Adhesive composite structure and its forming method, mucus and its use and using method
By using cross-linked polymer materials with hydrophilic blocks and lipophilic blocks in the adhesive, the solvent exchange mechanism is used to achieve high-strength adhesion under water and oil, which solves the problem of adhesives in multiple environments in the existing technology. It solves the problem of poor adhesion performance in medium and realizes a simple and economical multi-environment adhesion solution.
Patent Information
- Application Number
- CN202110986176.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-08-26
AI Technical Summary
Existing adhesives are difficult to achieve effective adhesion in oil, oil-wet, underwater, and water-wet environments, and the preparation process is complex and cannot meet the application needs of multiple environments at the same time.
A cross-linked polymer material with hydrophilic blocks and lipophilic blocks is used to form an adhesive layer through polymerization initiated by ultraviolet light. The solvent exchange mechanism is used to achieve adhesion under water or oil. Holes are distributed inside the adhesive layer to increase strength. .
It achieves high-strength adhesion in underwater and oil environments, simplifies the preparation process, reduces costs, and is suitable for adhesion applications in a variety of complex environments.
Smart Images

Figure CN115725254B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of adhesives, and specifically relates to a universal adhesive that can be used in oil-under-oil, oil-wet, underwater, and water-wet environments and its use, as well as an adhesive composite structure formed in the oil-under-oil, oil-wet, underwater, and water-wet environments and a forming method thereof. Background Art
[0002] In the field of adhesion, the adhesion strength of adhesives will be greatly reduced or even fail when subjected to various harsh environments, such as underwater environments such as automobiles or weak current, oil pipelines, tunnels, water pipe leaks, underwater robots, biological surfaces, tissues and organs, and other underwater or complex environments. Currently, commercial adhesives are difficult to achieve adhesion in oily, oil-wet, underwater, or water-wet environments, and are difficult to meet the application requirements of the above specific scenarios.
[0003] The existing methods for solving the underwater adhesion problem are mainly based on bionic adhesives of mussels, sand worms, octopuses, tree frogs, and throat fish. Some of them rely on molecules, such as the adhesion of catechol, while others rely on structures, such as using suction cups to form negative pressure, and others rely on capillary forces and mechanical interlocking structures to achieve adhesion in underwater environments.
[0004] The existing technology for solving the problem of oil adhesion mainly includes the following methods:
[0005] One of the prior art provides an octopus-like suction cup structure adhesive tape that can achieve adhesion under silicone oil (Baik S, Kim DW, Park Y, Lee TJ, Ho Bhang S, Pang CA wet-tolerant adhesive patch inspired by protuberances in suction cups of octopi. Nature 2017, 546, 396). However, the adhesive tape requires a complex structural design, a cumbersome preparation process, and only studies the adhesion strength in silicone oil, while the alkane oil commonly used in life may cause the tape to swell and lose its adhesion performance.
[0006] The second prior art provides a base-based gel adhesive tape that can achieve adhesion in different organic solvents, including alkane oils (Liu X, Zhang Q, Duan L, Gao G. Tough adhesion of nucleobase-tackifed gels in diverse solvents. Adv. Funct. Mater. 2019, 29, 1900450). However, the tape requires complex synthesis steps, and the adhesion strength of this gel tape is relatively low, with a maximum of only 10 to 20 kPa.
[0007] The third prior art provides an adhesive patch based on a shape memory polymer that can adhere in vegetable oil (Park JK, Eisenhaure JD, Kim S. Reversible underwater dry adhesion of a shape memory polymer. Adv. Mater. Interfaces 2019, 6, 1801542). However, the adhesive patch requires pre-pressure to passively remove the oil layer, and commonly used alkane oils may cause the material to swell.
[0008] It can be seen that in the prior art, whether it is underwater or oil-based adhesives, they often require complex molecular synthesis or surface structure construction, and the preparation process is cumbersome and complicated. At present, there is no adhesive glue or adhesive composite structure that can achieve underwater / oil adhesion at the same time, and it is impossible to achieve universal adhesion in multiple environments. The art needs to develop a high-strength adhesive glue or adhesive composite structure that is low in cost, simple to prepare, and can achieve adhesion on different substrates underwater and under oil. Summary of the invention
[0009] In view of the above technical problems, one of the purposes of the present invention is to provide an adhesive composite structure, through which the adhesive composite structure can achieve the adhesion of the target object under water or oil. The underwater or oil environment refers to that the adhesion interface of the target object is completely or mostly exposed to the aqueous or oily environment, typically but not limitedly including the adhesion of the target object in the aqueous or oily environment, or the adhesion of another target object when the surface of one target object contains more water or oil.
[0010] The adhesive composite structure of the present invention comprises a substrate and an adhesive layer adhered to the substrate, wherein holes are distributed inside the adhesive layer; the adhesive layer is a cross-linked polymer material having both hydrophilic blocks and lipophilic blocks.
[0011] In the adhesive composite structure provided by the present invention, the cross-linked polymer material of the adhesive layer has both hydrophilic blocks and lipophilic blocks, so that the adhesive composite structure can achieve adhesion under water or under oil. When in an underwater environment, the water-soluble hydrophilic blocks stretch to adhere to the substrate, and the water-insoluble lipophilic blocks aggregate to provide bulk strength, thereby achieving underwater adhesion; when in an oil-under-oil environment, the oil-soluble lipophilic blocks stretch to adhere to the substrate, and the oil-insoluble hydrophilic blocks aggregate to provide bulk strength, thereby achieving oil-under-oil adhesion. That is, one block aggregates to increase strength, and the other block is used for adhesion, and the holes distributed inside the adhesive layer are generated by solvent exchange between the organic solvent and water / oil.
[0012] As a preferred technical solution, the adhesion strength between the adhesive layer and the substrate is greater than 0, and there is a continuous medium around the adhesive layer; the continuous medium includes an oily continuous medium or an aqueous continuous medium. The adhesion strength between the adhesive layer and the substrate is greater than 0, thereby ensuring that there is adhesion strength between the two, and there is a continuous medium around the adhesive layer, ensuring that solvent exchange occurs in the continuous medium, one block can aggregate to provide strength, and the other block is used for adhesion.
[0013] As a preferred technical solution, a hydrophilic group is grafted onto the hydrophilic block;
[0014] Preferably, the hydrophilic group includes a cationic hydrophilic group, an anionic hydrophilic group and a nonionic hydrophilic group;
[0015] Preferably, the cationic hydrophilic group includes any one of a tertiary amine group and a quaternary amine group, or a combination of at least two thereof;
[0016] Preferably, the anionic hydrophilic group includes any one of a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, and a sulfate group, or a combination of at least two thereof;
[0017] Preferably, the nonionic hydrophilic group includes any one or a combination of at least two of a hydroxyl group, an ether group, an amine group, an amide group, dopamine and a dopamine derivative;
[0018] Preferably, the hydrophilic group includes any one or a combination of at least two of a carboxyl group, an amide group, a hydroxyl group, dopamine and a dopamine derivative.
[0019] The hydrophilic block has a hydrophilic group. By selecting a suitable hydrophilic group, the hydrophilic block is easily soluble in water and can stretch underwater to adhere to the substrate, thereby achieving underwater adhesion.
[0020] As a preferred technical solution, a hydrophobic group is grafted onto the lipophilic block;
[0021] Preferably, the hydrophobic group includes any one of an alkyl group, an ester group, an ether group, and an aromatic group, or a combination of at least two thereof;
[0022] Preferably, the hydrophobic group includes R-COO-, and the R includes a C1-C14 straight or branched alkyl group;
[0023] Preferably, the hydrophobic group includes any one of a methyl group, an ethyl group, a propyl group, a methyl ester group, an ethyl ester group, a butyl ester group, an octyl ester group, a hexyl ester group, and a lauryl ester group, or a combination of at least two of them.
[0024] There are hydrophobic groups on the lipophilic block. By selecting appropriate hydrophobic groups, the lipophilic block is easily soluble in organic solvents and can stretch under oil to adhere to the substrate, thereby achieving adhesion under oil.
[0025] A second object of the present invention is to provide a method for forming an adhesive composite structure, the method comprising the following steps:
[0026] (1) Prepare mucus as follows:
[0027] The hydrophilic monomer, the lipophilic monomer, the photoinitiator, the crosslinking agent and the organic solvent are uniformly mixed to obtain a dispersed liquid, and after ultraviolet light exposure, a mucus is obtained, wherein the polarity of the organic solvent is 4 to 8;
[0028] (2) Covering the mucus on the surface of a target substrate in an underwater environment or an underwater environment, and allowing it to stand and solidify, thereby obtaining a composite structure consisting of the substrate and an adhesive layer adhered to the substrate.
[0029] Compared with the traditional adhesion in air, the biggest problem of adhesion in underwater (water-wet) or oil-wet (oil-wet) environment is the existence of water film or oil film. Water film or oil film has a stronger barrier effect between the adhesive material and the adhesive interface than the adhesive interface in air, and will destroy the adhesion performance of some commonly used water-soluble or oil-soluble adhesives.
[0030] The hydrophilic monomer, lipophilic monomer and crosslinking agent in the present invention are photopolymerized by ultraviolet light under the action of a photoinitiator to form a copolymer having both a hydrophilic block and a lipophilic block, which is uniformly dispersed in an organic solvent to form a transparent mucus with a certain viscosity. When the mucus is dripped into water, the organic solvent in the adhesive rapidly exchanges with water, the medium water enters the adhesive phase, the organic solvent diffuses from the adhesive phase to the water phase, and drives away the water film, and the entry of water also causes the polymer in the adhesive to phase separate, the water-insoluble lipophilic block aggregates to provide bulk strength, and the water-soluble hydrophilic block stretches to adhere to the substrate, thereby achieving underwater adhesion. When the adhesive is dropped into an oil-based environment, the situation is the opposite to that under water, that is, the organic solvent in the adhesive rapidly exchanges with the oil, the medium oil enters the adhesive phase, the organic solvent diffuses from the adhesive phase to the oil phase, and drives away the oil film. The entry of oil also causes the polymer in the adhesive to phase separate, the hydrophilic blocks insoluble in oil aggregate to provide bulk strength, and the lipophilic blocks soluble in oil stretch to adhere to the substrate, thereby achieving oil-based adhesion. That is, a composite structure of one block aggregates to increase strength and the other block is used for adhesion, and due to the diffusion of the solvent, holes are formed inside the adhesive layer.
[0031] As a preferred technical solution, the hydrophilic monomer is a substituted or unsubstituted acrylic acid having a hydrophilic group;
[0032] Preferably, the hydrophilic monomer includes any one or a combination of at least two of acrylic acid, acrylamide, hydroxyl, dopamine and dopamine derivatives.
[0033] As a preferred technical solution, the lipophilic monomer is a substituted or unsubstituted acrylate;
[0034] Preferably, the lipophilic monomer includes any one of methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, hexyl methacrylate, and lauryl methacrylate, or a combination of at least two thereof.
[0035] As a preferred technical solution, the photoinitiator includes any one of benzophenones and benzoyls or a combination of at least two thereof, preferably 2,2-diethoxyacetophenone or 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone;
[0036] The cross-linking agent includes any one or a combination of at least two of polyisocyanates, polyamines, polyols, glycidyl ethers, organic peroxides, organosilicones, metal organic compounds, and inorganic substances, preferably polyethylene glycol dimethacrylate;
[0037] The organic solvent includes any one of ethanol, tetrahydrofuran, acetone, dimethyl sulfoxide, methanol and dimethylformamide, or a combination of at least two thereof.
[0038] As a preferred technical solution, the ultraviolet irradiation time is more than 20 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes, preferably 25 to 35 minutes;
[0039] Preferably, the power range of the ultraviolet light is 200-800W, for example 200W, 300W, 400W, 500W, 600W, 700W, 800W, preferably 500W.
[0040] As a preferred technical solution, the static curing time is 15 to 30 seconds, for example, 15 seconds, 20 seconds, 25 seconds, or 30 seconds.
[0041] The third object of the present invention is to provide a mucus obtained by subjecting a mixture comprising a hydrophilic monomer, a lipophilic monomer, a photoinitiator, a crosslinking agent and an organic solvent to ultraviolet light; the organic solvent has a polarity of 4 to 8;
[0042] Preferably, the hydrophilic monomer is a substituted or unsubstituted acrylic acid having a hydrophilic group;
[0043] Preferably, the hydrophilic monomer includes any one or a combination of at least two of acrylic acid, acrylamide, hydroxyl, dopamine and dopamine derivatives.
[0044] Preferably, the lipophilic monomer is a substituted or unsubstituted acrylate;
[0045] Preferably, the lipophilic monomer includes any one of methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, hexyl methacrylate, and lauryl methacrylate, or a combination of at least two thereof;
[0046] Preferably, the photoinitiator comprises any one of benzophenones and benzoyls or a combination of at least two thereof, preferably 2,2-diethoxyacetophenone or 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone;
[0047] The cross-linking agent includes any one or a combination of at least two of polyisocyanates, polyamines, polyols, glycidyl ethers, organic peroxides, organosilicones, metal organic compounds, and inorganic substances, preferably polyethylene glycol dimethacrylate;
[0048] The organic solvent includes any one or a combination of at least two of ethanol, tetrahydrofuran, acetone, dimethyl sulfoxide, methanol and dimethylformamide;
[0049] Preferably, during the preparation of the mucus, the amount of the hydrophilic monomer added is 0.1-8 mol / L, and the amount of the lipophilic monomer added is 0.1-4 mol / L, for example 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 3 mol / L, 4 mol / L. Too little hydrophilic or lipophilic monomer content will affect the aggregation and stretching of the hydrophilic / hydrophobic segments in the adhesive in the underwater / oil environment, thereby affecting the bulk and interfacial adhesion strength of the adhesive; too much hydrophilic or lipophilic monomer content will lead to a relative decrease in the organic solvent content in the adhesive, slowing down the solvent exchange, reducing the degree of phase separation, and resulting in a decrease in adhesion strength. The amount of the photoinitiator added is 0.01-4 mg / mL, for example, 0.01 mg / mL, 0.05 mg / mL, 0.1 mg / mL, 1 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL. Too little photoinitiator content will result in incomplete polymerization and reduced adhesion strength; too much photoinitiator content will result in implosion and cause the adhesive to lose its adhesion effect. The amount of the crosslinking agent added is 0.1-8 mg / mL, for example, 0.1 mg / mL, 0.5 mg / mL, 1 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL. Too little crosslinking agent content will result in incomplete crosslinking of the polymer and reduce the adhesion strength of the adhesive; too high crosslinking agent content will result in excessive crosslinking of the polymer, which will be in a gel state and cause the adhesive to lose its adhesion effect.
[0050] Preferably, the ultraviolet irradiation time is more than 20 min, for example 20 min, 25 min, 30 min, 35 min, 40 min, preferably 25 to 35 min;
[0051] Preferably, the power of the ultraviolet light is 200-800W, for example, 200W, 300W, 400W, 500W, 600W, 700W, 800W, preferably 500W.
[0052] If the UV irradiation time is too short or the light power is too low, the polymer polymerization will be incomplete, forming short-chain polymers and reducing the adhesion strength of the adhesive; if the UV irradiation time is too long or the light power is too high, the polymer will be over-cross-linked, and the heat emitted by the UV light will easily cause the polymer to explode and evaporate the organic solvent, greatly reducing the adhesion strength of the adhesive.
[0053] The fourth object of the present invention is to provide a use of the mucus, wherein the mucus is used as any one of an underwater adhesive and an oil-based adhesive or a combination of the two;
[0054] Preferably, the underwater adhesive is used for underwater leak prevention, underwater intelligent robots, biological surface adhesion, tissue adhesion, or any one or a combination of at least two thereof;
[0055] Preferably, the oil-under-oil adhesive is used for any one of pipes, oil tanks, and mechanical oil surface bonding, or a combination of at least two of them.
[0056] A fifth object of the present invention is to provide a method for using the mucus, wherein the mucus is used in an underwater environment, and the method comprises:
[0057] The mucus is contacted with the substrate to be adhered, and the diffusion time is maintained for 15 to 30 seconds to achieve adhesion;
[0058] or applying the mucus on the adhesive substrate to obtain an adhesive substrate coated with mucus; attaching the adhesive substrate coated with mucus to a target substrate to be adhered to achieve adhesion to the target substrate;
[0059] Preferably, the adhesive substrate is a flexible substrate insoluble in organic solvents, preferably any one of polyester film, nitrocellulose film, polyimide film, polyethylene film, polypropylene film, and polytetrafluoroethylene film.
[0060] As a preferred technical solution, the mucus is used in an oil-under-oil environment, and the method of use includes:
[0061] (1) deprotonating the mucus to obtain deprotonated mucus;
[0062] (2) The deprotonated mucus is quickly brought into contact with the substrate to be adhered, and the diffusion time is maintained for 15 to 30 seconds to achieve adhesion.
[0063] As a preferred technical solution, the deprotonation is achieved by adding a sodium hydroxide solution to the mucus;
[0064] Preferably, during the deprotonation process, the amount of sodium hydroxide added is 5-50% of the volume of the mucus, and the concentration of sodium hydroxide is 0.1-2 mol / L.
[0065] If the sodium hydroxide content is too low, the groups on the hydrophilic chain segments in the adhesive will not be completely deprotonated, resulting in low chain aggregation in the oil environment and reduced bulk strength; if the sodium hydroxide content is too high, it will be difficult to disperse in the adhesive and reduce the adhesion strength.
[0066] Compared with the prior art, this application has the following beneficial effects:
[0067] (1) The present invention provides an adhesive composite structure that can achieve adhesion in both underwater and oily environments. The cross-linked polymer used in the adhesive layer of the adhesive composite structure has both hydrophilic blocks and oleophilic blocks, one of which is aggregated to increase strength and the other is used for adhesion, thereby achieving effective adhesion in both underwater (water-wet) and oily (oil-wet) environments.
[0068] (2) The present invention also provides a method for forming an adhesive composite structure. The method does not require complex molecular synthesis or surface structure construction, has a simple preparation process, is low in price, has a short curing time, can achieve adhesion in a variety of complex environments, and has broad application prospects in real life.
[0069] (3) The present invention also provides a mucus used for an adhesive composite structure. The purpose and method of use of the mucus, as described above, can simultaneously achieve adhesion to a target object in an underwater or water-wet environment and in an oil-wet environment, filling a gap in the field. The use process is simple, and only requires mixing the components, performing a photopolymerization reaction, and then quickly bonding the adhesive object to achieve adhesion to the target object. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 It is the hole structure of the adhesive layer in the adhesive composite structure.
[0071] Figure 2 A diagram showing the morphology of mucus and its adhesion under oil and water.
[0072] Figure 3 The slime can achieve adhesion both under water and under oil when using different types of solvents.
[0073] Figure 4 The adhesion strength of mucus composed of different types of solvents.
[0074] Figure 5 is the adhesion strength of mucus on different substrates.
[0075] Figure 6 is the adhesion strength of mucus at different bonding times. DETAILED DESCRIPTION
[0076] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. The following embodiments are only exemplary to illustrate and explain the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0077] Example
[0078] The specific components and lighting conditions of Examples 1 to 18 of the present application are detailed in Table 1-1 and Table 1-2. The specific conditions of Example 1 are as follows: 7.21 g of acrylic acid, 8.51 g of hexyl methacrylate, 0.1 g of polyethylene glycol dimethacrylate, 40 mg of 2,2-diethoxyacetophenone and 40 mg of Irga 2959 are dispersed in 25 mL of ethanol and irradiated under ultraviolet light for 30 minutes at a power of 500 W to obtain a transparent mucus with a certain viscosity.
[0079] The reaction conditions of Example 2-18 are the same as those of Example 1 except for the conditions shown in the table.
[0080] Comparative Example 1 does not contain a hydrophilic monomer, Comparative Example 2 does not contain a lipophilic monomer, Comparative Example 3 does not contain a photoinitiator, Comparative Example 4 does not contain a crosslinking agent, and Comparative Example 5 does not contain an organic solvent. Other conditions are the same as those in Example 1.
[0081] Table 1-1
[0082]
[0083]
[0084] Table 1-2
[0085]
[0086] Application Examples
[0087] Application Example 1
[0088] The obtained mucus is used in an underwater environment, and the method of use comprises:
[0089] The mucus is contacted with the substrate to be adhered and maintained for a diffusion time of 30 seconds to achieve adhesion.
[0090] Application Example 2
[0091] The obtained mucus is used in an underwater environment, and the method of use comprises:
[0092] The mucus is smeared on the adhesive substrate to obtain an adhesive substrate smeared with mucus; the adhesive substrate smeared with mucus is attached to a target substrate to be attached to achieve attachment to the target substrate.
[0093] Application Example 3
[0094] The obtained mucus is used in an oil-under-oil environment, and the method of use comprises:
[0095] (1) deprotonating the mucus, i.e., deprotonating the carboxylate groups with a 1 mol / L sodium hydroxide solution (adding 0.3 mL of sodium hydroxide solution per 1 mL of the adhesive) to obtain a deprotonated mucus;
[0096] (2) The deprotonated mucus is quickly brought into contact with the substrate to be adhered, and the diffusion time is maintained for 30 seconds to achieve adhesion.
[0097] Application Example 4
[0098] The above mucus is quickly spread on a substrate film (such as polyester or nitrocellulose film) to prepare a simple adhesive tape.
[0099] Performance Testing
[0100] The target substrate with the adhesive substrate is subjected to the following performance tests:
[0101] (1) Adhesion performance: A glass slide was placed underwater as the target substrate, and then the prepared mucus was dropped onto the surface of the target substrate. Then, another target substrate was placed as the upper surface in contact with the target substrate surface in the solution, and a pre-pressure of 2 N was applied. After standing for a period of time, the substrate was pulled upward. The force measured when the two substrates were separated was the adhesion force between the upper and lower solid surfaces.
[0102] The test results are shown in Table 2
[0103] Table 2
[0104]
[0105] As can be seen from Table 2, the new multi-environment universal mucus composed of hydrophilic monomers, lipophilic monomers, photoinitiators, crosslinking agents, and organic solvents exhibits good adhesion to the target substrate both under oil and water. By adjusting the content and type of organic solvents, hydrophilic monomers, and lipophilic monomers, the desired corresponding product can be obtained.
[0106] 1. By comparing Examples 1-14, it is known that the mucus composed of various hydrophilic monomers, lipophilic monomers, photoinitiators, crosslinking agents, and organic solvents can achieve effective adhesion both under oil and under water. Figure 3 , Figure 4 As shown, the slime can achieve adhesion both under water and under oil when using different types of solvents.
[0107] 2. By comparing Examples 15-18, it is known that if the UV irradiation time is too short or the illumination power is too low, the polymer polymerization will be incomplete, reducing the adhesion strength of the adhesive; if the UV irradiation time is too long or the illumination power is too high, the polymer will be over-crosslinked, and the heat emitted by the UV light will easily cause the polymer to explode, greatly reducing the adhesion strength of the adhesive.
[0108] 3. It can be seen from the adhesion results of Comparative Examples 1-5 that the five active ingredients of the mucus of the present application are indispensable.
[0109] from Figure 1 It can be seen that since the mucus used in the present application has both hydrophilic segments and lipophilic segments, when used underwater or under oil, obvious holes will be formed inside the adhesive layer after solvent exchange with water / oil.
[0110] from Figure 2 It can be seen that the mucus used in the present application is a mucus with a certain viscosity, and can achieve adhesion both underwater and under oil.
[0111] from Figure 5 It can be seen that the mucus of the present application can achieve adhesion on different substrates.
[0112] from Figure 6 It can be seen that the adhesive strength of the mucus of the present application increases with the increase of bonding time and reaches stability at 2 minutes.
[0113] The applicant declares that the present application uses the above-mentioned embodiments to illustrate the process method of the present application, but the present application is not limited to the above-mentioned process steps, that is, it does not mean that the present application must rely on the above-mentioned process steps to be implemented. The technicians in the relevant technical field should understand that any improvement to the present application, the equivalent replacement of the raw materials selected in the present application, the addition of auxiliary components, the selection of specific methods, etc., all fall within the scope of protection and disclosure of the present application.
Claims
1. An adhesive composite structure, characterized in that: The adhesive composite structure comprises a substrate and an adhesive layer adhered to the substrate, wherein holes are distributed inside the adhesive layer; The adhesive layer is a cross-linked polymer material having a hydrophilic block and a lipophilic block; When in an underwater environment, the water-soluble hydrophilic blocks stretch to adhere to the substrate, and the water-insoluble lipophilic blocks aggregate to provide bulk strength, thereby achieving underwater adhesion; when in an oil-under-oil environment, the oil-soluble lipophilic blocks stretch to adhere to the substrate, and the oil-insoluble hydrophilic blocks aggregate to provide bulk strength, thereby achieving oil-under-oil adhesion; The adhesion strength between the adhesion layer and the substrate is greater than 0, and a continuous medium is disposed around the adhesion layer; the continuous medium includes an oily continuous medium or an aqueous continuous medium; The hydrophilic block has a hydrophilic group; the lipophilic block has a hydrophobic group; during the preparation of the composite structure, the amount of hydrophilic monomers added to provide the hydrophilic group is 0.1-8 mol / L, and the amount of lipophilic monomers added to provide the lipophilic group is 0.1-4 mol / L.
2. The adhesive composite structure according to claim 1, characterized in that: The hydrophilic group includes a cationic hydrophilic group, an anionic hydrophilic group and a nonionic hydrophilic group.
3. The adhesive composite structure according to claim 2, characterized in that: The cationic hydrophilic group includes any one of a tertiary amine group and a quaternary amine group, or a combination of at least two of them.
4. The adhesive composite structure according to claim 2, characterized in that: The anionic hydrophilic group includes any one of a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, and a sulfate group, or a combination of at least two of them.
5. The adhesive composite structure according to claim 2, characterized in that: The nonionic hydrophilic group includes any one of hydroxyl group, ether group, amine group, amide group, dopamine and derivatives thereof, or a combination of at least two thereof.
6. The adhesive composite structure according to claim 1, characterized in that: The hydrophilic group includes any one or a combination of at least two of a carboxyl group, an amide group, a hydroxyl group, dopamine, and a dopamine derivative.
7. The adhesive composite structure according to claim 1, characterized in that: The hydrophobic group includes any one of an alkyl group, an ester group, an ether group, and an aromatic group, or a combination of at least two of them.
8. The adhesive composite structure according to claim 1, characterized in that: The hydrophobic group includes R-COO-, and the R includes a C1-C14 straight-chain or branched alkyl group.
9. The adhesive composite structure according to claim 1, characterized in that: The hydrophobic group includes any one of methyl, ethyl, propyl, methyl ester, ethyl ester, butyl ester, octyl ester, hexyl ester, and lauryl ester, or a combination of at least two of them.
10. A method for forming an adhered composite structure according to any one of claims 1 to 9, characterized in that: The forming method comprises the following steps: (1) Prepare mucus as follows: The hydrophilic monomer, the lipophilic monomer, the photoinitiator, the crosslinking agent and the organic solvent are uniformly mixed to obtain a dispersed liquid, and after ultraviolet light exposure, a mucus is obtained; the polarity of the organic solvent is 4 to 8; (2) Covering the mucus on the surface of a target substrate in an underwater environment or an underwater environment, and allowing it to stand and solidify, thereby obtaining an adhesive composite structure including the substrate and an adhesive layer adhered to the substrate.
11. The forming method according to claim 10, characterized in that: The hydrophilic monomer is a substituted or unsubstituted acrylic acid having a hydrophilic group.
12. The forming method according to claim 10, characterized in that: The hydrophilic monomer includes any one or a combination of at least two of acrylic acid, acrylamide, hydroxyl, dopamine and dopamine derivatives.
13. The forming method according to any one of claims 10 to 12, characterized in that: The lipophilic monomer is a substituted or unsubstituted acrylic acid ester.
14. The forming method according to claim 13, characterized in that: The lipophilic monomer includes any one of methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, hexyl methacrylate, and lauryl methacrylate, or a combination of at least two of them.
15. The forming method according to any one of claims 10 to 12 and 14, characterized in that: The photoinitiator includes any one of benzophenones and benzoyls or a combination of at least two thereof; The cross-linking agent includes any one of polyisocyanates, polyamines, polyols, glycidyl ethers, organic peroxides, organosilicones, metal organic compounds, and inorganic substances, or a combination of at least two thereof; The organic solvent includes any one of ethanol, tetrahydrofuran, acetone, dimethyl sulfoxide, methanol and dimethylformamide, or a combination of at least two thereof.
16. The forming method according to claim 15, characterized in that: The photoinitiator includes 2,2-diethoxyacetophenone or 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone; The cross-linking agent includes polyethylene glycol dimethacrylate.
17. The forming method according to any one of claims 10 to 12, 14 and 16, characterized in that: The ultraviolet irradiation time is more than 20 minutes, and the power range of the ultraviolet irradiation is 200-800W.
18. The forming method according to claim 9, characterized in that: The ultraviolet irradiation time is 25 to 35 minutes; the ultraviolet irradiation power is 500W.
19. The forming method according to any one of claims 10 to 12, 14, 16, and 18, characterized in that: The static curing time is 15 to 30 seconds.
20. A mucus, characterized in that The mucus is obtained by subjecting a mixture of a hydrophilic monomer, a lipophilic monomer, a photoinitiator, a crosslinking agent and an organic solvent to ultraviolet light; the polarity of the organic solvent is 4-8.
21. A mucus according to claim 20, characterized in that The hydrophilic monomer is a substituted or unsubstituted acrylic acid having a hydrophilic group.
22. A mucus according to claim 20, characterized in that The hydrophilic monomer includes any one or a combination of at least two of acrylic acid, acrylamide, hydroxyl, dopamine and dopamine derivatives.
23. The mucus according to claim 20, characterized in that The lipophilic monomer is a substituted or unsubstituted acrylic acid ester.
24. The mucus according to claim 20, characterized in that The lipophilic monomer includes any one of methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isooctyl methacrylate, hexyl methacrylate, and lauryl methacrylate, or a combination of at least two of them.
25. The mucus according to claim 20, characterized in that The photoinitiator includes any one of benzophenones and benzoyls, or a combination of at least two of them.
26. A mucus according to claim 25, characterized in that The photoinitiator includes 2,2-diethoxyacetophenone or 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.
27. A mucus according to claim 20, characterized in that The cross-linking agent includes any one of polyisocyanates, polyamines, polyols, glycidyl ethers, organic peroxides, organosilicones, metal organic compounds, and inorganic substances, or a combination of at least two of them.
28. The mucus according to claim 20, characterized in that The cross-linking agent includes polyethylene glycol dimethacrylate.
29. A mucus according to claim 20, characterized in that The organic solvent includes any one of ethanol, tetrahydrofuran, acetone, dimethyl sulfoxide, methanol and dimethylformamide, or a combination of at least two thereof.
30. The mucus according to claim 20, characterized in that During the preparation of the mucus, the amount of the hydrophilic monomer added is 0.1-8 mol / L, the amount of the lipophilic monomer added is 0.1-4 mol / L, the amount of the photoinitiator added is 0.01-4 mg / mL, and the amount of the cross-linking agent added is 0.1-8 mg / mL.
31. A mucus according to claim 20, characterized in that The ultraviolet irradiation time is more than 20 minutes.
32. A mucus according to claim 20, characterized in that The ultraviolet irradiation time is 25 to 35 minutes.
33. A mucus according to claim 20, characterized in that The power of the ultraviolet light is 200-800W.
34. A mucus according to claim 20, characterized in that The power of the ultraviolet light is 500W.
35. Use of the mucus according to any one of claims 20 to 34, characterized in that: The mucus is used as either one of an underwater adhesive and an oil-based adhesive or a combination of at least two of them.
36. The use of mucus according to claim 35, characterized in that The underwater adhesive is used for underwater leak prevention, underwater intelligent robots, biological surface adhesion, and tissue adhesion, any one of them or a combination of at least two of them.
37. The use of mucus according to claim 36, characterized in that The oil-under-oil adhesive is used for any one of or a combination of at least two of the following: pipes, oil tanks, and mechanical oil surfaces.
38. A method of using the mucus according to any one of claims 20 to 34, characterized in that: The mucus is used in an underwater environment, and the method of use comprises: The mucus is contacted with the substrate to be adhered, and the diffusion time is maintained for 15 to 30 seconds to achieve adhesion; Alternatively, the mucus is applied on the adhesive substrate to obtain an adhesive substrate coated with mucus; the adhesive substrate coated with mucus is attached to the target substrate to be attached to achieve attachment to the target substrate.
39. The method for using mucus according to claim 38, characterized in that: The adhesive substrate is a flexible substrate insoluble in organic solvents, preferably any one of polyester film, nitrocellulose film, polyimide film, polyethylene film, polypropylene film and polytetrafluoroethylene film.
40. A method of using the mucus according to any one of claims 20 to 34, characterized in that: The mucus is used in an oil-under-oil environment, and the method of use comprises: (1) deprotonating the mucus to obtain deprotonated mucus; (2) The deprotonated mucus is quickly brought into contact with the substrate to be adhered, and the diffusion time is maintained for 15 to 30 seconds to achieve adhesion.
41. The method of use according to claim 40, characterized in that: The deprotonation is achieved by adding sodium hydroxide solution to the mucus.
42. The method of use according to claim 41, characterized in that: During the deprotonation process, the amount of sodium hydroxide added is 5-50% of the volume of the mucus, and the concentration of sodium hydroxide is 0.1-2 mol / L.