A SBS modified asphalt waterproofing membrane and its preparation method and application

By mixing naphthenic oil with SBS modifier under low temperature conditions and contacting it with asphalt and other materials, a low-temperature molded SBS modified asphalt waterproofing membrane is formed, which solves the problems of toxic smoke release and water resource consumption caused by high-temperature processes. High-performance and environmentally friendly waterproof membrane preparation is achieved.

CN115726199BActive Publication Date: 2024-10-01WEINAN KESHUN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211584683.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-01
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The existing SBS modified asphalt waterproofing membrane requires high temperatures during the preparation process, which results in the release of toxic smoke, and the cooling process consumes a large amount of water, affecting environmental protection and energy efficiency. At the same time, reducing the amount of modifier will lead to unqualified heat resistance.

Method used

By mixing naphthenic oil and SBS modifier into gel-like swollen SBS, and contacting it with asphalt, anti-aging agent, petroleum resin and filler at 120-160℃, a low-temperature formed waterproofing membrane is formed, reducing the process temperature and cooling water usage.

Benefits of technology

It achieves safe and environmentally friendly low-temperature molding of SBS modified asphalt waterproofing membranes while ensuring heat resistance and joint peeling strength. It reduces smoke and odor emissions, saves the use of cooling water, and improves the environmental protection and environmental protection of the process. efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003991795960000091
    Figure BDA0003991795960000091
  • Figure BDA0003991795960000101
    Figure BDA0003991795960000101
  • Figure BDA0003991795960000102
    Figure BDA0003991795960000102
Patent Text Reader

Abstract

The present invention relates to the technical field of waterproofing rolls, and discloses an SBS modified asphalt waterproofing roll, a preparation method thereof, and an application thereof. The method comprises: (1) mixing cyclohexane oil and an SBS modifier to obtain a swollen SBS in a gel state at 25°C; (2) first contacting the swollen SBS with asphalt to obtain a mixture I; (3) second contacting the mixture I with an anti-aging agent, a petroleum resin, a BL modifier, and a filler to obtain a coating; (4) coating the coating on a tire base cloth to obtain the waterproofing roll; the temperatures of the first contact and the second contact are independently 120-160°C. The method provided by the present invention can safely and environmentally prepare a low-temperature formed SBS modified asphalt waterproofing roll under the premise of ensuring the heat resistance and seam peeling strength of the asphalt waterproofing roll.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to an SBS modified asphalt waterproof coiled material and a preparation method and application thereof. Background Art

[0002] Waterproof materials are important materials in building waterproofing, among which SBS modified asphalt waterproofing membranes account for half of the waterproofing materials. However, in the preparation process of conventional SBS modified asphalt waterproofing membranes on the market today, a large amount of complex modifiers must be added, resulting in the swelling process temperature often needing to be higher than 190°C, or even up to 220°C. On the other hand, a large amount of asphalt is required in SBS modified asphalt waterproofing membranes, and asphalt will produce toxic smoke at such high temperatures, threatening the atmospheric environment and the health of workers.

[0003] In addition, the cooling process of the product will consume a lot of water resources. Moreover, reducing the amount of modifier will cause the product's heat resistance to be seriously unqualified.

[0004] CN113528083A discloses a low-temperature formed hot-melt coiled material, which can reduce the viscosity of SBS modified asphalt glue, control the production temperature between 145-155°C, reduce the release of toxic fumes during production, and make SBS modified asphalt glue more environmentally friendly and energy-saving during production. However, in step one of the scheme: add asphalt and plasticizer to the reactor, heat it to 185-195°C at a stirring speed of 760-840r / min to obtain mixture A; and in step two: add SBS modifier and high-temperature modifier to mixture A and heat it to 185-195°C, stir it at a stirring speed of 660-740r / min for 1.5-3h to obtain mixture B. In both steps, the mixture containing asphalt needs to be heated to a high temperature of 185-195°C, and 195°C is used in the embodiment, so the scheme does not completely solve the problem of asphalt generating toxic fumes at high temperatures.

[0005] CN110016291A discloses a new type of high temperature resistant non-curing waterproof coating, which can be applied by heating to 130°C, greatly reducing the harm to personnel and the environment. This method only achieves that the temperature during the construction process is 130°C, and does not solve the problem of toxic fumes generated by asphalt at high temperatures during the coating production process.

[0006] Therefore, it is of great significance to solve the problem of SBS modified asphalt waterproof membrane molding under low temperature conditions through a safe and environmentally friendly method, while ensuring the heat resistance and joint peeling strength of the asphalt waterproof membrane. Summary of the invention

[0007] The purpose of the present invention is to overcome the problem in the prior art that it is not possible to safely and environmentally prepare SBS modified asphalt waterproofing membrane that can be formed at low temperature while ensuring the heat resistance and joint peeling strength of the asphalt waterproofing membrane.

[0008] In order to achieve the above object, the present invention provides a method for preparing an SBS modified asphalt waterproofing membrane, the method comprising:

[0009] (1) mixing cyclohexane oil and SBS modifier to obtain a swollen SBS in a gel state at 25° C.

[0010] (2) contacting the swollen SBS with asphalt to obtain a mixture I;

[0011] (3) contacting the mixture I with an anti-aging agent, a petroleum resin, a BL modifier and a filler for a second time to obtain a coating;

[0012] (4) applying the coating on the base fabric to obtain the waterproof coiled material;

[0013] The temperatures of the first contacting and the second contacting are each independently 120-160°C.

[0014] The second aspect of the present invention provides a low-temperature moldable SBS modified asphalt waterproofing membrane prepared by the method described in the first aspect.

[0015] The third aspect of the present invention provides the use of the low-temperature moldable SBS modified asphalt waterproof membrane described in the second aspect in building waterproofing.

[0016] Compared with the prior art, the method provided by the present invention has at least the following advantages:

[0017] (1) The method provided by the present invention can solve the problem of too high process temperature of SBS modified asphalt waterproofing membrane;

[0018] (2) The SBS modified asphalt waterproofing membrane prepared by the method provided by the present invention has excellent properties, good heat resistance, high joint peeling strength, easy oil discharge during hot melt construction, good adhesion, short batching time during the molding process, saving cooling water, and low smoke and odor emissions. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0020] It should be noted that, in various aspects of the present invention, for the same components or terms in various aspects, the present invention is described only once in one aspect without repeated description, which should not be understood by those skilled in the art as a limitation of the present invention.

[0021] As mentioned above, the first aspect of the present invention provides a method for preparing an SBS modified asphalt waterproofing membrane, the method comprising:

[0022] (1) mixing cyclohexane oil and SBS modifier to obtain a swollen SBS in a gel state at 25° C.

[0023] (2) contacting the swollen SBS with asphalt to obtain a mixture I;

[0024] (3) contacting the mixture I with an anti-aging agent, a petroleum resin, a BL modifier and a filler for a second time to obtain a coating;

[0025] (4) applying the coating on the base fabric to obtain the waterproof coiled material;

[0026] The temperatures of the first contacting and the second contacting are each independently 120-160°C.

[0027] According to a preferred embodiment, in step (1), the mixing temperature is 140-230°C.

[0028] Preferably, the cycloparaffinic oil has a kinematic viscosity of 5-20 mPa·s at 100°C.

[0029] Preferably, the melt index of the SBS modifier is 0.2-1.5 g / 10 min.

[0030] Preferably, in step (1), the mixing conditions at least meet the following requirements: mixing is carried out under stirring conditions, with a rotation speed of 800-1400 r / min, a mixing temperature of 160-220° C., and a mixing time of 2.5-4.0 h.

[0031] According to a preferred embodiment, in step (1), the specific operation of mixing includes: heating the cyclohexane oil to the mixing temperature of 140-230° C. for mixing I under a stirring condition of a rotation speed of 800-1200 r / min, and a heating rate of 5-8° C. / min, and then adding the SBS modifier for mixing II under a heat preservation condition for a time of 0.5-2 h, and cooling to room temperature to obtain the swollen SBS, wherein the rotation speed of the mixing II is 1200-1400 r / min.

[0032] It should be noted that, in the present invention, the mixing I and / or the mixing II can be performed using a high-speed shearing instrument.

[0033] It should be noted that, in the present invention, the normal temperature or the room temperature is 25±3°C.

[0034] According to a preferred embodiment, in step (2), the asphalt is selected from at least one of 200# asphalt, 90# asphalt, and 70# asphalt.

[0035] Preferably, the conditions for the first contact at least meet the following requirements: the first contact is carried out under stirring, with a rotation speed of 800-1200 r / min, a temperature of 130-150° C., and a time of 0.5-2 h.

[0036] According to a preferred embodiment, in step (2), the operation of the first contact specifically includes: under the stirring condition of a rotation speed of 800-1200r / min, first heating the asphalt to a first contact temperature of 130-150°C, with a heating rate of 5-8°C / min, and then adding the swollen SBS under insulation conditions to perform the first contact to obtain the mixture I, wherein the time of the first contact is 0.5-2h.

[0037] Preferably, in step (3), the anti-aging agent is selected from at least one of antioxidant 1010 and anti-aging agent 3050.

[0038] Preferably, the petroleum resin is selected from at least one of terpene resin, C5 petroleum resin and C9 petroleum resin.

[0039] According to a preferred embodiment, the BL modifier is selected from at least one of polyethylene wax AC316A, polyethylene wax LD-808T, and polyethylene wax TL-500C. The inventors found that under this preferred embodiment, the method of the present invention can provide a guarantee for the heat-oxidative aging resistance of the SBS waterproof membrane prepared at 140°C.

[0040] Preferably, the filler is selected from at least one of nano calcium carbonate, organic bentonite and organic diatomaceous earth.

[0041] Preferably, in step (3), the second contacting condition at least satisfies the following conditions: it is carried out under stirring, at a rotation speed of 800-1200 r / min, at a temperature of 130-150° C., and for a time of 0.1-2 h.

[0042] According to a preferred embodiment, in step (3), the second contacting operation specifically includes: adding petroleum resin, anti-aging agent and BL modifier into the reactor at a rotation speed of 800-1200 r / min and a temperature of 130-150°C for a first stirring for 0.5-1h, and then adding filler for a second stirring for 0.5-1h to obtain the coating.

[0043] According to a preferred embodiment, step (4) of the present invention specifically comprises: coating the coating on the tire base cloth, and then covering the upper surface and the lower surface of the coated tire base cloth with an isolation material, and obtaining the waterproof coiled material after compacting, cooling, trimming, and rolling;

[0044] Among them, the gram weight of the tire base cloth is 240-270g / ㎡; the thickness of the coating is 0.8-1.5mm; the isolation material is a polyethylene film with a thickness of 0.012-0.015mm; the thickness of the waterproof coiled material is 3-4.5mm.

[0045] More preferably, the tire base fabric is a polyester tire base fabric that is oil-impregnated and then dried.

[0046] Preferably, in the method of the present invention, relative to 100 parts by weight of the petroleum resin, relative to 100 parts by weight of the coating, the amount of the cyclohexane oil is 11-14 parts by weight, the amount of the SBS modifier is 5.5-7.5 parts by weight, the amount of the asphalt is 50-56 parts by weight, the amount of the anti-aging agent is 0.05-0.10 parts by weight, the amount of the petroleum resin is 12-15 parts by weight, the amount of the BL modifier is 2.2-4 parts by weight, and the amount of the filler is 10-12 parts by weight.

[0047] As mentioned above, the second aspect of the present invention provides a low-temperature moldable SBS modified asphalt waterproof membrane prepared by the method described in the first aspect.

[0048] As mentioned above, the third aspect of the present invention provides the use of the low-temperature moldable SBS modified asphalt waterproof membrane described in the second aspect in building waterproofing.

[0049] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the raw materials used are all common commercially available products.

[0050] Some of the raw materials and their sources used in the following examples are as follows:

[0051] Naphthenic oil: purchased from Shanghai Yanzhong Industrial Co., Ltd., brand KN4010;

[0052] SBS modifier: purchased from LG Chemical Company, brand 411;

[0053] Asphalt: 200# asphalt, purchased from Hebei Lunte Company;

[0054] Anti-aging agent: antioxidant 1010, purchased from BASF, brand number 1010;

[0055] Petroleum resin: terpene resin, purchased from Shangrao Sinan Resin Co., Ltd., brand SNT-1001;

[0056] BL modifier:

[0057] BL modifier I: polyethylene wax AC316A, purchased from Honeywell, brand 316A;

[0058] BL modifier II: polyethylene wax TL-500C, purchased from Guangdong Taili New Materials Technology Co., Ltd.;

[0059] BL modifier III: NV-408P, purchased from Comino New Materials Technology (Zhejiang) Co., Ltd., brand number 007;

[0060] Filler: nano calcium carbonate, purchased from Shaanxi Huateng Nanotechnology Co., Ltd., with an average particle size of 90 nm;

[0061] High-speed shear tester; purchased from Anhui Wannan Electric Motor Co., Ltd., model number is YE3VF250-4 V1.

[0062] In the following examples, each "part by weight" means 100 g unless otherwise specified.

[0063] Preparation Example 1

[0064] Preparation of swollen SBS G1:

[0065] Under the stirring condition of a rotation speed of 800 r / min, 11 parts by weight of cyclohexane oil were first introduced into a high-speed shear instrument and heated to a mixing temperature of 140°C for mixing I, and the heating rate was 5°C / min. Then, under the condition of heat preservation, 5.5 parts by weight of SBS modifier were added for mixing II for 1 hour. After cooling to room temperature, a swollen SBS was obtained, named G1, wherein the rotation speed of the mixing II was 1200 r / min.

[0066] Preparation Example 2

[0067] Preparation of swollen SBS G2:

[0068] Under stirring condition of a rotation speed of 1000 r / min, 14 parts by weight of cyclohexane oil were first introduced into a high-speed shear instrument and heated to a mixing temperature of 180°C for mixing I, and the heating rate was 7°C / min. Then, under heat preservation condition, 5.5 parts by weight of SBS modifier were added for mixing II for 0.7 h. After cooling to room temperature, swollen SBS was obtained, named G2, wherein the rotation speed of mixing II was 1300 r / min.

[0069] Embodiment 1:

[0070] This embodiment is used to illustrate the waterproofing membrane provided by the present invention with reference to the parameters in Table 1, specifically including:

[0071] S1, bringing the swollen SBS G1 into first contact with asphalt, specifically comprising:

[0072] Under the condition of a stirring speed of 1200 r / min, the asphalt is first heated to a first contact temperature of 140° C. at a heating rate of 5° C. / min, and then the swollen SBS is added under the condition of heat preservation to perform the first contact to obtain the mixture I, wherein the first contact time is 1 hour;

[0073] S2, bringing the mixture I into second contact with an anti-aging agent, a petroleum resin, a BL modifier (BL modifier I) and a filler, specifically comprising:

[0074] At a stirring speed of 1200 r / min and a temperature of 140° C., a petroleum resin, an anti-aging agent and a BL modifier are first added into a reactor, and a first stirring is performed for 0.5 h, and then a filler is added and a second stirring is performed for 0.5 h to obtain the coating;

[0075] S3, coating:

[0076] The coating is applied to the tire base fabric which is treated with oil and then dried, and then the upper and lower surfaces of the coated tire base fabric are covered with a polyethylene film of an insulating material, and after compaction, cooling, trimming, and rolling, a waterproof coiled material with a thickness of 3 mm is obtained, which is named P1;

[0077] The weight of the tire base fabric is 260 g / m 2 ; The thickness of the coating is 1.2 mm, and the thickness of the isolation material is 0.012 mm.

[0078] Example 2

[0079] This embodiment adopts the same process as that of embodiment 1, except that in step S1, swelling SBSG2 is used instead of swelling SBS G1, and the process parameters and addition amount are changed. For specific parameters, refer to Table 1;

[0080] The waterproof membrane with a thickness of 3 mm was obtained and named P2.

[0081] Example 3

[0082] This example is carried out using the same process as Example 1, except that BL modifier II is used instead of BL modifier I, and the process parameters are changed. For specific parameters, refer to Table 1;

[0083] The waterproof membrane with a thickness of 3 mm was obtained and named P3.

[0084] Example 4

[0085] This example is carried out using the same process as Example 1, except that BL modifier III is used instead of BL modifier I. For specific parameters, refer to Table 1;

[0086] The waterproof membrane with a thickness of 3 mm was obtained and named P4.

[0087] Comparative Example 1

[0088] This comparative example is carried out by the same process as Example 1, except that in step S1, the raw materials for preparing swollen SBS (naphthenic oil and modifier) ​​in the same weight parts as those in Preparation Example 1 are directly used instead of swollen SBS, wherein the specific operation of the first contact is:

[0089] Under the condition of a stirring speed of 1200r / min, 50 parts by weight of 200# asphalt and 11 parts by weight of cyclohexane oil are first heated to a first contact temperature of 140°C at a heating rate of 5°C / min, and then 5.5 parts by weight of SBS modifier are added and stirred for 1h under the condition of heat preservation to obtain the mixture I applied to step S2.

[0090] The waterproof membrane with a thickness of 3 mm was obtained and named DP1.

[0091] Comparative Example 2

[0092] This comparative example is carried out using the same process as Example 1, except that in step S2 of this comparative example, no BL modifier is added, that is, the amount of BL modifier added is 0 parts by weight.

[0093] The waterproof membrane with a thickness of 3 mm was obtained and named DP2.

[0094] Comparative Example 3

[0095] This comparative example is carried out using the same process as Example 1, except that in step S1, an oil-extended SBS (manufacturer: Huizhou Li Changrong; brand: 1475; in a granular state at 25° C., oil content: 31-36wt%) having the same weight portion as the swollen SBS in Example 1 is used instead of the swollen SBS.

[0096] The waterproof membrane with a thickness of 3 mm was obtained and named DP3.

[0097] Test Example 1

[0098] Coil samples were cut according to the standard GB 18242-2008, and the heat resistance, low temperature flexibility and seam peel strength of some products in the above examples were measured respectively. The test results are shown in Table 2.

[0099] Table 1

[0100]

[0101]

[0102] Table 2

[0103]

[0104] From the above results, it can be seen that the method provided by the present invention can prepare a waterproof roll that can be formed at low temperature by a safe and environmentally friendly method while ensuring the heat resistance and joint peeling strength of the asphalt waterproof roll.

[0105] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing SBS modified asphalt waterproofing membrane, It is characterized in that The method includes: (1) mixing cyclohexane oil and SBS modifier to obtain a swollen SBS in a gel state at 25° C. (2) contacting the swollen SBS with asphalt for the first time to obtain a mixture I; the conditions of the first contact at least meet the following conditions: a temperature of 130-150° C. and a time of 0.5-2 h; (3) contacting the mixture I with an anti-aging agent, a petroleum resin, a BL modifier and a filler for a second time to obtain a coating; the conditions of the second contact at least meet the following conditions: a temperature of 130-150° C. and a time of 0.1-2 h; (4) coating the coating on the base fabric to obtain the waterproof roll material.

2. The method according to claim 1, in, In step (1), the mixing temperature is 140-230°C.

3. The method according to claim 2, in, The naphthenic oil has a kinematic viscosity of 5-20 mPa·s at 100° C.; and / or The melt index of the SBS modifier is 0.2-1.5 g / 10 min.

4. The method according to claim 2, in, In step (1), the mixing conditions at least meet the following requirements: mixing under stirring, with a rotation speed of 800-1400 r / min, a mixing temperature of 160-220° C., and a mixing time of 2.5-4.0 h.

5. The method according to any one of claims 1 to 4, in, In step (2), the asphalt is selected from at least one of 200# asphalt, 90# asphalt, and 70# asphalt; and / or The first contacting condition also includes: being carried out under stirring condition with a rotation speed of 800-1200 r / min.

6. The method according to any one of claims 1 to 4, in, In step (3), the anti-aging agent is selected from at least one of antioxidant 1010 and anti-aging agent 3050; and / or The petroleum resin is selected from at least one of terpene resin, C5 petroleum resin and C9 petroleum resin; and / or The BL modifier is selected from at least one of polyethylene wax AC316A, polyethylene wax LD-808T, and polyethylene wax TL-500C; and / or The filler is selected from at least one of nano calcium carbonate, organic bentonite and organic diatomaceous earth.

7. The method according to any one of claims 1 to 4, in, In step (3), the second contacting condition also includes: being carried out under stirring conditions at a rotation speed of 800-1200 r / min.

8. The method according to any one of claims 2 to 4, in, Relative to 100 parts by weight of the coating, the amount of the cyclohexane oil is 11-14 parts by weight, the amount of the SBS modifier is 5.5-7.5 parts by weight, the amount of the asphalt is 50-56 parts by weight, the amount of the anti-aging agent is 0.05-0.10 parts by weight, the amount of the petroleum resin is 12-15 parts by weight, the amount of the BL modifier is 2.2-4 parts by weight, and the amount of the filler is 10-12 parts by weight.

9. The SBS modified asphalt waterproofing membrane capable of being formed at low temperature prepared by any one of claims 1 to 8.

10. Use of the low-temperature moldable SBS modified asphalt waterproofing membrane according to claim 9 in building waterproofing.