A catalytic conversion method and device for producing ethylene, propylene and light aromatics
By using different catalysts and reaction conditions to process heavy and light raw materials in catalytic cracking technology, and using coupled heat utilization, the problem of insufficient yields of ethylene, propylene and light aromatics in the existing technology has been solved, and efficient ethylene, propylene and light aromatics have been achieved. Production of propylene and light aromatics reduces energy consumption.
Patent Information
- Application Number
- CN202111016666.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-08-31
AI Technical Summary
Existing catalytic cracking technology is difficult to effectively process heavy raw materials, and it is difficult to achieve independent zone control of different reaction regeneration systems, resulting in insufficient yields of ethylene, propylene and light aromatics, insufficient heat utilization of the device, and high energy consumption.
Preheated heavy raw materials and catalysts containing Y-type and β-type molecular sieves are used for catalytic cracking in the first reactor. Light raw materials and catalysts containing MFI structure molecular sieves are used for catalytic cracking in the second reactor, and are regenerated. The heat coupling utilization of the reactor enables independent zone control of different reaction regeneration systems and improves the yields of ethylene, propylene and light aromatics.
Through coupled heat utilization, the yields of ethylene, propylene and light aromatics are increased, the energy consumption of the device is reduced, and efficient conversion of heavy raw materials and light raw materials is achieved.
Smart Images

Figure CN115725326B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of petroleum processing, and in particular, to a catalytic conversion method and device for producing ethylene, propylene and light aromatics. Background Art
[0002] In recent years, with the continuous development of the chemical industry, the demand for low-carbon olefins such as ethylene and propylene and light aromatics (benzene, toluene and xylene, referred to as BTX) has shown a rapid growth trend. At present, the main methods for producing low-carbon olefins are steam cracking technology, catalytic cracking technology, propane dehydrogenation to produce propylene technology and coal-to-methanol to produce olefins technology. BTX is mainly derived from light hydrocarbon reforming process and steam thermal cracking process. With the use of new light raw materials in steam cracking, the product distribution will change. For example, using ethane as a steam cracking raw material, compared with naphtha as a raw material, the proportion of ethylene in the product is significantly increased, while the yield of low-carbon olefins and light aromatics will be reduced. The catalytic cracking process can process heavy crude oil and can produce more low-carbon olefins and light aromatics, which is an effective supplementary measure for steam cracking technology. However, the conventional catalytic cracking process has a low yield of low-carbon olefins and light aromatics, among which the yield of low-carbon olefins does not exceed 15% of the crude oil, which is difficult to meet the market demand. Therefore, it is very necessary to develop a catalytic cracking technology that can process heavy crude oil and produce more low-carbon olefins and light aromatics.
[0003] Chinese patent document CN1031834A discloses a catalytic conversion method for producing low-carbon olefins. The method uses petroleum fractions, residual oil or crude oil with different boiling ranges as raw materials, a mixture containing Y zeolite and pentacyclic high-silicon zeolite as catalyst, and a fluidized bed or moving bed as a reactor. The reaction conditions are: temperature 500-650°C, pressure 0.15-0.30MPa, weight hourly space velocity 0.2-20h -1 , catalyst-oil ratio 2-12, the catalyst after reaction is charred and regenerated and then returned to the reactor for recycling. Compared with conventional catalytic cracking and steam cracking, this method can produce more propylene and butene.
[0004] Chinese patent document CN1566267A discloses a catalytic thermal cracking method for producing ethylene and propylene from petroleum hydrocarbons. In this method, a preheated petroleum hydrocarbon feedstock is fed into a riser reactor, contacted with a hot catalyst containing a five-membered ring high-silicon zeolite, and reacted under catalytic thermal cracking conditions. The five-membered ring high-silicon zeolite contains phosphorus and transition metals. This method can increase the yield of light olefins, especially ethylene and propylene.
[0005] Chinese patent document CN104560149A discloses a catalytic conversion method for producing butene. The method has a total of 4 reactors. In addition to the reactor configuration of double risers plus fluidized bed, a fluidized bed reactor is also set outside the settler for cracking the gasoline fraction, and the reaction product enters the riser reactor to continue the cracking reaction. The catalyst after the reaction is charred and regenerated and then returned to the reactor for recycling. The method uses a mixture containing Y zeolite and β zeolite as a catalyst, and can obtain a higher yield of propylene and butene.
[0006] Chinese patent document CN102206509A discloses a hydrocarbon catalytic conversion method for producing propylene and light aromatics. The method adopts a combined reactor form of a double riser and a fluidized bed reactor, wherein heavy hydrocarbons and a cracking catalyst containing modified beta zeolite are contacted and reacted in a first reactor, and C4 hydrocarbons and / or light gasoline fractions and a cracking catalyst containing modified beta zeolite are contacted and reacted in a second reactor and then introduced into a third reactor for further reaction. The third reactor is a fluidized bed reactor, which creates conditions for the secondary cracking reaction of the gasoline fraction, thereby increasing the yield of propylene and light aromatics.
[0007] Chinese patent document CN102690680A discloses a catalytic conversion method and device for producing propylene. The method allows heavy raw materials to contact and react with a catalyst with Y-type zeolite as the main active component in the first riser reactor, and allows light hydrocarbons to contact and react with a catalyst with a selective zeolite with a pore size of less than 0.7nm as the main active component in the second riser reactor. The device adopts a combined reactor configuration formed by a double riser reactor and a fluidized bed, and the stripper is separated into two independent stripping zones by a partition. The method can realize the reaction and regeneration of two different catalysts in one reaction device, and the structure is simple.
[0008] The above technologies improve the yield of light olefins and light aromatics by adjusting the catalyst formula, adopting a combined reactor form combining a riser and a fluidized bed, and using different catalysts for different hydrocarbon feedstocks. However, it is difficult to achieve separate zoning control of different reaction regeneration systems. The yields of ethylene, propylene and light aromatics need to be further improved, and there is no coupled utilization of the device heat to reduce energy consumption. Summary of the invention
[0009] The purpose of the present disclosure is to provide a method for effectively adjusting the reaction environment of heavy feedstocks and light feedstocks, and separately controlling different reaction regeneration systems to achieve coupled utilization of heat and increase the yields of ethylene, propylene and light aromatics.
[0010] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a catalytic conversion method for producing ethylene, propylene and light aromatics, the method comprising:
[0011] S1, feeding the preheated heavy raw material into the first reactor, contacting it with the heavy oil catalyst containing Y-type molecular sieve and β-type molecular sieve, and performing the first catalytic cracking reaction to obtain the first reaction oil gas and the first spent catalyst;
[0012] S2, feeding the light raw material into the second reactor, contacting it with the light oil catalyst containing the MFI structure molecular sieve, and performing a second catalytic cracking reaction to obtain a second reaction oil gas and a second catalyst to be produced; introducing the second reaction oil gas into the raw material preheater, exchanging heat with the heavy raw material to obtain the preheated heavy raw material;
[0013] S3. After stripping, the first catalyst to be regenerated is introduced into the first regenerator for a first regeneration reaction to obtain a first regenerated catalyst and a first regenerated flue gas; part or all of the first regenerated flue gas is introduced into the second regenerator, and the first regenerated catalyst is returned to the first reactor; after stripping, the second catalyst to be regenerated is introduced into the second regenerator for a second regeneration reaction to obtain a second regenerated catalyst and a second regenerated flue gas, and the second regenerated catalyst is returned to the second reactor.
[0014] Optionally, the heavy feedstock is selected from one or more of vacuum wax oil, atmospheric residue oil, vacuum residue oil, coker wax oil, deasphalted oil, furfural refined raffinate oil, coal liquefaction oil, oil sand oil, shale oil, distillate oil obtained by FT synthesis and animal and vegetable oil; the light feedstock includes at least one of C4 hydrocarbons and light gasoline fractions; the C4 hydrocarbons are a mixture of C4 alkanes and C4 olefins; the content of C4 olefins in the C4 hydrocarbons is greater than 50% by weight, preferably greater than 60% by weight; the light gasoline fraction The invention relates to a novel light gasoline fraction comprising olefin-rich light gasoline, wherein the olefin content of the light gasoline fraction is 20-95% by weight, preferably 50-95% by weight; the weight ratio of the light raw material to the heavy raw material is 0.02-0.6:1, preferably 0.04-0.3:1; the weight ratio of the C4 hydrocarbon to the heavy raw material is 0-0.30:1, preferably 0.02-0.15:1; the weight ratio of the light gasoline fraction to the heavy raw material is 0-0.30:1, preferably 0.02-0.15:1.
[0015] Optionally, the first reactor comprises a first riser reactor and / or a first fluidized bed reactor, preferably a combination reactor of a first riser reactor and a first fluidized bed reactor; in the combination reactor, the first fluidized bed reactor is located above the first riser reactor and is connected to the first riser reactor.
[0016] Optionally, the reaction temperature of the first riser reactor is 500-580°C, preferably 520-560°C; the catalyst-oil ratio is 2-25, preferably 5-20; the reaction time is 0.5-10 seconds, preferably 1-5 seconds; the reaction temperature of the first fluidized bed reactor is 480-560°C, preferably 500-540°C; the weight hourly space velocity is 1-20 hours -1 , preferably 2-8 hours -1 ; Catalyst density is 50-350kg / m 3 , preferably 100-250kg / m 3 ; The bed height of the first fluidized bed reactor is 1 / 2-4 / 5 of the height of the first fluidized bed reactor, preferably 1 / 2-3 / 4 of the height of the first fluidized bed reactor; The pressure inside the first fluidized bed reactor is 0.1-0.4MPa, preferably 0.15-0.3MPa.
[0017] Optionally, the second reactor is a combined reactor of a second riser reactor and a second fluidized bed reactor, and the second fluidized bed reactor is located above the second riser reactor and is connected to the second riser reactor.
[0018] Optionally, the reaction temperature of the second riser reactor is 630-690°C, preferably 650-670°C; the catalyst-oil ratio is 20-80, preferably 40-60; the reaction time is 0.5-15 seconds, preferably 1-10 seconds; the reaction temperature of the second fluidized bed reactor is 590-650°C, preferably 610-630°C; the weight hourly space velocity is 1-20 hours -1 , preferably 2-8 hours -1 The catalyst density in the second fluidized bed reactor is 50-350 kg / m 3 , preferably 100-250kg / m 3 ; The bed height of the second fluidized bed reactor is 1 / 2-4 / 5 of the height of the second fluidized bed reactor, preferably 1 / 2-3 / 4 of the height of the second fluidized bed reactor; The pressure inside the second fluidized bed reactor is 0.1-0.4MPa, preferably 0.15-0.3MPa.
[0019] Optionally, the temperature of the preheated heavy feedstock is 100-350°C, preferably 150-300°C.
[0020] Optionally, the first regeneration reaction includes complete regeneration or incomplete regeneration, preferably incomplete regeneration; the regeneration temperature in the first regenerator is 620-720°C, preferably 650-680°C; the second regeneration reaction includes complete regeneration or incomplete regeneration, preferably complete regeneration; the regeneration temperature in the second regenerator is 650-750°C, preferably 680-730°C.
[0021] Optionally, the heavy oil catalyst comprises the Y-type molecular sieve, the β-type molecular sieve, a first clay and a first binder; based on the total weight of the heavy oil catalyst, the content of the Y-type molecular sieve is 20-60% by weight, preferably 30-50% by weight; the content of the β-type molecular sieve is 1-40% by weight, preferably 1-20% by weight; the content of the first clay is 10-70% by weight, preferably 15-45% by weight; the content of the first binder is 10-40% by weight, preferably 20-35% by weight; the Y-type molecular sieve is selected from HY type molecular sieve, USY The β-type molecular sieve is at least one of a β-type molecular sieve, a REUSY-type molecular sieve, a REY-type molecular sieve, a REHY-type molecular sieve, a DASY-type molecular sieve and a REDASY-type molecular sieve; the β-type molecular sieve is a β-type molecular sieve modified by phosphorus and a transition metal M, wherein M is selected from at least one of Fe, Co, Ni, Cu, Mn, Zn and Sn; the first clay is selected from at least one of kaolin, montmorillonite and bentonite; the first binder is selected from at least one of silica sol, alumina sol and pseudo-boehmite, preferably, the first binder is a double aluminum binder of alumina sol and pseudo-boehmite.
[0022] Optionally, the light oil catalyst comprises the MFI structure molecular sieve, a second clay and a second binder; based on the total weight of the light oil catalyst, the content of the MFI structure molecular sieve is 20-60% by weight, preferably 30-50% by weight; the content of the second clay is 10-70% by weight, preferably 15-45% by weight; the content of the second binder is 10-40% by weight, preferably 20-35% by weight; the MFI structure molecular sieve is selected from at least one of ZRP molecular sieve, phosphorus-containing ZRP molecular sieve, rare earth-containing ZRP molecular sieve, ZRP molecular sieve containing phosphorus and rare earth, ZRP molecular sieve containing phosphorus and alkaline earth metal, and ZRP molecular sieve containing phosphorus and transition metal, preferably ZRP zeolite containing phosphorus and rare earth; the second clay is selected from at least one of kaolin, montmorillonite, and bentonite; the second binder is selected from at least one of silica sol, aluminum sol and pseudo-boehmite, preferably, the second binder is a double aluminum binder of aluminum sol and pseudo-boehmite.
[0023] Optionally, the method further comprises: separating the second reaction oil gas after heat exchange to obtain olefin-containing C4 hydrocarbons and light gasoline fraction segments, and returning part or all of the olefin-containing C4 hydrocarbons and the light gasoline fraction segments to the second reactor.
[0024] The second aspect of the present disclosure provides a device for a catalytic conversion method for producing ethylene, propylene and light aromatics, the catalytic conversion device comprising a first reactor, a second reactor, a first regenerator, a second regenerator and a raw material preheater, the first reactor being connected to the first regenerator through a first catalyst delivery pipeline; the second reactor being connected to the second regenerator through a second catalyst delivery pipeline; the first reactor comprising an inlet for preheated heavy raw materials, the second reactor comprising an outlet for reaction oil and gas of light raw materials, the raw material preheater comprising an inlet for reaction oil and gas before heat exchange, an outlet for reaction oil and gas after heat exchange, an inlet for heavy raw materials before preheating and an outlet for heavy raw materials after preheating; the outlet for reaction oil and gas of light raw materials is connected to the inlet for reaction oil and gas before heat exchange, and the outlet for heavy raw materials after preheating is connected to the inlet for heavy raw materials after preheating of the first reactor; the first regenerator and the second regenerator are arranged in parallel or coaxially, preferably in parallel; the first regenerator comprises a first regeneration flue gas outlet, the second regenerator comprises a first regeneration flue gas inlet, and the first regeneration flue gas outlet is connected to the first regeneration flue gas inlet.
[0025] Through the above technical scheme, in the catalytic conversion method and device provided by the present disclosure, the heavy raw material and the light raw material react in different reaction regeneration systems respectively, which can realize the separate zone control of the reaction and regeneration of different heavy raw materials and light raw materials, and adopt different catalysts and reaction conditions to strengthen the primary cracking of heavy raw materials and the secondary cracking reaction of light raw materials, so as to improve the yield of ethylene, propylene and light aromatics; at the same time, the first regeneration flue gas generated by the first regenerator provides heat for the regeneration of the light oil catalyst to reach the temperature required for the regeneration of the light oil catalyst, and provides heat for the catalytic conversion reaction of the light raw material. The second reaction oil gas generated by the catalytic cracking of the light raw material provides heat for the preheating of the heavy raw material, and the energy consumption of the device can be greatly reduced through the coupled utilization of heat.
[0026] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0028] Figure 1 is a schematic flow diagram of an apparatus suitable for the catalytic conversion method disclosed herein;
[0029] Figure 2 It is a specific embodiment of the device applicable to the catalytic conversion method of the present disclosure;
[0030] Figure 3 is another specific embodiment of the device applicable to the catalytic conversion method of the present disclosure;
[0031] Figure 4 It is a preferred embodiment of the device suitable for the catalytic conversion method disclosed in the present invention;
[0032] Figure 5 It is another specific embodiment of the device suitable for the catalytic conversion method disclosed in the present invention.
[0033] Description of Reference Numerals
[0034] 1First reactor 2First regenerator
[0035] 3 Second regenerator 4 Second reactor
[0036] 5Raw material preheater
[0037] 1-1 First riser reactor 1-2 First stripper
[0038] 1-3 The first fluidized bed reactor 1-4 The first settler
[0039] 101 Heavy raw material 102 Cracking heavy oil
[0040] 103 first pre-lifting gas 104 first stripping gas
[0041] 105 First stripping baffle 106 Heavy oil catalyst delivery pipeline
[0042] 107 first cyclone separator 108 second cyclone separator
[0043] 109 first gas collecting chamber 110 first separation system pipeline
[0044] 2-1 The first regenerator 201 The first regenerator main air inlet pipeline
[0045] 202 Heavy oil regeneration catalyst delivery pipeline 203 The third cyclone separator
[0046] 204 fourth cyclone separator 205 second air collecting chamber
[0047] 206 First regeneration flue gas
[0048] 3-1 Second regenerator 301 Second regenerator main air inlet pipeline
[0049] 302 Light oil regeneration catalyst delivery pipeline 303 Fifth cyclone separator
[0050] 304 sixth cyclone separator 305 fourth air collecting chamber
[0051] 306 Second regeneration flue gas
[0052] 4-1 Second riser reactor 4-2 Second stripper
[0053] 4-3 Second fluidized bed reactor 4-4 Second settler
[0054] 401 Part 1 Light Raw Materials 402 Part 2 Light Raw Materials
[0055] 403 second pre-lifting gas 404 second stripping gas
[0056] 405 Second air lift baffle 406 Light oil catalyst delivery pipeline
[0057] 407 seventh cyclone separator 408 eighth cyclone separator
[0058] 409 third gas collecting chamber 410 second separation system pipeline
[0059] 501 Reaction oil and gas before heat exchange 502 Reaction oil and gas after heat exchange
[0060] 503 Heavy raw material before preheating 504 Heavy raw material after preheating DETAILED DESCRIPTION
[0061] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0062] A first aspect of the present disclosure provides a catalytic conversion method for producing ethylene, propylene and light aromatics, the method comprising:
[0063] S1, feeding the preheated heavy raw material into the first reactor, contacting it with the heavy oil catalyst containing Y-type molecular sieve and β-type molecular sieve, and performing the first catalytic cracking reaction to obtain the first reaction oil gas and the first spent catalyst;
[0064] S2, feeding the light raw material into the second reactor, contacting it with the light oil catalyst containing the MFI structure molecular sieve, and performing a second catalytic cracking reaction to obtain a second reaction oil gas and a second catalyst to be produced; introducing the second reaction oil gas into the raw material preheater, exchanging heat with the heavy raw material to obtain the preheated heavy raw material;
[0065] S3. After stripping, the first catalyst to be regenerated is introduced into the first regenerator for a first regeneration reaction to obtain a first regenerated catalyst and a first regenerated flue gas; part or all of the first regenerated flue gas is introduced into the second regenerator, and the first regenerated catalyst is returned to the first reactor; after stripping, the second catalyst to be regenerated is introduced into the second regenerator for a second regeneration reaction to obtain a second regenerated catalyst and a second regenerated flue gas, and the second regenerated catalyst is returned to the second reactor.
[0066] The catalytic conversion method disclosed in the present invention reacts heavy raw materials and light raw materials in different reaction regeneration systems respectively, and adopts different catalysts and reaction conditions to strengthen the primary cracking reaction of heavy raw materials and the secondary cracking reaction of light raw materials, thereby improving the yield of ethylene, propylene and light aromatics; at the same time, the regeneration flue gas generated by the first regenerator provides heat for the regeneration of the light oil catalyst to reach the temperature required for the regeneration of the light oil catalyst, and provides heat for the catalytic conversion reaction of the light raw materials. The reaction oil gas provides heat for the preheating of the heavy raw materials, which can greatly reduce the energy consumption of the device.
[0067] According to the present disclosure, the heavy raw material mainly undergoes cracking reaction in the first reactor, and is converted from macromolecular reactants into small molecular products. The heavy raw material can be selected from one or more of vacuum wax oil, atmospheric residue oil, vacuum residue oil, coker wax oil, deasphalted oil, furfural refined raffinate oil, coal liquefaction oil, oil sand oil, shale oil, distillate oil obtained by FT synthesis, or animal and vegetable oils.
[0068] The light feedstock of the present disclosure can be introduced at the same position of the second riser reactor, or at different positions, preferably at different positions. The weight ratio of the light feedstock to the heavy feedstock in the present disclosure is 0.02-0.6:1, preferably 0.04-0.3:1. The light feedstock may include at least one of C4 hydrocarbons and light gasoline fractions; the C4 hydrocarbons may be a mixture of C4 alkanes and C4 olefins; the content of C4 olefins in the C4 hydrocarbons may be greater than 50% by weight, preferably greater than 60% by weight. The C4 hydrocarbons in the present disclosure include C4 hydrocarbons produced by the catalytic converter of the present disclosure during the reaction process or C4 hydrocarbons produced by other devices, preferably C4 hydrocarbons produced by the catalytic converter of the present disclosure. The weight ratio of the C4 hydrocarbons injected into the second reactor to the heavy feedstock injected into the first reactor in the present disclosure is 0-0.30:1, preferably 0.02-0.15:1. The light gasoline fraction is a light gasoline fraction rich in olefins, and its olefin content is 20-95% by weight, preferably 50-95% by weight. The light gasoline fraction includes the light gasoline fraction produced by the catalytic converter of the present disclosure or the light gasoline fraction produced by other devices; the light gasoline fraction produced by other devices can be selected from the light gasoline fraction, the coking light gasoline fraction, the visbreaking light gasoline fraction and the mixture of one or more light gasoline fractions produced by other oil refining or chemical processes, preferably the light gasoline fraction produced by the present device. In the present disclosure, the weight ratio of the light gasoline fraction injected into the second riser reactor to the heavy feedstock injected into the first reactor is 0-0.30:1, preferably 0.02-0.15:1.
[0069] According to the present disclosure, the first reactor may include a first riser reactor and / or a first fluidized bed reactor, preferably a combination reactor of the first riser reactor and the first fluidized bed reactor. When the first reactor is a combination reactor of the first riser reactor and the first fluidized bed reactor, it can create different reaction environments for the primary cracking reaction of the heavy raw material and the secondary cracking reaction of the intermediate product, which is more conducive to the conversion of the heavy raw material and can produce more light olefins and aromatics. Among them, in the combination reactor, the first fluidized bed reactor can be located above the first riser reactor and connected to the first riser reactor.
[0070] According to the present disclosure, the reaction temperature of the first riser reactor can be 500-580°C, preferably 520-560°C; the catalyst-oil ratio can be 2-25, preferably 5-20; the reaction time can be 0.5-10 seconds, preferably 1-5 seconds; the reaction temperature of the first fluidized bed reactor can be 480-560°C, preferably 500-540°C; the weight hourly space velocity can be 1-20 hours -1 , preferably 2-8 hours -1 ; Catalyst density can be 50-350kg / m 3, preferably 100-250kg / m 3 ; The bed height of the first fluidized bed reactor can be 1 / 2-4 / 5 of the height of the first fluidized bed reactor, preferably 1 / 2-3 / 4 of the height of the first fluidized bed reactor; The pressure inside the first fluidized bed reactor can be 0.1-0.4MPa, preferably 0.15-0.3MPa.
[0071] According to the present disclosure, the second reactor may be a combined reactor of a second riser reactor and a second fluidized bed reactor. As a preferred embodiment of the present disclosure, the second fluidized bed reactor is located above the second riser reactor and is connected to the second riser reactor.
[0072] According to the present disclosure, the reaction temperature of the second riser reactor can be 630-690°C, preferably 650-670°C; the catalyst-oil ratio can be 20-80, preferably 40-60; the reaction time can be 0.5-15 seconds, preferably 1-10 seconds; the reaction temperature of the second fluidized bed reactor can be 590-650°C, preferably 610-630°C; the weight hourly space velocity can be 1-20 hours -1 , preferably 2-8 hours -1 The catalyst density in the second fluidized bed reactor can be 50-350 kg / m 3 , preferably 100-250kg / m 3 ; The bed height of the second fluidized bed reactor can be 1 / 2-4 / 5 of the height of the second fluidized bed reactor, preferably 1 / 2-3 / 4 of the height of the second fluidized bed reactor; The pressure inside the second fluidized bed reactor can be 0.1-0.4MPa, preferably 0.15-0.3MPa.
[0073] According to the present disclosure, the temperature of the preheated heavy feedstock may be 100-350°C, preferably 150-300°C.
[0074] According to the present disclosure, the first regeneration reaction may include complete regeneration or incomplete regeneration, preferably incomplete regeneration; the regeneration temperature in the first regenerator may be 620-720°C, preferably 650-680°C; the second regeneration reaction may include complete regeneration or incomplete regeneration, preferably complete regeneration; the regeneration temperature in the second regenerator may be 650-750°C, preferably 680-730°C. In the method disclosed in the present disclosure, the regeneration flue gas generated in the first regenerator is partially or completely introduced into the second regenerator to provide heat for the regeneration of the light oil catalyst, thereby realizing the coupled utilization of heat, preferably partially introduced into the second regenerator.
[0075] According to the present disclosure, the heavy oil catalyst may include the Y-type molecular sieve, the β-type molecular sieve, a first clay and a first binder; based on the total weight of the heavy oil catalyst, the content of the Y-type molecular sieve may be 20-60% by weight, preferably 30-50% by weight; the content of the β-type molecular sieve may be 1-40% by weight, preferably 1-20% by weight; the content of the first clay may be 10-70% by weight, preferably 15-45% by weight; the content of the first binder may be 10-40% by weight, preferably 20-35% by weight; the Y-type molecular sieve is selected from HY-type molecular sieve, USY-type molecular sieve, REUSY-type molecular sieve, At least one of β-type molecular sieves, REY-type molecular sieves, REHY-type molecular sieves, DASY-type molecular sieves and REDASY-type molecular sieves; the β-type molecular sieve may be a β-type molecular sieve modified by phosphorus and transition metal M, wherein M may be selected from at least one of Fe, Co, Ni, Cu, Mn, Zn and Sn; the β-type molecular sieve modified by phosphorus and transition metal M may be prepared by various methods, such as introducing phosphorus and the transition metal M during the synthesis of the β-type molecular sieve, or introducing phosphorus and the transition metal M by ammonium exchange, phosphorus modification, transition metal M modification and calcination after the synthesis of the β-type molecular sieve. The first clay may be selected from at least one of kaolin, montmorillonite and bentonite; the first binder may be selected from at least one of silica sol, alumina sol and pseudo-boehmite, preferably, the first binder may be a bi-aluminum binder of alumina sol and pseudo-boehmite.
[0076] According to the present disclosure, the light oil catalyst may include the MFI structure molecular sieve, a second clay and a second binder; based on the total weight of the light oil catalyst, the content of the MFI structure molecular sieve may be 20-60% by weight, preferably 30-50% by weight; the content of the second clay may be 10-70% by weight, preferably 15-45% by weight; the content of the second binder may be 10-40% by weight, preferably 20-35% by weight; the MFI structure molecular sieve may be selected from one or more of a ZRP molecular sieve, a phosphorus-containing ZRP molecular sieve, a rare earth-containing ZRP molecular sieve, a phosphorus- and rare earth-containing ZRP molecular sieve, a phosphorus- and alkaline earth metal-containing ZRP molecular sieve, and a phosphorus- and transition metal-containing ZRP molecular sieve, preferably a phosphorus- and rare earth-containing ZRP zeolite; the second clay may be selected from at least one of kaolin, montmorillonite, and bentonite; the second binder may be selected from at least one of silica sol, alumina sol, and pseudo-boehmite, preferably, the second binder is a dual aluminum binder of alumina sol and pseudo-boehmite.
[0077] According to the present disclosure, the method may also include: the second reaction oil and gas passing through the heavy feedstock preheater is further separated into products such as dry gas, cracked gas, gasoline, light oil and oil slurry in the product separation system, wherein the cracked gas can obtain polymerization-grade propylene products and olefin-rich C4 hydrocarbons after subsequent product separation and refining; the gasoline is first cut into light and medium gasoline fractions, and part or all of the olefin-rich C4 hydrocarbons are directly returned to the second riser reactor for reaction; part or all of the light gasoline is returned to the second riser reactor for reaction.
[0078] The second aspect of the present disclosure provides a device for a catalytic conversion method for producing ethylene, propylene and light aromatics, the catalytic conversion device comprising a first reactor, a second reactor, a first regenerator, a second regenerator and a raw material preheater, the first reactor being connected to the first regenerator through a first catalyst delivery pipeline; the second reactor being connected to the second regenerator through a second catalyst delivery pipeline; the first reactor comprising an inlet for preheated heavy raw materials, the second reactor comprising an outlet for reaction oil and gas of light raw materials, the raw material preheater comprising an inlet for reaction oil and gas before heat exchange, an outlet for reaction oil and gas after heat exchange, an inlet for heavy raw materials before preheating and an outlet for heavy raw materials after preheating; the outlet for reaction oil and gas of light raw materials is connected to the inlet for reaction oil and gas before heat exchange, and the outlet for heavy raw materials after preheating is connected to the inlet for heavy raw materials after preheating of the first reactor; the first regenerator and the second regenerator are arranged in parallel or coaxially, preferably in parallel; the first regenerator comprises a first regeneration flue gas outlet, the second regenerator comprises a first regeneration flue gas inlet, and the first regeneration flue gas outlet is connected to the first regeneration flue gas inlet.
[0079] The catalytic conversion device disclosed in the present invention may specifically include: a first riser reactor 1-1, a first fluidized bed reactor 1-3, a first regenerator 2-1, a second regenerator 3-1, a second riser reactor 4-1, a second fluidized bed reactor 4-3, and a raw material preheater 5-1. The first riser reactor 1-1 is connected to the first regenerator 2-1 through a heavy oil regenerated catalyst delivery pipeline 202, and the first stripper 1-2 is connected to the first regenerator 2-1 through a heavy oil regenerated catalyst delivery pipeline 106, which are used for catalytic conversion reaction of heavy raw materials and regeneration of heavy oil catalysts; the second riser reactor 4-1 is connected to the second regenerator 3-1 through a light oil regenerated catalyst delivery pipeline 302, and the second stripper 4-2 is connected to the second regenerator 3-1 through a light oil regenerated catalyst delivery pipeline 406, which are used for catalytic conversion reaction of light raw materials and regeneration of light oil catalysts.
[0080] Lifting gas is introduced into the first riser reactor 1-1 through the first pre-lifting gas pipeline 103. The lifting gas used is well known to those skilled in the art and can be selected from one or more of water vapor, nitrogen, and dry gas, preferably water vapor. The first stripper 1-2 at least wraps a portion of the first riser reactor 1-1 and is connected to the first regenerator 2-1 through the heavy oil catalyst delivery pipeline 106. The first fluidized bed reactor 1-3 is located above the first riser reactor 1-1 and is connected to the first riser reactor 1-1. The first settler 1-4 is connected to the first fluidized bed reactor 1-3, and the reaction oil and gas in the first fluidized bed reactor 1-3 can directly enter the first settler 1-4, enter the first gas collecting chamber 109 after separation by the first cyclone separator 107 and the second cyclone separator 108, and then lead out of the reactor through the separation system pipeline 110. The inlet of the first cyclone separator 107 and the second cyclone separator 108 are located at the upper part of the first settler 1-4. The catalyst outlet positions of the first cyclone separator 107 and the second cyclone separator 108 enable the catalyst therein to enter the first stripper 1-2. The oil and gas outlets of the first cyclone separator 107 and the second cyclone separator 108 are connected and connected to the oil and gas separation system through the first gas collecting chamber 109 and the first separation system pipeline 110. The regenerated catalyst from the first stripper 1-2 enters the first regenerator 2-1 through the heavy oil regenerated catalyst delivery pipeline 106 for charring and regeneration, thereby converting the regenerated catalyst into a regenerated catalyst. The regenerated catalyst in the first regenerator 2-1 is returned to the pre-lifting section of the first riser reactor 1-1 through the heavy oil regenerated catalyst delivery pipeline 202 for recycling, wherein the delivery speed of the catalyst can be adjusted by the valves on the heavy oil regenerated catalyst delivery pipeline 202 and the heavy oil regenerated catalyst delivery pipeline 106. The stripper 1-2 is provided with a first stripping baffle 105 and a stripping gas distribution ring, which are used to reduce the falling speed of the catalyst to be regenerated and make the stripping gas distribution more uniform, so that the residual reaction oil gas on the catalyst to be regenerated can be fully removed from the catalyst to be regenerated. The bottom of the first regenerator 2-1 is provided with a first regenerator main air inlet pipeline 201, which can introduce regeneration gas into the first regenerator 2-1. The flue gas generated after regeneration passes through the third cyclone separator 203 and the fourth cyclone separator 204 into the second gas collecting chamber 205, and then is introduced into the second regenerator 3-1 to provide heat for the regeneration of the light oil catalyst.
[0081] The lifting gas is introduced into the second riser reactor 4-1 through the second pre-lift gas pipeline 403. The lifting gas used is well known to those skilled in the art and can be selected from one or more of water vapor, nitrogen, and dry gas, preferably water vapor. The second stripper 4-2 at least wraps a portion of the second riser reactor 4-1 and is connected to the second regenerator 3-1 through the light oil catalyst delivery pipeline 406. The second fluidized bed reactor 4-3 is located above the second riser reactor 4-1 and is connected to the second riser reactor 4-1. The second settler 4-4 is connected to the second fluidized bed reactor 4-3, and the reaction oil and gas in the second fluidized bed reactor 4-3 can directly enter the second settler 4-4, enter the third gas collection chamber 409 after separation by the seventh cyclone separator 407 and the eighth cyclone separator 408, and then lead out of the reactor through the second separation system pipeline 410. The inlet of the seventh cyclone separator 407 and the eighth cyclone separator 408 are located at the upper part of the second settler 4-4. The catalyst outlet positions of the seventh cyclone separator 407 and the eighth cyclone separator 408 enable the catalyst therein to enter the second stripper 4-2. The oil and gas outlets of the seventh cyclone separator 407 and the eighth cyclone separator 408 are connected and connected to the oil and gas separation system through the third gas collecting chamber 409 and the second separation system pipeline 410. The catalyst to be regenerated from the second stripper 4-2 enters the second regenerator 3-1 through the light oil catalyst to be regenerated delivery pipeline 406 for charring and regeneration, thereby converting the catalyst to be regenerated into a regenerated catalyst. The regenerated catalyst in the second regenerator 3-1 is returned to the pre-lifting section of the second riser reactor 4-1 through the light oil regenerated catalyst pipeline 302 for recycling, wherein the delivery speed of the catalyst can be adjusted by the valves on the light oil regenerated catalyst delivery pipeline 302 and the light oil catalyst to be regenerated delivery pipeline 406. The second stripper 4-2 is provided with a second stripping baffle 405 and a stripping gas distribution ring, which are used to reduce the falling speed of the catalyst to be regenerated and make the stripping gas distribution more uniform, so that the residual reaction oil gas on the catalyst to be regenerated can be fully removed from the catalyst to be regenerated. The bottom of the second regenerator 3-1 is provided with a second regenerator main air inlet pipeline 301, which can introduce regeneration gas into the second regenerator 3-1. The flue gas generated after regeneration passes through the fifth cyclone separator 303 and the sixth cyclone separator 304 into the fourth gas collecting chamber 305, and is led out of the system after treatment.
[0082] As a preferred embodiment of the present disclosure, the method of the present disclosure may also include using a separation device to quickly separate the oil gas from the carbon deposited catalyst after the reaction, thereby reducing the dry gas yield and inhibiting the conversion of propylene after it is generated. The product separation system used in the present disclosure may be various separation systems in the prior art.
[0083] According to this disclosure, Figure 1As shown, the first reactor 1 is connected to the first regenerator 2 through the heavy oil regenerated catalyst delivery pipeline 106 and the heavy oil regenerated catalyst delivery pipeline 202, and is used for the catalytic conversion reaction of heavy raw materials and the regeneration of heavy oil catalysts; the second reactor 4 is connected to the second regenerator 3 through the light oil regenerated catalyst delivery pipeline 302 and the light oil regenerated catalyst delivery pipeline 406, and is used for the catalytic conversion reaction of light raw materials and the regeneration of light oil catalysts.
[0084] As a specific implementation of the present disclosure, Figure 2 As shown, the first reactor 1 is a first riser reactor 1-1, the first regenerator 2-1 and the second regenerator 3-1 are arranged in parallel, the second regenerator 3-1 is connected to the first regenerator 2-1 through a regeneration flue gas conveying pipeline, the regeneration reaction carried out in the first regenerator 2-1 is an incomplete regeneration, and part of the regeneration flue gas generated enters the second regenerator 3-1.
[0085] As another specific embodiment of the present disclosure, Figure 3 As shown, the first regenerator 2-1 and the second regenerator 3-1 are coaxially arranged. The second regenerator 3-1 is located at the upper part of the first regenerator 2-1 and is connected to the first regenerator 2-1 through a regeneration flue gas conveying pipeline. The regeneration reaction carried out in the first regenerator 2-1 is incomplete regeneration, and part of the regeneration flue gas generated enters the second regenerator 3-1.
[0086] As a preferred embodiment of the present disclosure, Figure 4 As shown, the first reactor 1 is a combination reactor of a first riser reactor 1-1 and a first fluidized bed reactor 1-3, the first regenerator 2-1 and the second regenerator 3-1 are arranged in parallel, the second regenerator 3-1 is connected to the first regenerator 2-1 through a regeneration flue gas conveying pipeline, the regeneration reaction in the first regenerator 2-1 is an incomplete regeneration, and part of the regeneration flue gas generated enters the second regenerator 3-1. This embodiment can effectively improve the catalytic cracking efficiency of heavy raw materials by setting the first reactor 1 as a combination reactor of the first riser reactor 1-1 and the first fluidized bed reactor 1-3, and can effectively achieve heat coupling utilization by arranging the first regenerator 2-1 and the second regenerator 3-1 in parallel.
[0087] As another specific embodiment of the present disclosure, Figure 5 As shown, the first reactor 1 is a combined reactor of a first riser reactor 1-1 and a first fluidized bed reactor 1-3, the first regenerator 2-1 and the second regenerator 3-1 are coaxially arranged, the second regenerator 3-1 is located at the upper part of the first regenerator 2-1, and is connected to the first regenerator 2-1 through a regeneration flue gas conveying pipeline, the regeneration reaction carried out in the first regenerator 2-1 is incomplete regeneration, and part of the regeneration flue gas generated enters the second regenerator 3-1.
[0088] The present disclosure is further described in detail by examples below. The raw materials used in the examples can be obtained through commercial channels. Among them, in the examples and comparative examples of the present disclosure, the gas product is tested by the petrochemical analysis method RIPP 77-90 method, the coke content is determined by the petrochemical analysis method RIPP 107-90 method, the composition of the organic liquid product is determined by the SH / T 0558-1993 method, the fraction cut points of gasoline and diesel are 221°C and 331°C respectively, and the light aromatics in gasoline are determined by the petrochemical analysis method RIPP 82-90.
[0089] In the following examples, the conversion rate of the feedstock oil and the yield of the cracked product are calculated according to the following formula:
[0090]
[0091]
[0092] The RIPP petrochemical analysis method used in the present invention is selected from "Petrochemical Analysis Methods (RIPP Test Methods)", edited by Yang Cuiding et al., Science Press, 1990.
[0093] Unless otherwise specified, all reagents used below are chemically pure.
[0094] The Y-type molecular sieves used are all produced by Qilu Catalyst Factory, and their industrial grades are:
[0095] DASY, the physical property parameters are: unit cell constant is 2.443nm, Na2O content is 0.85 wt%;
[0096] The β molecular sieve used was produced by Qilu Catalyst Factory, SiO2 / Al2O3=25;
[0097] The MFI structure molecular sieves used are all produced by Qilu Catalyst Factory, and their industrial grades are:
[0098] ZRP-1: wherein SiO2 / Al2O3=30, the content of Na2O is 0.17 wt%, the content of rare earth oxide RE2O3 is 1.4 wt%, the content of lanthanum oxide is 0.84 wt%, the content of cerium oxide is 0.18 wt%, and the content of other rare earth oxides is 0.38 wt%.
[0099] The specific properties of the feedstock oil used in the examples and comparative examples are shown in Table 1.
[0100] The catalysts used in the examples and comparative examples are homemade catalysts, and their compositions and properties are shown in Table 2.
[0101] Table 1
[0102]
[0103]
[0104] Table 2
[0105] project CAT-1 CAT-2 CAT-3 Molecular sieve type USY+β ZRP-1 USY+β+ZRP-1 Element composition, %(w) <![CDATA[Al2O3]]> 54.6 50.9 52.8 <![CDATA[SiO2]]> 40.9 43.7 42.6 Micro-reaction, %(W) 69 63 67 <![CDATA[Specific surface area, m 2 / g]]> 151 169 158 Pore volume, ml / g 0.459 0.524 0.496 Bulk ratio, g / ml 0.89 0.91 0.9 Particle size distribution 0-20μm 0.4 0.3 0.4 0-40μm 15.8 16.2 15.9 0-80μm 65.2 68.4 68.7 0-105μm 88.7 86.3 89.2 >105μm 11.3 13.7 10.8
[0106] Example 1
[0107] Test in Figure 2 The test was carried out on the medium-sized test device shown in the figure. The device includes two riser reactors, a fluidized bed reactor and two regenerators. The inner diameter of the first riser reactor 1-1 is 20mm and the height is 4000mm, the inner diameter of the second riser reactor 4-1 is 16mm and the height is 3000mm, and the inner diameter of the second fluidized bed reactor 4-3 is 80mm and the height is 500mm. The inner diameter of the first regenerator 2-1 is 150mm and the height is 800mm, and the inner diameter of the second regenerator 3-1 is 100mm and the height is 600mm. The first regenerator 2-1 and the second regenerator 3-1 are arranged in parallel.
[0108] The preheated feedstock oil is introduced into the bottom of the first riser reactor 1-1, contacts with the catalyst CAT-1 and undergoes the first catalytic cracking reaction, and the obtained oil-agent mixture is separated by a cyclone separator to obtain the first reaction oil gas and the first regenerated catalyst. The first regenerated catalyst enters the first stripper 1-2 and then enters the first regenerator 2-1 for regeneration to obtain the first regenerated catalyst and the first regenerated flue gas. The first regenerated catalyst returns to the first riser reactor 1-1 for recycling, and the first regenerated flue gas is introduced into the second regenerator. The first reaction oil gas is introduced into the fractionation system for separation.
[0109] C4 hydrocarbons are introduced into the bottom of the second riser reactor 4-1, contacted with the catalyst CAT-2 and a second catalytic cracking reaction occurs. The resulting oil mixture is introduced into the fluidized bed reactor 4-3. The reacted oil mixture is separated by a cyclone separator to obtain a second reaction oil gas and a second catalyst to be regenerated. The second catalyst to be regenerated enters the second stripper 4-2 and then enters the second regenerator 3-1 for regeneration. The regenerated second regenerated catalyst returns to the second riser reactor 4-1 for recycling, and the second reaction oil gas is introduced into the fractionation system for separation. The mass ratio of C4 hydrocarbons to feedstock oil in this embodiment is 0.4:1. The reaction conditions and results are shown in Table 3.
[0110] Example 2
[0111] Test in Figure 3The test was carried out on the medium-sized test device shown in the figure. The device includes two riser reactors, a fluidized bed reactor and two regenerators. The inner diameter of the first riser reactor 1-1 is 20mm and the height is 4000mm, the inner diameter of the second riser reactor 4-1 is 16mm and the height is 3000mm, and the inner diameter of the fluidized bed reactor 4-3 is 80mm and the height is 500mm. The inner diameter of the first regenerator 2-1 is 150mm and the height is 800mm, and the inner diameter of the second regenerator 3-1 is 100mm and the height is 600mm. The first regenerator 2-1 is coaxially arranged with the second regenerator 3-1, and the second regenerator 3-1 is located on the upper part of the first regenerator 2-1.
[0112] The preheated feedstock oil is introduced into the bottom of the first riser reactor 1-1, contacts with the catalyst CAT-1 and undergoes the first catalytic cracking reaction, and the obtained oil-agent mixture is separated by a cyclone separator to obtain the first reaction oil gas and the first regenerated catalyst. The first regenerated catalyst enters the first stripper 1-2 and then enters the first regenerator 2-1 for regeneration to obtain the first regenerated catalyst and the first regenerated flue gas. The first regenerated catalyst returns to the first riser reactor 1-1 for recycling, and the first regenerated flue gas is introduced into the second regenerator. The first reaction oil gas is introduced into the fractionation system for separation.
[0113] C4 hydrocarbons are introduced into the bottom of the second riser reactor 4-1, contacted with the catalyst CAT-2 and reacted, and the resulting oil-agent mixture is introduced into the fluidized bed reactor 4-3. The reacted oil-agent mixture is separated by a cyclone separator to obtain the second reaction oil gas and the second regenerated catalyst. The second regenerated catalyst enters the second stripper 4-2 and then enters the second regenerator 3-1 for regeneration. The regenerated second regenerated catalyst returns to the second riser reactor 4-1 for recycling, and the second reaction oil gas is introduced into the fractionation system for separation. The mass ratio of C4 hydrocarbons to feedstock oil is 0.4:1. The reaction conditions and results are shown in Table 3.
[0114] Example 3
[0115] Test in Figure 4 The experiment was carried out on the medium-sized test device shown in the figure. The device includes two riser reactors, two fluidized bed reactors and two regenerators. The inner diameter of the first riser reactor 1-1 is 20mm and the height is 4000mm, and the inner diameter of the second riser reactor 4-1 is 16mm and the height is 3000mm. The inner diameter of the first fluidized bed reactor 1-3 is 90mm and the height is 600mm, and the inner diameter of the second fluidized bed reactor 4-3 is 80mm and the height is 500mm. The inner diameter of the first regenerator 2-1 is 150mm and the height is 800mm, and the inner diameter of the second regenerator 3-1 is 100mm and the height is 600mm. The first regenerator 2-1 and the second regenerator 3-1 are arranged in parallel.
[0116] The preheated feedstock oil is introduced into the bottom of the first riser reactor 1-1, contacts with the catalyst CAT-1 and undergoes the first catalytic cracking reaction, and the obtained oil-agent mixture is separated by a cyclone separator to obtain the first reaction oil gas and the first regenerated catalyst. The first regenerated catalyst enters the first stripper 1-2 and then enters the first regenerator 2-1 for regeneration to obtain the first regenerated catalyst and the first regenerated flue gas. The first regenerated catalyst returns to the first riser reactor 1-1 for recycling, and the first regenerated flue gas is introduced into the second regenerator. The first reaction oil gas is introduced into the fractionation system for separation.
[0117] C4 hydrocarbons are introduced into the bottom of the second riser reactor 4-1, and the light gasoline fraction (distillation range 40-80°C, olefin content 65% by weight) is introduced into the middle of the second riser reactor 4-1, contacted with the catalyst CAT-2 and reacted, and the resulting oil mixture is introduced into the fluidized bed reactor 4-3. The reacted oil mixture is separated by a cyclone separator to obtain the second reaction oil gas and the second regenerated catalyst; the second regenerated catalyst enters the second stripper 4-2 and then enters the second regenerator 3-1 for regeneration, and the regenerated second regenerated catalyst returns to the second riser reactor 4-1 for recycling, and the second reaction oil gas is introduced into the fractionation system for separation. The mass ratio of C4 hydrocarbons, light gasoline fractions and feedstock oil is 0.2:0.2:1. The reaction conditions and results are shown in Table 3.
[0118] Example 4
[0119] Test in Figure 5 The test was carried out on the medium-sized test device shown in the figure. The device includes two riser reactors, two fluidized bed reactors and two regenerators. The inner diameter of the first riser reactor 1-1 is 20mm and the height is 4000mm, and the inner diameter of the second riser reactor 4-1 is 16mm and the height is 3000mm. The inner diameter of the first fluidized bed reactor 1-3 is 90mm and the height is 600mm, and the inner diameter of the second fluidized bed reactor 4-3 is 80mm and the height is 500mm. The inner diameter of the first regenerator 2-1 is 150mm and the height is 800mm, and the inner diameter of the second regenerator 3-1 is 100mm and the height is 600mm. The first regenerator 2-1 is coaxially arranged with the second regenerator 3-1, and the second regenerator 3-1 is located on the upper part of the first regenerator 2-1.
[0120] The preheated feedstock oil is introduced into the bottom of the first riser reactor 1-1, contacts with the catalyst CAT-1 and undergoes the first catalytic cracking reaction, and the obtained oil-agent mixture is separated by a cyclone separator to obtain the first reaction oil gas and the first regenerated catalyst. The first regenerated catalyst enters the first stripper 1-2 and then enters the first regenerator 2-1 for regeneration to obtain the first regenerated catalyst and the first regenerated flue gas. The first regenerated catalyst returns to the first riser reactor 1-1 for recycling, and the first regenerated flue gas is introduced into the second regenerator. The first reaction oil gas is introduced into the fractionation system for separation.
[0121] C4 hydrocarbons are introduced into the bottom of the second riser reactor 4-1, and the light gasoline fraction (distillation range 40-80°C, olefin content 65% by weight) is introduced into the middle of the second riser reactor 4-1, contacted with the catalyst CAT-2 and reacted, and the resulting oil mixture is introduced into the fluidized bed reactor 4-3. The reacted oil mixture is separated by a cyclone separator to obtain the second reaction oil gas and the second regenerated catalyst; the second regenerated catalyst enters the second stripper 4-2 and then enters the second regenerator 3-1 for regeneration, and the regenerated second regenerated catalyst returns to the second riser reactor 4-1 for recycling, and the second reaction oil gas is introduced into the fractionation system for separation. The mass ratio of C4 hydrocarbons, light gasoline fractions and feedstock oil is 0.2:0.2:1. The reaction conditions and results are shown in Table 3.
[0122] Table 3
[0123]
[0124]
[0125] Comparative Example 1
[0126] The test was conducted on a medium-sized test device, which included a riser reactor with an inner diameter of 16 mm and a length of 3200 mm and a fluidized bed reactor with an inner diameter of 64 mm and a height of 500 mm.
[0127] The crude oil is introduced into the bottom of the riser reactor, where it contacts and reacts with the catalyst CAT-3. The resulting oil-agent mixture is introduced into the fluidized bed reactor. The reacted oil-agent mixture is separated by a quick separation device to obtain reaction oil gas and regenerated catalyst. The reaction oil gas is introduced into a cyclone separator, and the regenerated catalyst is introduced into a stripper for stripping.
[0128] The regenerated catalyst enters the stripper and then the regenerator for regeneration. The regenerated catalyst returns to the riser reactor for recycling, and the oil and gas are introduced into the fractionation system for separation. The reaction conditions and results are shown in Table 4.
[0129] Comparative Example 2
[0130] The test was conducted on a medium-sized test device. The device includes two riser reactors and a fluidized bed reactor. The first riser reactor has an inner diameter of 16 mm and a length of 3200 mm, the second riser reactor has an inner diameter of 16 mm and a height of 3000 mm, and the fluidized bed reactor has an inner diameter of 64 mm and a height of 500 mm.
[0131] The crude oil is introduced into the bottom of the first riser reactor, where it contacts and reacts with the catalyst CAT-3, and the oil-agent mixture after the reaction is separated by a cyclone separator;
[0132] C4 hydrocarbons are introduced into the bottom of the second riser reactor, contacted with the catalyst CAT-3 and reacted, and the resulting oil-agent mixture is introduced into the fluidized bed reactor. The reacted oil-agent mixture is separated by a quick separation device to obtain reaction oil gas and regenerated catalyst. The reaction oil gas is introduced into a cyclone separator, and the regenerated catalyst is introduced into a stripper for stripping.
[0133] After entering the stripper, the catalyst enters the regenerator for regeneration. The regenerated catalyst returns to the riser reactor for recycling, and the oil and gas are introduced into the fractionation system for separation. The mass ratio of C4 hydrocarbons to feedstock oil is 0.1:1. The reaction conditions and results are shown in Table 4.
[0134] Comparative Example 3
[0135] The test was conducted on a medium-sized test device. The device includes two riser reactors and a fluidized bed reactor. The first riser reactor has an inner diameter of 16 mm and a length of 3200 mm, the second riser reactor has an inner diameter of 16 mm and a height of 3000 mm, and the fluidized bed reactor has an inner diameter of 64 mm and a height of 500 mm.
[0136] The crude oil is introduced into the bottom of the first riser reactor, where it contacts and reacts with the catalyst CAT-3. The resulting oil-agent mixture is introduced into the fluidized bed reactor. The reacted oil-agent mixture is separated by a quick separation device to obtain reaction oil gas and regenerated catalyst. The reaction oil gas is introduced into a cyclone separator, and the regenerated catalyst is introduced into a stripper for stripping.
[0137] C4 hydrocarbons are introduced into the bottom of the second riser reactor, contacted with the catalyst CAT-3 and reacted, and the resulting oil-agent mixture is introduced into the fluidized bed reactor. The reacted oil-agent mixture is separated by a quick separation device to obtain reaction oil gas and regenerated catalyst. The reaction oil gas is introduced into a cyclone separator, and the regenerated catalyst is introduced into a stripper for stripping.
[0138] After entering the stripper, the catalyst enters the regenerator for regeneration. The regenerated catalyst returns to the riser reactor for recycling, and the oil and gas are introduced into the fractionation system for separation. The mass ratio of C4 hydrocarbons to feedstock oil is 0.1:1. The reaction conditions and results are shown in Table 4.
[0139] Comparative Example 4
[0140] The method of Comparative Example 3 was followed, except that the C4 hydrocarbons obtained by fractionation were not introduced into the second riser reactor, and the light gasoline fraction obtained by fractionation (distillation range 40-80°C, olefin content 65 wt%) was introduced into the fluidized bed reactor 4-1, wherein the mass ratio of light gasoline to crude oil was 0.1:1. The reaction conditions and results are shown in Table 4.
[0141] Table 4
[0142]
[0143]
[0144] It can be seen from Tables 3 and 4 that, compared with the comparative example, the method and device provided by the present invention can increase the processing volume of light raw materials, realize separate partition control of different reaction regeneration systems, and coupled utilization of heat inside the device, thereby obtaining higher yields of ethylene, propylene and light aromatics.
[0145] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0146] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0147] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A catalytic conversion method for producing ethylene, propylene and light aromatics, characterized in that: The method includes: S1, feeding the preheated heavy raw material into the first reactor, contacting it with the heavy oil catalyst containing Y-type molecular sieve and β-type molecular sieve, and performing the first catalytic cracking reaction to obtain the first reaction oil gas and the first spent catalyst; S2, feeding the light raw material into the second reactor, contacting it with the light oil catalyst containing the MFI structure molecular sieve, and performing a second catalytic cracking reaction to obtain a second reaction oil gas and a second catalyst to be produced; introducing the second reaction oil gas into the raw material preheater, exchanging heat with the heavy raw material to obtain the preheated heavy raw material; S3, introducing the first catalyst to be regenerated into the first regenerator after stripping to carry out a first regeneration reaction, so as to obtain a first regenerated catalyst and a first regenerated flue gas; introducing part or all of the first regenerated flue gas into the second regenerator, and returning the first regenerated catalyst to the first reactor; introducing the second catalyst to be regenerated into the second regenerator after stripping to carry out a second regeneration reaction, so as to obtain a second regenerated catalyst and a second regenerated flue gas, and returning the second regenerated catalyst to the second reactor; The light feedstock includes at least one of C4 hydrocarbons and light gasoline fractions; The C4 hydrocarbon is a mixture of C4 alkanes and C4 olefins; the content of C4 olefins in the C4 hydrocarbon is greater than 50% by weight; The light gasoline fraction is a light gasoline fraction rich in olefins, and the olefin content in the light gasoline fraction is 20-95% by weight; The second reactor is a combined reactor of a second riser reactor and a second fluidized bed reactor, the second fluidized bed reactor is located above the second riser reactor and is connected to the second riser reactor; the reaction temperature of the second riser reactor is 630-690° C.; the catalyst-oil ratio is 20-80; and the reaction time is 0.5-15 seconds; The heavy oil catalyst comprises a molecular sieve, a first clay and a first binder; the molecular sieves in the heavy oil catalyst are Y-type molecular sieve and β-type molecular sieve; based on the total weight of the heavy oil catalyst, the content of the Y-type molecular sieve is 20-60% by weight; the content of the β-type molecular sieve is 1-40% by weight; the content of the first clay is 10-70% by weight; the content of the first binder is 10-40% by weight; the total weight of the components of the heavy oil catalyst is 100% by weight; The Y-type molecular sieve is at least one selected from HY-type molecular sieve, USY-type molecular sieve, REUSY-type molecular sieve, REY-type molecular sieve, REHY-type molecular sieve, DASY-type molecular sieve and REDASY-type molecular sieve; the β-type molecular sieve is a β-type molecular sieve modified by phosphorus and transition metal M, wherein M is selected from at least one of Fe, Co, Ni, Cu, Mn, Zn and Sn; the first clay is selected from at least one of kaolin, montmorillonite and bentonite; the first binder is selected from at least one of silica sol, alumina sol and pseudo-boehmite; The light oil catalyst comprises a molecular sieve, a second clay and a second binder; the molecular sieve in the light oil catalyst is an MFI structure molecular sieve; based on the total weight of the light oil catalyst, the content of the MFI structure molecular sieve is 20-60% by weight; the content of the second clay is 10-70% by weight; the content of the second binder is 10-40% by weight; the total weight of the components of the light oil catalyst is 100% by weight; The MFI structured molecular sieve is selected from ZRP molecular sieve; the second clay is selected from at least one of kaolin, montmorillonite and bentonite; the second binder is selected from at least one of silica sol, alumina sol and pseudo-boehmite.
2. The catalytic conversion method according to claim 1, wherein: The heavy raw material is selected from one or a mixture of vacuum wax oil, atmospheric residue oil, vacuum residue oil, coker wax oil, deasphalted oil, furfural refined raffinate oil, coal liquefaction oil, oil sand oil, shale oil, distillate oil obtained by FT synthesis and animal and vegetable oils; The content of C4 olefins in the C4 hydrocarbons is greater than 60% by weight; the content of olefins in the light gasoline fraction is 50-95% by weight; the weight ratio of the light raw material to the heavy raw material is 0.02-0.6:1; The weight ratio of the C4 hydrocarbon to the heavy raw material is 0-0.30:1; the weight ratio of the light gasoline fraction to the heavy raw material is 0-0.30:
1.
3. The catalytic conversion method according to claim 2, wherein: The weight ratio of the light raw material to the heavy raw material is 0.04-0.3:1; The weight ratio of the C4 hydrocarbon to the heavy raw material is 0.02-0.15:1; the weight ratio of the light gasoline fraction to the heavy raw material is 0.02-0.15:
1.
4. The catalytic conversion method according to claim 1, wherein: The first reactor includes a first riser reactor and / or a first fluidized bed reactor; in the combined reactor, the first fluidized bed reactor is located above the first riser reactor and is connected to the first riser reactor.
5. The catalytic conversion method according to claim 1, wherein: The first reactor is a combined reactor of a first riser reactor and a first fluidized bed reactor.
6. The catalytic conversion method according to claim 4 or 5, wherein: The reaction temperature of the first riser reactor is 500-580°C; the catalyst-oil ratio is 2-25; and the reaction time is 0.5-10 seconds; The reaction temperature of the first fluidized bed reactor is 480-560°C; the weight hourly space velocity is 1-20 hours -1 ; Catalyst density is 50-350kg / m 3 ; The bed height of the first fluidized bed reactor is 1 / 2-4 / 5 of the height of the first fluidized bed reactor; The pressure inside the first fluidized bed reactor is 0.1-0.4 MPa.
7. The catalytic conversion method according to claim 6, wherein: The reaction temperature of the first riser reactor is 520-560°C; the catalyst-oil ratio is 5-20; and the reaction time is 1-5 seconds; The reaction temperature of the first fluidized bed reactor is 500-540°C; the weight hourly space velocity is 2-8 hours -1 ; Catalyst density is 100-250kg / m 3 ; The bed height of the first fluidized bed reactor is 1 / 2-3 / 4 of the height of the first fluidized bed reactor; The pressure inside the first fluidized bed reactor is 0.15-0.3MPa.
8. The catalytic conversion method according to claim 1, wherein: The reaction temperature of the second riser reactor is 650-670°C; the catalyst-oil ratio is 40-60; and the reaction time is 1-10 seconds; The reaction temperature of the second fluidized bed reactor is 590-650°C; the weight hourly space velocity is 1-20 hours -1 The catalyst density in the second fluidized bed reactor is 50-350 kg / m 3 ; The bed height of the second fluidized bed reactor is 1 / 2-4 / 5 of the height of the second fluidized bed reactor; The pressure inside the second fluidized bed reactor is 0.1-0.4MPa.
9. The catalytic conversion method according to claim 8, wherein: The reaction temperature of the second fluidized bed reactor is 610-630°C; the weight hourly space velocity is 2-8 hours -1 The catalyst density in the second fluidized bed reactor is 100-250kg / m 3 ; The bed height of the second fluidized bed reactor is 1 / 2-3 / 4 of the height of the second fluidized bed reactor; The pressure inside the second fluidized bed reactor is 0.15-0.3MPa.
10. The catalytic conversion method according to claim 1, wherein: The temperature of the preheated heavy raw material is 100-350°C.
11. The catalytic conversion method according to claim 10, wherein: The temperature of the preheated heavy raw material is 150-300°C.
12. The catalytic conversion method according to claim 1, wherein: The first regeneration reaction includes complete regeneration or incomplete regeneration; the regeneration temperature in the first regenerator is 620-720°C; The second regeneration reaction includes complete regeneration or incomplete regeneration; the regeneration temperature in the second regenerator is 650-750°C.
13. The catalytic conversion method according to claim 12, wherein: The first regeneration reaction is an incomplete regeneration; the regeneration temperature in the first regenerator is 650-680°C; The second regeneration reaction is complete regeneration; the regeneration temperature in the second regenerator is 680-730°C.
14. The catalytic conversion method according to claim 1, wherein: Based on the total weight of the heavy oil catalyst, the content of the Y-type molecular sieve is 20-60% by weight; the content of the β-type molecular sieve is 1-20% by weight; the content of the first clay is 15-45% by weight; the content of the first binder is 20-35% by weight; The first binder is a dual aluminum binder of aluminum sol and pseudo-boehmite.
15. The catalytic conversion method according to claim 1, wherein: Based on the total weight of the light oil catalyst, the content of the MFI structured molecular sieve is 30-50% by weight; the content of the second clay is 15-45% by weight; the content of the second binder is 20-35% by weight; The second binder is a dual aluminum binder of aluminum sol and pseudo-boehmite.
16. The catalytic conversion method according to claim 1, wherein: The method further comprises: separating the second reaction oil gas after heat exchange to obtain C4 hydrocarbons containing olefins and light gasoline fraction segments, and returning part or all of the C4 hydrocarbons containing olefins and the light gasoline fraction segments to the second reactor.