A prepreg containing biphenyl diphenol polyaryletherketone and a high-toughness composite material

By using bisperdinol polyaryletherketone thermoplastic toughened particles in prepregs and combining with fiber reinforcement, the lack of performance of polyamide toughened particles under humid and heat conditions is solved, and high damage tolerance and high compression are achieved Composite materials with strength are suitable for aerospace and other fields.

CN115710408BActive Publication Date: 2024-11-01AEROSPACE INST OF ADVANCED MATERIALS & PROCESSING TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211405552.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-10
Publication Date
2024-11-01
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

The existing prepregs containing polyamide toughened particles show low heat resistance, easy water absorption and poor compatibility with epoxy resin under humid and heat conditions, which affect the mechanical properties of composite materials, especially in the aerospace field. It is difficult to meet the needs of high compression strength and damage tolerance in applications.

Method used

Bifencin-containing polyaryletherketone is used as thermoplastic toughening particles, and it is swelled insoluble in epoxy resin, and reinforced with carbon fibers and other fibers, and has high damage tolerance, interlayer fracture toughness and wet/ Prepregs with compressive strength under thermal conditions.

Benefits of technology

It significantly improves the impact damage resistance and compression strength retention rate under wet/heat conditions, has low water absorption, and the compression strength after impact is higher than 350MPa, and the 0° compression strength retention rate under wet/heat conditions reaches more than 70%. , surpassing the properties of traditional thermoplastic particle toughened epoxy resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003936556120000021
    Figure BDA0003936556120000021
  • Figure BDA0003936556120000041
    Figure BDA0003936556120000041
  • Figure BDA0003936556120000061
    Figure BDA0003936556120000061
Patent Text Reader

Abstract

The present invention discloses a prepreg and a high-toughness composite material containing biphenyl diphenol polyaryletherketone, belonging to the technical field of composite materials. The prepreg comprises reinforcing fibers and an uncured resin matrix; the uncured resin matrix comprises a resin component, a curing agent, a soluble thermoplastic toughening agent and thermoplastic toughening particles, wherein the resin component comprises at least one epoxy resin, and the thermoplastic toughening particles comprise biphenyl diphenol polyaryletherketone. The thermoplastic toughening particles containing biphenyl diphenol polyaryletherketone have strong hydrophobicity, low water absorption, high heat resistance, and only swell but not dissolve in epoxy resin, which can significantly improve the post-impact compression strength of the composite material and the compression strength retention rate under hot and humid conditions, meeting the requirements of the aerospace field for high impact toughness of carbon fiber composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a prepreg containing biphenyl diphenol polyaryletherketone and a high-toughness composite material made of the prepreg, belonging to the technical field of composite materials. Background Art

[0002] Polymer-based composite materials have the advantages of high specific modulus, high specific strength, strong designability, excellent fatigue resistance, etc. Compared with metal materials, they have obvious structural weight reduction benefits and have become one of the main structural materials used in the contemporary aerospace field. For example, composite parts such as wings, fuselages, bulkheads and control surfaces are manufactured by molding and curing pre-impregnated composite materials (prepregs). The use of prepregs to manufacture composite parts can accurately control the amount and position of resin impregnated into the fiber network, ensuring the distribution of resin and fiber in the composite material, so that the composite material has sufficient mechanical properties.

[0003] The impact resistance of composite materials is a bottleneck that limits their application in aerospace and other fields. Thermosetting resin systems (such as epoxy resins, bismaleimide resins, etc.) usually have the disadvantages of low elongation at break and poor damage tolerance after curing. The corresponding composite materials show insufficient interlayer toughness. When subjected to low-speed impact, large-scale delamination is likely to occur between the layers, which seriously affects the load-bearing capacity and service life of the composite materials. Therefore, it is necessary to toughen the composite materials to improve their resistance to impact damage and delamination.

[0004] The interlaminar toughening method of thermoplastic resin particles can effectively improve the impact impedance and damage tolerance of thermosetting resin-based composite materials. The interlaminar particle toughening technology utilizes the advantages of thermosetting resin matrix and thermoplastic resin particles, and concentrates the thermosetting resin matrix with good process performance and high modulus in the fiber layer to achieve fiber infiltration, while the thermoplastic resin particles with excellent fracture toughness are mainly enriched in the interlaminar of the composite material, giving full play to its advantages of high fracture toughness, preventing the laminate from delamination damage and inhibiting the excessive expansion of cracks in the interlaminar resin matrix.

[0005] Interlayer particle toughening is currently the most commonly used, most mature and most extensive composite material toughening method. At present, the M21 and M91 systems of Hexel Corporation of the United States, the 3900 and 3960 systems of Toray Industries, Japan, and the X850 system of Cytec Technology Co., Ltd. of the United States all adopt interlayer particle toughening methods, which significantly improves the damage tolerance of the composite material system. The most critical thing about interlayer particle toughening is to select suitable interlayer toughening particles (thermoplastic resin particles). As early as 2008, in order to improve the damage tolerance of composite materials, Hexel Corporation simultaneously adopted toughening particles with a melting point higher than the curing temperature and toughening particles with a melting point lower than or equal to the curing temperature (CN101679606B). Further, in 2011, Hexel Corporation adopted a blend of insoluble elastic toughening particles and insoluble rigid toughening particles to improve composite material damage tolerance and interlayer toughness (CN102869507B). The toughening particles in these patents all involve different types of polyamides, indicating that polyamide is a preferred toughening particle. Similarly, other multiple patents disclosed by Hexel also involve the use of polyamide as toughening particles (CN104704029B, CN106062051B, CN110337461B). Toray Industries, Ltd. of Japan also reported the toughening effect of different polyamides and prepared different types of polyamide particles (CN104955883B). Cytec Technology Co., Ltd. of the United States uses a combination of insoluble toughening particles and swellable toughening particles in a patent (CN103249776A) to improve the interlaminar toughness of composite materials, which also involves a variety of polyamide particles.

[0006] Although polyamide is a preferred thermoplastic interlayer toughening particle, it also has shortcomings such as low heat resistance, easy water absorption, and poor compatibility with epoxy resin, which will affect the tensile and compression mechanical properties of composite parts to a certain extent, especially the compression performance under wet and hot conditions. In the aerospace field, resin-based composite parts usually need to maintain high compressive strength under both room temperature / dry and hot / wet conditions. Therefore, it is necessary to screen new interlayer toughening particles to develop prepregs with high damage tolerance, interlayer fracture toughness and compressive strength under wet / hot conditions to meet the continuous demand for high-performance prepregs in the aerospace field. Summary of the invention

[0007] The purpose of the present invention is to solve the problem of insufficient moisture and heat resistance of conventional prepregs containing polyamide toughening particles, and to propose a prepreg containing biphenyl diphenol polyaryletherketone and a high-toughness composite material made of the prepreg. By using a thermoplastic toughening particle containing biphenyl diphenol polyaryletherketone, a prepreg with high damage tolerance, interlaminar fracture toughness and compressive strength under wet / hot conditions is developed. It includes the following aspects:

[0008] The first aspect of the present invention provides a prepreg containing biphenyl diphenol polyaryletherketone, comprising reinforcing fibers and an uncured resin matrix; the uncured resin matrix comprises a resin component, a curing agent, a soluble thermoplastic toughening agent and thermoplastic toughening particles, wherein the resin component comprises at least one epoxy resin, the thermoplastic toughening particles comprise biphenyl diphenol polyaryletherketone, and the molecular structure of the biphenyl diphenol polyaryletherketone is as follows:

[0009]

[0010] Wherein, m and n are integers, and the ratio thereof may be 1:10 to 9:1. In order to ensure that the epoxy resin can swell but not completely dissolve in the epoxy resin system, the ratio of m to n is preferably 3:7 to 7:3.

[0011] Preferably, the reinforcing fiber is selected from one or more combinations of carbon fiber, glass fiber, aramid fiber, polyimide fiber, and more preferably carbon fiber.

[0012] Preferably, in the reinforcing fibers and the uncured resin matrix, the mass proportion of the uncured resin is 25% to 40%, but not limited thereto.

[0013] Preferably, the resin component comprises one or more of a difunctional epoxy resin, a trifunctional epoxy resin and a tetrafunctional epoxy resin, which is a saturated, unsaturated, cycloaliphatic, alicyclic or heterocyclic epoxy resin; the difunctional epoxy resin is selected from a combination of one or more of diglycidyl ether of bisphenol F, diglycidyl ether of bisphenol A, diglycidyl dihydroxynaphthalene, glycidyl ether of phenolic adduct, glycidyl ether of aliphatic diol, diglycidyl ether, diethylene glycol diglycidyl ether, and ... diglycidyl ether of phenolic adduct, diglycidyl ether of aliphatic diol, diglycidyl ether, diglycidyl ether of diethylene glycol, and the difunctional epoxy resin is selected from a combination of one or more of diglycidyl ether of bisphenol F, diglycidyl ether of bisphenol A, diglycidyl dihydroxynaphthalene, diglycidyl ether of phenolic adduct, diglycidyl ether of bisphenol A, diglycidyl ether of bisphenol A, diglycidyl dihydroxynaphthalene, diglycidyl ether of phenolic adduct, diglycidyl ether of bisphenol F, diglycidyl ether of bisphenol A, diglycidyl dihydroxynaphthalene, di The amount of the epoxy resin added is 10wt% to 40wt% of the uncured resin matrix, preferably 15wt% to 35wt%, and more preferably 20wt% to 25wt%; the trifunctional epoxy resin is trifunctional meta-glycidylamine, and the amount of the trifunctional epoxy resin added is 15wt% to 35wt% of the uncured resin matrix, preferably 20wt% to 30wt%; the tetrafunctional epoxy resin is tetrafunctional para-glycidylamine, 5wt% to 15wt%.

[0014] Preferably, the curing agent is one or more of anhydride, aromatic amine, polyol, cyanoguanidine, aromatic, aliphatic amine, acid anhydride, Lewis acid, substituted urea, imidazole and hydrazine, and the amount of the curing agent is 10wt% to 35wt% of the uncured resin matrix, preferably 15wt% to 25wt%.

[0015] Preferably, the soluble thermoplastic toughening agent is selected from one or more combinations of polyethersulfone, polysulfone, polyetherimide, polyimide, polyaryletherketone, polyaryletherketonenitrile, and block copolymer; preferably polyaryletherketone; the amount of the toughening agent is 3wt% to 25wt% of the uncured resin matrix, preferably 10wt% to 20wt%.

[0016] Preferably, the thermoplastic toughening particles also include copolymers of one or more of vinyl polymers, polyesters, polyamides, polyarylethers, polyarylether sulfides, polyethersulfones, polysulfones, polyetherketones, polyetheretherketones, polyurethanes, polycarbonates, polyamideimides, polyimides, polyetherimides, polyacetals, and polysiloxanes; preferably polyamides or polyimides, and the total addition amount of the thermoplastic toughening particles is 5wt% to 30wt% of the uncured resin matrix, preferably 5wt% to 15wt%.

[0017] Preferably, the addition amount of the biphenyl diphenol polyaryletherketone is 2 wt% to 20 wt% of the resin matrix.

[0018] The second aspect of the present invention provides a high-toughness composite material containing biphenyl diphenol polyaryletherketone, which is prepared by curing the prepreg containing biphenyl diphenol polyaryletherketone provided in the first aspect of the present invention.

[0019] Advantages of the present invention compared with the prior art

[0020] (1) Since the biphenyl diphenol polyaryletherketone thermoplastic toughened particles involved in the present invention are used for the first time in the preparation of high-toughness prepregs, and the prepared composite materials have high damage tolerance, interlaminar fracture toughness and compressive strength under wet / hot conditions, they are significantly innovative.

[0021] (2) The polyaryletherketone molecular chain used in the present invention contains a biphenol structure, which only swells but does not dissolve in epoxy resin. On the one hand, compared with polyamide particles, swelling improves the interfacial bonding force of epoxy resin. On the other hand, when the resin system is composited with reinforcing fibers, since the thermoplastic particles swell instead of dissolving in the matrix resin, they can be well retained on the fiber surface, significantly improving the impact damage resistance of the composite material and making the post-impact compression strength higher than 350MPa.

[0022] (3) Since the thermoplastic toughening particles containing biphenyl diphenol polyaryletherketone used in the present invention have strong hydrophobicity, low water absorption and high heat resistance; therefore, the composite material parts prepared by the prepreg containing the toughening particles have low water absorption and high compressive strength under wet / hot conditions. Tests show that the 0° compressive strength retention rate of the cured laminate under wet / hot conditions can reach more than 70%, which is significantly higher than the 50% to 60% retention rate of existing thermoplastic particle toughened epoxy resins, and can be used in aerospace, rail transportation, weapons and equipment and other fields. DETAILED DESCRIPTION

[0023] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0024] The present invention provides a prepreg containing biphenyl diphenol polyaryletherketone, comprising reinforcing fibers and an uncured resin matrix. The reinforcing fibers may be any conventional fibers in the prepreg industry. The uncured resin matrix comprises a resin component, a curing agent, a soluble thermoplastic toughening agent and thermoplastic toughening particles. The resin component comprises at least one epoxy resin; the thermoplastic toughening particle component comprises biphenyl diphenol polyaryletherketone, having the following structure:

[0025]

[0026] Wherein, m and n are integers, and the ratio thereof may be 1:10 to 9:1. In order to ensure that the epoxy resin can swell but not completely dissolve in the epoxy resin system, the ratio of m to n is preferably 3:7 to 7:3.

[0027] According to some embodiments, the reinforcing fiber is selected from a combination of one or more of carbon fiber, glass fiber, aramid fiber, and polyimide fiber; more preferably, carbon fiber.

[0028] According to some embodiments, in the reinforcing fibers and the uncured resin matrix, the mass proportion of the uncured resin is 25% to 40%, but not limited thereto.

[0029] According to some embodiments, the resin component may be a saturated, unsaturated, cycloaliphatic, alicyclic or heterocyclic epoxy resin, and may be one or more of a difunctional epoxy resin, a trifunctional epoxy resin and a tetrafunctional epoxy resin.

[0030] According to some embodiments, the difunctional epoxy resin is exemplified by: diglycidyl ether of bisphenol F, diglycidyl ether of bisphenol A (optionally brominated), diglycidyl dihydroxynaphthalene, glycidyl ether of phenolic adducts, glycidyl ether of aliphatic diols, diglycidyl ether, one of diethylene glycol diglycidyl ether or any combination thereof. The most preferred is diglycidyl ether of bisphenol F (Shanghai Huayi Resin Factory 370). The addition amount of the difunctional epoxy resin is 10wt% to 40wt% of the uncured resin matrix, preferably 15wt% to 35wt%, and more preferably 20wt% to 25wt%.

[0031] According to some embodiments, the trifunctional epoxy resin is understood to have three epoxy groups directly or indirectly located at the para or meta position on the benzene ring of the main chain of the compound, and trifunctional meta-glycidylamine is selected; the tetrafunctional epoxy resin is understood to have four epoxy groups directly or indirectly located at the para or meta position on the benzene ring of the main chain of the compound, and tetrafunctional para-glycidylamine is selected. A preferred exemplary trifunctional epoxy resin is triglycidyl meta-aminophenol (AFG-90M of Shanghai Huayi Resin Factory). A preferred exemplary tetrafunctional epoxy resin is tetraglycidyl para-aminophenol (1721 of Hanshuo High-tech Materials Co., Ltd.). The addition amount of the trifunctional epoxy resin is 15wt% to 35wt% of the uncured resin matrix, preferably 20wt% to 30wt%. The addition amount of the tetrafunctional epoxy resin is 5wt% to 15wt% of the uncured resin matrix.

[0032] According to some embodiments, the curing agent includes one or more of anhydride, aromatic amine, polyol, cyanoguanidine, aromatic, aliphatic amine, anhydride, Lewis acid, substituted urea, imidazole and hydrazine. Exemplary preferred curing agents include 4,4'-diaminodiphenyl sulfone (4,4'-DDS) and 3,3'-diaminodiphenyl sulfone (3,3'-DDS). The amount of curing agent is 10wt% to 35wt% of the uncured resin matrix, preferably 15wt% to 25wt%.

[0033] According to some embodiments, the soluble thermoplastic toughening agent is usually added to the resin matrix as particles and dissolved in the resin mixture by heating before adding the curing agent, including: polyethersulfone, polysulfone, polyetherimide, polyimide, polyaryletherketone, polyaryletherketonenitrile, block copolymer; preferably polyaryletherketone. The amount of toughening agent is 3wt% to 25wt% of the uncured resin matrix, preferably 10wt% to 20wt%.

[0034] According to some embodiments, the thermoplastic toughening particles can be used alone or mixed with other types of thermoplastic particles. The material of other types of thermoplastic particles is not particularly limited, and can be vinyl polymers, polyesters, polyamides, polyarylethers, polyarylether sulfides, polyethersulfones, polysulfones, polyetherketones, polyetheretherketones, polyurethanes, polycarbonates, polyamideimides, polyimides, polyetherimides, polyacetals, polysiloxanes and copolymers thereof, etc.; preferably polyamides and polyimides. The total amount of thermoplastic toughening particles added is 5wt% to 30wt% of the uncured resin matrix, preferably 5wt% to 15wt%.

[0035] According to some embodiments, the biphenyl diphenol polyaryletherketone is added in an amount of 2 wt % to 20 wt % of the uncured resin matrix.

[0036] According to some embodiments, the uncured resin matrix is ​​processed according to a standard prepreg resin matrix, and various epoxy resins are mixed at room temperature to form a resin mixture; a thermoplastic toughening agent is added to the resin mixture, and then heated to about 120° C. and maintained for about 1-2 hours to dissolve the soluble thermoplastic toughening agent; the mixture is then cooled to about 80° C., and the remaining ingredients (thermoplastic particle component, curing agent and other additives (if any)) are mixed into the resin and stirred evenly to form a resin matrix.

[0037] The invention discloses a high-toughness composite material containing biphenyl diphenol polyaryletherketone, which is prepared by curing a prepreg containing biphenyl diphenol polyaryletherketone.

[0038] Uncured matrix resin is applied to fiber reinforced material according to any known prepreg manufacturing technology. Fiber reinforced material can be impregnated with matrix resin in whole or in part. Prepreg is usually covered on two faces with a protective film and rolled up for storage and transportation at the following temperature, and the temperature is usually kept far below room temperature to avoid premature curing. The fibrous reinforcement material of prepreg can be selected from mixed or mixed fiber systems, including synthetic fibers or natural fibers, or their combination. This fibrous reinforcement material can preferably be selected from any suitable material, such as glass fiber, carbon fiber or aramid fiber. This fibrous reinforcement material is preferably carbon fiber, can be woven, non-curled, nonwoven, unidirectional or multiaxial fabric structure form.

[0039] The following are several specific embodiments of the present invention, and the raw materials used in each embodiment are commercially available products:

[0040] Embodiments 1 to 4

[0041] Preferred exemplary resin matrix formulations according to the present invention are listed in Table 1. The uncured resin matrix resin preparation steps are as follows: various epoxy resins are mixed at room temperature to form a resin mixture; a thermoplastic toughening agent is added to the resin mixture, and then heated to about 130° C. for about 1-2 hours to dissolve the soluble thermoplastic toughening agent; then the mixture is cooled to about 80° C., the remaining ingredients are mixed into the resin, and stirred to form a resin matrix.

[0042] The steps of preparing the prepreg are as follows: impregnating a unidirectional carbon fiber layer with the resin formulation of Table 1 to form a prepreg consisting of reinforcing fibers and an uncured resin matrix. Among them, the unidirectional carbon fiber used is Guangwei Extension CCFT800S carbon fiber, the resin content is controlled at 34wt%, and the fiber surface density is 194 grams per square meter. The post-impact compression strength and tensile strength tests are carried out in accordance with the corresponding ASTM standards.

[0043] Comparative Example 1

[0044] The resin matrix and the cured prepreg were prepared in the same manner as in Example 1. The difference was that polyamide PA6 particles (1013B) were used instead of biphenyl diphenol-containing polyaryletherketone, and the specific composition and content were shown in Table 1.

[0045] Comparative Example 2

[0046] The resin matrix and the cured prepreg were prepared in the same manner as in Example 2. The difference was that polyamide particles (Rilsan PA11) were used instead of the biphenyl diphenol-containing polyaryletherketone. The specific components and contents were shown in Table 1.

[0047] Comparative Example 3

[0048] The resin matrix and the cured prepreg were prepared in the same manner as in Example 3. The difference was that polyaryletherketone particles were used instead of biphenyl diphenol-containing polyaryletherketone, and the specific composition and content were shown in Table 1. It is worth noting that the polyaryletherketone used here was ultrafine powder with an average particle size of 30 μm, and was added in powder form at 80°C.

[0049] Table 1 Different resin matrix formulations

[0050]

[0051]

[0052] As can be seen from Table 1, the composite material after the prepreg is cured using the resin matrix formula containing biphenyl diphenol polyaryletherketone thermoplastic toughening particles has a high post-impact compressive strength, and the maximum value can reach 369MPa. In particular, compared with Comparative Example 3, after the polyaryletherketone particles are used to replace the biphenyl diphenol polyaryletherketone, the post-impact compressive strength of the composite material decreases. Combined with the metallographic microscope test results, it can be found that this is because the biphenyl diphenol polyaryletherketone only swells but does not dissolve during the resin curing process, and can be better retained on the surface of the fiber to form a more stable and regular thermoplastic toughening layer, thereby improving the composite material's ability to resist impact damage.

[0053] It can also be seen from Table 1 that the resin matrix formula using thermoplastic toughening particles containing biphenyl diphenol polyaryletherketone has a higher compression strength retention rate under wet and hot conditions. The compression strength retention rate under wet and hot conditions is higher than 70%, and some can be higher than 75%, which is significantly higher than the 50% to 60% retention rate of existing thermoplastic particle toughened epoxy resin composite materials. This is because the thermoplastic toughening particles containing biphenyl diphenol polyaryletherketone used in the present invention are highly hydrophobic, low in water absorption, and high in heat resistance; therefore, the composite material parts prepared with the prepreg containing the toughening particles have low water absorption and high compression strength under wet / hot conditions.

[0054] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A prepreg containing biphenyl diphenol polyaryletherketone, characterized in that: The invention comprises reinforcing fibers and an uncured resin matrix; the uncured resin matrix comprises a resin component, a curing agent, a soluble thermoplastic toughening agent and thermoplastic toughening particles, wherein the resin component comprises at least one epoxy resin, and the thermoplastic toughening particles comprise biphenyl diphenol polyaryletherketone, and the molecular structure of the biphenyl diphenol polyaryletherketone is as follows: Among them, m and n are integers, and the ratio of m to n is 3:7 to 7:

3.

2. The prepreg according to claim 1, wherein the reinforcing fiber is selected from a combination of one or more of carbon fiber, glass fiber, aramid fiber and polyimide fiber. 3 . The prepreg according to claim 1 , wherein the mass proportion of the uncured resin matrix in the reinforcing fibers and the uncured resin matrix is ​​25% to 40%.

4. The prepreg according to claim 1, wherein the resin component comprises one or more of a difunctional epoxy resin, a trifunctional epoxy resin and a tetrafunctional epoxy resin, and is a saturated, unsaturated, cycloaliphatic, alicyclic or heterocyclic epoxy resin.

5. The prepreg as claimed in claim 4, wherein the difunctional epoxy resin is selected from the group consisting of one or more combinations of diglycidyl ether of bisphenol F, diglycidyl ether of bisphenol A, diglycidyl dihydroxynaphthalene, glycidyl ether of phenolic adducts, glycidyl ether of aliphatic diols, diglycidyl ether, and diethylene glycol diglycidyl ether, and the addition amount thereof is 10wt% to 40wt% of the uncured resin matrix; the trifunctional epoxy resin is trifunctional meta-glycidyl amine, and the addition amount thereof is 15wt% to 35wt% of the uncured resin matrix; the tetrafunctional epoxy resin is tetrafunctional para-glycidyl amine, 5wt% to 15wt%.

6. The prepreg according to claim 1, wherein the curing agent is a combination of one or more of anhydride, aromatic amine, polyol, cyanoguanidine, aromatic, aliphatic amine, acid anhydride, Lewis acid, substituted urea, imidazole and hydrazine, and the addition amount thereof is 10wt% to 35wt% of the uncured resin matrix.

7. The prepreg according to claim 1, wherein the soluble thermoplastic toughening agent is selected from one or more combinations of polyethersulfone, polysulfone, polyetherimide, polyimide, polyaryletherketone, polyaryletherketonenitrile, and block copolymer, and the added amount is 3wt% to 25wt% of the uncured resin matrix.

8. The prepreg as claimed in claim 1, wherein the thermoplastic toughening particles further comprise copolymers of one or more of vinyl polymers, polyesters, polyamides, polyarylethers, polyarylether sulfides, polyethersulfones, polysulfones, polyetherketones, polyetheretherketones, polyurethanes, polycarbonates, polyamideimides, polyimides, polyetherimides, polyacetals, and polysiloxanes; and the total addition amount of the thermoplastic toughening particles is 5wt% to 30wt% of the resin matrix.

9. The prepreg according to claim 1, wherein the amount of the biphenyl diphenol polyaryletherketone added is 2 wt% to 20 wt% of the uncured resin matrix.

10. A high-toughness composite material containing biphenyl diphenol polyaryletherketone, characterized in that: The prepreg according to any one of claims 1 to 9 is prepared by curing.