50°C to 200°C below the melting point of the metal scrap within 10 to 60 minutes.
32. The method according to claim 1, characterized in that The temperature of the metal melt is 50°C to 200°C higher than the melting point of the metal scrap.
33. The method according to claim 1, characterized in that The purity of the high-purity recycled metal is ≥99.99%.
34. The method according to claim 1, characterized in that Step (1) and step (2) are independently carried out under the protection of an inert atmosphere.
35. The method according to claim 34, characterized in that The inert atmosphere includes any one of a nitrogen atmosphere, an argon atmosphere or a helium atmosphere, or a combination of at least two of them.
36. The method according to claim 1, characterized in that The method comprises the following steps: (1) Solid electroslag is heated in the vacuum electroslag refining unit at an absolute vacuum of 10 -3 Pa~10 -1 Pa, and then add metal scraps with a size of 0.001 mm to 50 mm for refining to obtain metal melt and liquid electroslag; the ratio of the thickness of the electroslag melt to the inner height of the container is 1 / 10 to 1 / 2; the ratio of the thickness of the solid electroslag to the inner height of the container is 1 / 10 to 1 / 2; the depth of the non-consumable electrode immersed in the solid electroslag is 1 / 10 to 9 / 10 of the thickness of the solid electroslag; the density of the electroslag melt is less than the density of the metal melt by 0.5 to 5.0 g / cm 3 ; The melting point of the solid electroslag is 50°C to 200°C lower than the melting point of the metal melt; the temperature of the refining treatment is 50°C to 200°C higher than the melting point of the metal waste; the electrical conductivity of the material of the container is greater than 200s / cm; the melting point of the material of the container is more than 200°C higher than the melting point of the metal waste; (2) After removing the liquid electroslag, the molten metal is transported to a rotary segregation purification unit via a transport unit, and subjected to rotary segregation purification under an inert atmosphere to obtain a high-purity recycled metal with a purity of ≥99.99%; The depth of the rotary crystallization device immersed in the metal melt is 1 / 5 to 1 / 1 of the depth of the metal melt; the rotation speed of the rotary crystallization device is 1 to 500 r / min; the wall temperature of the rotary crystallization device is reduced from the temperature of the metal melt to 50°C to 200°C below the melting point of the metal waste within 10 to 60 minutes; the temperature of the metal melt is 50°C to 200°C higher than the melting point of the metal waste.