Adhesive tape
By using plant-derived fibers to laminate polyolefin as the base material in the adhesive tape, and adding natural rubber, wood-based fillers, and plant plasticizers to the adhesive layer, the adhesive tape is easily deformed and greenhouse gases are eliminated. emissions issues, achieving high biobase and good adhesive properties.
Patent Information
- Application Number
- CN202080102465.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-04-27
AI Technical Summary
Existing adhesive tapes are easily deformed and sticky on the sides during use, and produce a large amount of greenhouse gases, especially carbon dioxide, when burned.
It uses plant-derived fibers laminated with processed polyolefin as the base material, and uses natural rubber, wood-based fillers, plant-derived plasticizers and tackifiers in the adhesive layer as fillers and softening ingredients to improve adhesion. Shape stability and biobasedness of the mixture.
It effectively suppresses the deformation and side stickiness of the adhesive tape, reduces carbon dioxide emissions during incineration, improves the smoothness and adhesive performance of the adhesive surface, and improves the biobase.
Smart Images

Figure BDA0004017843010000121 
Figure BDA0004017843010000131
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive tape for use in packaging, maintenance and the like. Background Art
[0002] In the past, a cloth adhesive tape having a structure in which a polyethylene resin layer is provided on one side of a woven fabric formed by using rayon spun yarn for warp and weft, and a rubber adhesive layer is provided on the other side, has been used for packaging, maintenance, and the like. The rubber adhesive of the adhesive tape used for such purposes is manufactured by masticating, for example, natural rubber to reduce its molecular weight, and kneading it with various compounding materials. However, the adhesive tape using such a rubber adhesive has the following problems: due to the low molecular weight of the rubber adhesive, when the adhesive tape is wound and set in a roll, the roll is deformed, and the rubber adhesive is squeezed out from the side of the roll to cause stickiness on the side of the roll.
[0003] After manufacturing, cloth adhesive tapes used for packaging, maintenance, etc. are packaged and delivered to retail stores or their warehouses, displayed in stores, or delivered directly to users. Therefore, due to deformation caused by contact between tapes during delivery and loads applied to the tape sides, packaging materials may stick to the tape sides, making it difficult to peel off the packaging materials, etc. In particular, tapes with thick adhesive layers are easily affected, and deformation and side stickiness must be suppressed.
[0004] On the other hand, the adhesive tape is peeled off and incinerated after being used for packaging purposes, maintenance purposes, etc. Therefore, when a large amount of materials derived from petroleum are used, the emission of greenhouse gases represented by carbon dioxide becomes a problem. As a technology for suppressing greenhouse gas emissions from adhesive tapes, Patent Document 1 can be cited. Patent Document 1 discloses a technology for suppressing greenhouse gas emissions from adhesive tapes, wherein a bio-based material is used as a substrate, but most of the adhesive components use materials derived from petroleum, so there is a problem that the proportion of bio-based materials in the overall material, i.e., the bio-based degree, is low and the inhibitory effect of greenhouse gas emissions is limited.
[0005] In addition, in the past, the rubber-based adhesive used for the adhesive of the adhesive tape contained a large amount of heavy calcium carbonate as a filler, which has been widely used so far because it is cheap and easy to obtain. However, when a large amount of adhesive tape containing heavy calcium carbonate is incinerated, carbon dioxide is produced due to the decarbonation of the heavy calcium carbonate, and thus a large amount of greenhouse gas is discharged. Therefore, it is sought to suppress the discharge of greenhouse gas caused by incineration by using a large amount of plant-derived materials in the adhesive tape and using a wood-based filler that can replace heavy calcium carbonate. However, when the filler of the adhesive uses a wood-based filler, there are the following problems: the dispersibility of the filler in the adhesive becomes poor, the coating property to the substrate is reduced, the smoothness of the adhesive surface is impaired, and the adhesive properties are reduced.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: WO2015 / 056499 Pamphlet Summary of the invention
[0009] Problems to be solved by the invention
[0010] An object of the present invention is to provide a pressure-sensitive adhesive tape that can satisfy the required properties of a pressure-sensitive adhesive tape, such as adhesive force and holding force, while being less likely to deform, suppressing stickiness on the side surfaces, and suppressing the emission of greenhouse gases.
[0011] Means for solving problems
[0012] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have solved the above-mentioned problems by adopting the following configuration.
[0013] That is, the adhesive tape of the present invention is an adhesive tape comprising a substrate obtained by laminating processed polyolefin on plant-derived fibers, and an adhesive layer provided on at least one surface of the substrate, wherein the adhesive layer contains natural rubber, a wood-based filler, a plant-derived plasticizer, and a tackifier.
[0014] Effects of the Invention
[0015] The adhesive tape of the present invention uses a wood-based filler from a plant as a filler for an adhesive, thereby improving the shape stability of the adhesive, and compared with a filler from a mineral such as heavy calcium carbonate, the tape is not easily deformed, and the stickiness of the tape side is also reduced. In addition, by using a plasticizer from a plant as a softening component for the adhesive, the smoothness of the adhesive surface can be maintained and the reduction of the required characteristics can be suppressed even if a wood-based filler is used. In addition, since the material from the plant is included, the increase of carbon dioxide in the atmosphere caused by incineration can be suppressed, and the discharge of carbon dioxide caused by the decarbonation of the heavy calcium carbonate can also be prevented. DETAILED DESCRIPTION
[0016] The pressure-sensitive adhesive tape of the present invention comprises a substrate obtained by laminating a processed polyolefin on a plant-derived fiber, and a pressure-sensitive adhesive layer provided on at least one surface of the substrate.
[0017] [Adhesive layer]
[0018] The adhesive layer contains natural rubber, a wood-based filler, a plant-derived plasticizer, and a tackifier. Each component is described in detail below.
[0019] (Natural Rubber)
[0020] The adhesive component used in the adhesive layer of the present invention contains natural rubber.
[0021] Natural rubber is obtained by solidifying the sap (latex) collected from the rubber tree called Hevea brasiliensis. Natural rubber is roughly divided into sheet rubber, which is coagulated with acid such as formic acid, dried and made into sheets, and lump rubber, which is made by repeatedly crushing, washing, drying and pressing the cup rubber obtained by natural coagulation in the cup for collecting latex in the rubber farm.
[0022] The classification of sheet rubber is determined by the rating of "International Quality Packaging Standards for Various Grades of Natural Rubber" (commonly known as "Green Book"), and the variety is determined by the raw materials and the manufacturing method. There are crepe sheets (Japanese: レープ), etc., which are obtained by smoking and drying the sheets, and the resulting smoked sheet rubber (RSS) and coagulant are fully washed with water and dried with hot air. Sheet rubber is classified into grades such as RSS#3, RSS#1, white wrinkled sheet, and bottom crepe sheet (Japanese: ソールレープ). When sheet rubber is used as the adhesive component of the present invention, any one grade of them can be used alone, or a plurality of grades can be used in combination.
[0023] Block rubber is a natural rubber obtained by washing and drying solidified small granules of rubber, pressing and molding, and rating it according to ISO standards (ISO2000). There are standard grades such as TSR20 and TSR10, TSRCV grades with hydroxylamine hydrochloride added as a viscosity stabilizer, and TSRL grades with sodium pyrosulfite added as an anti-discoloration agent. When block rubber is used as the adhesive component of the present invention, any one grade of these may be used alone, or a plurality of grades may be used in combination.
[0024] In addition, when natural rubber is described in this specification, liquid natural rubber described later is not included unless otherwise specified.
[0025] (Wood-based filler)
[0026] The adhesive layer of the present invention contains a wood-based filler as a filler. Examples of the wood-based filler include powdered cellulose and lignin compounds. Among them, powdered cellulose has an effect of reinforcing the adhesive due to its fibrous shape, and because of its large volume, it can reduce the amount of adhesive in the tape thickness, thereby reducing material costs.
[0027] Powdered cellulose includes acid-treated cellulose obtained by pulverizing a cellulose raw material such as pulp that has been subjected to an acid hydrolysis treatment with a mineral acid (i.e., an inorganic acid) such as hydrochloric acid, sulfuric acid, or nitric acid, and mechanically pulverized cellulose obtained by mechanically pulverizing a cellulose raw material such as pulp that has not been subjected to an acid hydrolysis treatment. Powdered cellulose can be appropriately selected and used depending on the required performance, etc.
[0028] The average particle size of the wood-based filler is preferably more than 1 μm and less than 50 μm. When the average particle size is less than 50 μm, the surface smoothness of the adhesive layer will not be damaged. It should be noted that when the adhesive surface is not smooth, the adhesive tape sometimes cannot obtain sufficient adhesion relative to the adherend and cannot fully exert the adhesive performance. In addition, when the average particle size is more than 1 μm, the desired large volume can be obtained, and the thickness of the adhesive layer can be ensured. In addition, the increase in the amount of adhesive occupied in the tape thickness can be suppressed, and the rise in material cost can be suppressed. The average particle size used here is the median particle size represented by D50.
[0029] The amount of the wood-based filler added is preferably 10 to 250 parts by mass, more preferably 50 to 150 parts by mass, relative to 100 parts by mass of natural rubber. When it is 10 parts by mass or more, the rubber elasticity of the adhesive is suppressed from increasing, and the coating property when the adhesive is applied to the substrate can be suppressed from decreasing. On the other hand, when it is 250 parts by mass or less, the rubber elasticity of the adhesive is suppressed from decreasing, and the adhesive performance can be prevented from decreasing.
[0030] (Plasticizer)
[0031] The adhesive layer of the present invention contains a plant-derived plasticizer as a softening component of the adhesive. As the plant-derived plasticizer, liquid natural rubber, soybean oil, sunflower oil, rapeseed oil, cottonseed oil, linseed oil, corn oil, canola oil, palm oil, or modified substances thereof (e.g., epoxidized soybean oil, etc.) can be used. Any of these plant-derived plasticizers can be used alone, or multiple types can be used in combination.
[0032] When liquid natural rubber is used as a plasticizer, the rapid viscosity reduction during the matching can be suppressed, so the dispersibility of the adhesive becomes good. In addition, when vegetable oils such as soybean oil are used, since the vegetable oils and wood-based fillers have polar groups, they have high affinity and will not cause a rapid viscosity reduction during the matching, and the dispersibility becomes good. Among them, liquid natural rubber is preferred.
[0033] Liquid natural rubber is obtained by depolymerizing natural rubber. Examples of depolymerization methods include a method of cutting rubber molecules by a mechanochemical reaction using shear force using a rolling mill, a method of decomposing the rubber solution by photochemical reaction by irradiating the rubber solution with ultraviolet rays, a method of chemical oxidation decomposition using phenylhydrazine, and a method of air oxidation in the presence of a free radical initiator.
[0034] The weight average molecular weight (Mw) of the liquid natural rubber is preferably 100,000 or less, more preferably 80,000 or less, and further preferably 40,000 or less. When Mw is 100,000 or less, the decrease in wettability of the adhesive layer is suppressed, and deterioration in adhesion at low temperatures can be prevented.
[0035] The amount of the plant-derived plasticizer added is preferably 5 to 50 parts by mass, more preferably 10 to 30 parts by mass, relative to 100 parts by mass of natural rubber. When the amount of the plasticizer is 5 parts by mass or more, the decrease in wettability of the adhesive layer is suppressed, and the deterioration of the adhesion at low temperatures can be prevented. When the amount is 50 parts by mass or less, the plasticizer does not ooze out, and contamination of the adherend and changes in adhesive properties over time can be suppressed.
[0036] (Thickener)
[0037] The adhesive layer of the present invention includes a tackifier. By using a plant-derived tackifier as the tackifier, it is possible to further seek to improve the bio-basedness. As plant-derived tackifiers, terpene resins, terpene phenol resins, rosin resins, rosin ester resins, etc. can be cited. Among them, terpene resins have a high bio-basedness and can reduce carbon dioxide emissions, so they are preferred. Any one of the tackifiers can be used alone, or multiple types can be used in combination.
[0038] As the tackifier, it is preferable to select a softening point in the range of 70°C to 150°C. When the softening point is 70°C or higher, the decrease in adhesive strength is suppressed, and side stickiness can also be suppressed. In addition, when the softening point is 150°C or lower, the compatibility with natural rubber is excellent, and the decrease in adhesive strength can be suppressed.
[0039] Examples of the terpene resin include unmodified terpene polymers such as α-pinene polymers, β-pinene polymers, and limonene polymers; and modified terpene polymers obtained by modifying the terpene polymers by one or more treatments selected from phenol modification, aromatic modification, hydrogenation modification, and hydrocarbon modification. Examples of modified terpene polymers include terpene phenol resins and aromatic modified terpene resins. Any of these may be used alone, or a plurality of them may be used in combination.
[0040] Examples of the rosin resin include unmodified rosins such as gum rosin, wood rosin, and tall oil rosin; modified rosins obtained by modifying unmodified rosins by one or more treatments selected from hydrogenation, disproportionation, polymerization, and chemical modification; and various rosin derivatives.
[0041] Examples of the rosin derivatives include: rosin esters obtained by esterifying unmodified rosin or modified rosin with alcohols; unsaturated fatty acid-modified rosins obtained by modifying unmodified rosin or modified rosin with unsaturated fatty acids; unsaturated fatty acid-modified rosin esters obtained by modifying rosin esters with unsaturated fatty acids; rosin alcohols obtained by reducing the carboxyl groups in unmodified rosin, modified rosin, unsaturated fatty acid-modified rosin, or unsaturated fatty acid-modified rosin esters; ; Metal salts of rosins (especially rosin esters) such as unmodified rosin, modified rosin, various rosin derivatives, etc.; Rosin phenol resin obtained by adding phenol to rosins such as unmodified rosin, modified rosin, various rosin derivatives, etc. with an acid catalyst and performing thermal polymerization; Acid-modified rosins obtained by modifying unmodified rosin or modified rosin with acids such as acrylic acid, fumaric acid, or maleic acid; Acid-modified rosin esters obtained by modifying rosin esters with acids such as acrylic acid, fumaric acid, or maleic acid, etc. Any of them can be used alone, or multiple types can be used in combination.
[0042] The amount of the tackifier added is preferably 30 to 150 parts by mass, more preferably 60 to 120 parts by mass, relative to 100 parts by mass of natural rubber. When the tackifier is 30 parts by mass or more, a decrease in adhesive strength can be suppressed, and when it is 150 parts by mass or less, a decrease in removability when the adhesive tape is peeled off can be suppressed.
[0043] (Other matching materials)
[0044] The adhesive layer may contain, in addition to the above-mentioned components, other components known in the art, such as vulcanizing agents, vulcanization accelerators, vulcanization aids, antioxidants, conductive materials, mastication accelerators, colorants, and the like.
[0045] [Base material]
[0046] As the substrate used for the pressure-sensitive adhesive tape of the present invention, a laminate obtained by laminating a polyolefin on a plant-derived fiber is used.
[0047] (Fiber from plants)
[0048] As the fiber from plants, rayon, cotton, kapok, flax, ramie, hemp, jute, Manila hemp, sisal, palm, coconut, cuprammonia fiber etc. can be mentioned. Any one or a plurality of plant-derived fibers can be used. In addition, about their blending, it is arbitrary and is not particularly limited. In addition, the fiber can be in the form of woven fabric, knitted fabric, nonwoven fabric etc., which is not particularly limited.
[0049] (Polyolefin)
[0050] As polyolefins, high-density polyethylene (HDPE), low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), polypropylene (PP), ethylene-vinyl acetate copolymer (EVA), ethylene-ethyl acrylate copolymer (EEA), etc. can be cited. From the viewpoint of increasing the bio-based content, it is preferred to use bio-based polyolefins. Here, the so-called bio-based polyolefins refer to polyolefins produced from bioethanol from plants such as sugarcane. The method for producing bio-based polyolefins is not particularly limited, and various known methods can be used. As bio-based polyolefins, for example, commercially available bio-based polyethylene can be used. Any one of the bio-based polyolefins can be used alone, or multiple types can be used in combination.
[0051] [Biobasedness]
[0052] For the adhesive tape of the present invention, it is preferred to select each material in such a way that the biobased content is 50% or more. The so-called biobased content of the adhesive tape refers to the mass ratio of the components derived from biomass in the total mass of the adhesive tape. The biobased content of the adhesive tape can be calculated by ISO16620-4 (method for calculating the biobased mass content). Specifically, it is a value calculated by calculating the mass of the entire adhesive tape (A) and the mass of the components derived from biomass (B) and using the following formula.
[0053] Biobase (%) = {mass (B) / mass (A)} × 100
[0054] The higher the biobase, the more it can reduce the actual carbon dioxide emissions. In the present invention, since the biobase of the adhesive layer can be effectively improved, which has not been available before, it is easy to achieve a biobase of 90% or more as an adhesive tape. It should be noted that when a copolymer or a combination of multiple materials is used, a part of the components derived from biomass is used and the rest is a component derived from petroleum, the biobase is calculated based on the ratio of the components derived from biomass in each component.
[0055] The biomass-derived component used in the adhesive tape of the present invention refers to renewable organic resources from plants, excluding materials that have been exhausted by mining, such as fossil resources. The biomass-derived component may be, for example, the renewable organic resources themselves, or a material obtained by chemically or biologically modifying the organic resources, or synthesizing the organic resources.
[0056] Components from biomass also release carbon dioxide when burned, but the amount of carbon dioxide released is the same as the amount of carbon dioxide absorbed from the atmosphere by plants through photosynthesis during growth, so it can be considered that it does not affect the increase or decrease of carbon dioxide in the atmosphere. This way of thinking is called carbon neutrality. By using components from biomass as the constituent materials of the adhesive tape, the amount of carbon dioxide can be reduced.
[0057] [Method for producing adhesive tape]
[0058] The manufacturing method of the adhesive tape is not particularly limited and can be manufactured by a known method. For example, regarding the substrate, the fiber from the plant is formed into a desired woven fabric, etc., and an olefin resin is laminated on both sides or one side thereof. The lamination method can be any of a method in which a film of an olefin resin is overlapped on a woven fabric and hot-pressed, or an olefin resin is hot-melted and extruded on a woven fabric. In addition, a surface treatment can be applied to the surface of the woven fabric, etc., on which the laminated layer is formed, and then the laminated layer is formed.
[0059] Next, the adhesive composition prepared by mixing separately is applied to one or both surfaces of the substrate to form an adhesive layer. In order to improve the adhesion, the surface of the substrate to be coated with the adhesive composition may be subjected to a surface treatment.
[0060] As a surface treatment, a physical or chemical anchoring treatment (AC treatment) is performed. As a physical treatment, corona treatment, UV treatment, sputtering treatment, etc. can be mentioned, and as a chemical treatment, a treatment of coating a resin selected from organic titanium, isocyanate, polyethyleneimine, polybutadiene, etc. can be mentioned. It should be noted that from the viewpoint of increasing the biobased content, physical treatment is preferred.
[0061] The pressure-sensitive adhesive layer is formed by coating with various coating devices, such as a calendar coater, a roll coater, a die coater, a lip coater, a Meyer bar coater, and a gravure coater.
[0062] Here, the thickness of the substrate is preferably in the range of 50 to 500 μm, more preferably in the range of 100 to 300 μm. When it is 100 μm or more, the rigidity of the substrate is improved and the workability becomes good, and when it is 500 μm or less, the adhesion to the concave and convex surface of the adherend is improved and it is not easy to peel off from the adherend.
[0063] Regarding the adhesive layer, for example, the coating amount per single side can be 30 to 400 g / m2 depending on the purpose. 2 The thickness of the tape can be selected from a range of 80 to 900 μm.
[0064] The produced adhesive tape is wound into a roll and cut into a predetermined width. The cut tape is protected on the sides with a packaging material such as a polyethylene film to prevent adhesives of other tapes from contacting each other, and is packed in a box.
[0065] The adhesive tape of the present invention can effectively suppress stickiness on the tape side.
[0066] Example
[0067] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples. In addition, the physical property values of each raw material and the like are the values in the product specifications of the manufacturers.
[0068] [Example 1]
[0069] The warp and weft yarns were both 30-count rayon yarns, and the woven fabric was woven with a warp density of 45 strands / inch and a weft density of 35 strands / inch. A biomass low-density polyethylene (trade name "SBC818", manufactured by BRASKEM SA, density 0.918 g / cm) was formed on one surface of the woven fabric by extrusion lamination using a T-die at a processing temperature of 300°C. 3) to prepare a substrate with a total thickness of 200 μm. The adhesive composition was prepared as follows: 100 parts by mass of powdered cellulose (1) (trade name "KC FLOCK W-200", manufactured by Nippon Paper Industries, Ltd.) with an average particle size of 32 μm as a filler, 25 parts by mass of liquid natural rubber (1) (trade name "DPR-40", manufactured by DPR Industries, Ltd.) with a weight average molecular weight (Mw) of 40,000 as a plasticizer, and 100 parts by mass of a terpene resin (trade name "YS Resin PX1000", manufactured by YASUHARA CHEMICAL, Ltd., softening point: 100±5°C) as a tackifier were mixed with 100 parts by mass of natural rubber masticated by a kneader. The adhesive composition was applied to the other side of the woven fabric in a manner to a film thickness of 100 μm using a calender coater to obtain an adhesive tape with a total thickness of 300 μm.
[0070] [Example 2]
[0071] A pressure-sensitive adhesive composition was prepared in the same manner as in Example 1 except that the filler was changed to 80 parts by mass of powdered cellulose (2) having an average particle size of 37 μm (trade name "KC FLOCK W-100", manufactured by Nippon Paper Industries, Ltd.). The pressure-sensitive adhesive composition was applied to the same substrate as in Example 1 to obtain a pressure-sensitive adhesive tape having a total thickness of 300 μm.
[0072] [Example 3]
[0073] A pressure-sensitive adhesive composition was prepared in the same manner as in Example 1 except that the filler was changed to 40 parts by mass of powdered cellulose (3) having an average particle size of 45 μm (trade name "KC FLOCK W-50", manufactured by Nippon Paper Industries, Ltd.). The pressure-sensitive adhesive composition was applied to the same substrate as in Example 1 to obtain a pressure-sensitive adhesive tape having a total thickness of 300 μm.
[0074] [Example 4]
[0075] A pressure-sensitive adhesive composition was prepared in the same manner as in Example 1 except that the filler was changed to 120 parts by mass of powdered cellulose (4) having an average particle size of 24 μm (trade name "KC FLOCK W-400", manufactured by Nippon Paper Industries, Ltd.). The pressure-sensitive adhesive composition was applied to the same substrate as in Example 1 to obtain a pressure-sensitive adhesive tape having a total thickness of 300 μm.
[0076] [Example 5]
[0077] A pressure-sensitive adhesive composition was prepared in the same manner as in Example 1 except that the plasticizer was changed to 25 parts by mass of liquid natural rubber (2) having a weight average molecular weight (Mw) of 80,000 (trade name "DPR-400", manufactured by DPR INDUSTRIES INC.). The pressure-sensitive adhesive composition was applied to the same substrate as in Example 1 to obtain a pressure-sensitive adhesive tape having a total thickness of 300 μm.
[0078] [Example 6]
[0079] A PSA composition was prepared in the same manner as in Example 1 except that the plasticizer was changed to 25 parts by mass of soybean oil (trade name "NIKKA soybean white twist oil", manufactured by Nikka Oil & Fats Co., Ltd.). The PSA composition was applied to the same substrate as in Example 1 to obtain a PSA tape having a total thickness of 300 μm.
[0080] [Example 7]
[0081] A PSA composition was prepared in the same manner as in Example 1 except that the plasticizer was changed to 25 parts by mass of epoxidized soybean oil (trade name "ADK CIZER O-130P", manufactured by ADEKA Corporation). The PSA composition was applied to the same substrate as in Example 1 to obtain a PSA tape having a total thickness of 300 μm.
[0082] [Comparative Example 1]
[0083] The woven fabric was woven using 30-count rayon yarns for both the warp and weft yarns with a warp density of 45 yarns / inch and a weft density of 35 yarns / inch. Low-density polyethylene (trade name "NUC8008", density 0.918 g / cm2) was formed on one side of the woven fabric by extrusion lamination using a T-die at a processing temperature of 300°C. 3 , made by Nippon Unicar), to prepare a substrate with a total thickness of 200 μm. The adhesive composition was prepared as follows: 200 parts by mass of heavy calcium carbonate (made by MARUO CALCIUM (Strain)) with an average particle size of 12 μm as a filler, 25 parts by mass of processing oil (trade name "Mobiltherm 610", made by EMG LUBRICANTS Contract Co., Ltd.) as a plasticizer, and 100 parts by mass of C5 resin (trade name "T-REZ RC100", made by JXTG Energy, softening point: 95-105°C) as a tackifier were mixed with 100 parts by mass of natural rubber masticated by a kneading machine. The adhesive composition was applied to the above substrate in a manner to form a film thickness of 100 μm to obtain an adhesive tape with a total thickness of 300 μm.
[0084] [Comparative Example 2]
[0085] 100 parts by mass of natural rubber masticated by a kneader were mixed with 180 parts by mass of starch powder (first-grade starch manufactured by Hayashi Junyaku Kogyo Co., Ltd.) having an average particle size of 10 μm as a filler, 25 parts by mass of processing oil (trade name "Mobiltherm 610", manufactured by EMG LUBRICANTS) as a plasticizer, and 100 parts by mass of C5 resin (trade name "T-REZ RC100", manufactured by JXTG Energy, softening point: 95-105° C.) as a tackifier to prepare an adhesive composition. The adhesive composition was applied to the same substrate as in Comparative Example 1 to obtain an adhesive tape having a total thickness of 300 μm.
[0086] <Test method>
[0087] The tape samples obtained as the above examples and comparative examples were tested and evaluated for various properties by the following methods. The results are shown in Tables 1 and 2.
[0088] [Adhesion]
[0089] Adhesion was measured according to 10 (Adhesion) of JIS Z 0237 (Testing methods for adhesive tapes and sheets). The test conditions were as follows: [Adhesion tape width: 10 mm, peeling angle: 180 degrees, test temperature: 23°C]
[0090] [Retention force]
[0091] The holding force was measured according to 13 (holding force) of JIS Z 0237 (Testing methods for adhesive tapes and adhesive sheets). The test conditions are as follows. [Area of adhesive tape: width 25 mm × length 25 m, weight: 1000 g, test temperature: 40°C]
[0092] [Constant load peel force]
[0093] A 10 mm wide tape was attached to a stainless steel (SUS304BA) plate under an environment of 23°C and 50% RH, and a 2 kg rubber roller was reciprocated once for pressure bonding. After being left in the same environment for 30 minutes, a load was applied to the tape in a 90 degree direction with a 100 g weight hung at the end of the tape, and the time until it fell was measured at room temperature (23°C).
[0094] [Yield point load]
[0095] A 50 mm wide and 25 m belt was sandwiched between two parallel plates in contact with only the side surfaces of the belt at 23°C and 50% RH, and a load was applied using a compression tester. The stress until failure was measured to determine the yield point load value.
[0096] [Side stickiness]
[0097] A 50 mm wide and 25 m tape was placed with the tape side facing downward, with a PE liner sandwiched between the tapes, and 5 rolls were overlapped. The tape was placed in a dryer at 40°C for 28 days. After returning to room temperature, the stickiness of the tape side at the bottom was evaluated based on the following criteria.
[0098] ○: The PE liner can be easily peeled off.
[0099] ×: The PE liner could not be easily peeled off.
[0100] [Table 1]
[0101]
[0102] [Table 2]
[0103]
[0104] Industrial Applicability
[0105] As described above, according to the results of the yield point load value, the adhesive tape of the present invention is not easily deformed, can suppress the stickiness of the tape side, and can be widely used in various fields such as packaging and maintenance, just like existing products. In addition, since it is easy to make the bio-based content 90% or more, it is possible to achieve a high level of suppression of greenhouse effect (carbonic acid) gas emissions.
Claims
1. An adhesive tape comprising: a substrate comprising plant-derived fibers; a laminate layer comprising an olefin resin laminated on both sides or one side of the substrate; and an adhesive layer provided on at least one surface of the substrate, The adhesive layer contains natural rubber as adhesive components, a wood-based filler, a plant-derived plasticizer, and a tackifier. The plant-derived plasticizer is liquid natural rubber.
2. The pressure-sensitive adhesive tape according to claim 1, wherein the biobased content is 50% by mass or more.
3. The adhesive tape according to claim 1 or 2, wherein The adhesive layer contains 10 to 250 parts by mass of the wood-based filler, 5 to 50 parts by mass of the plant-derived plasticizer, and 30 to 150 parts by mass of the tackifier, based on 100 parts by mass of the natural rubber.
4. The adhesive tape according to claim 1 or 2, wherein The wood-based filler is powdered cellulose.
5. The adhesive tape according to claim 4, wherein The average particle size of the powdered cellulose is 1 μm to 50 μm.
6. The adhesive tape according to claim 1 or 2, wherein The weight average molecular weight Mw of the liquid natural rubber is 100,000 or less.
7. The adhesive tape according to claim 1 or 2, wherein The tackifier is a tackifier derived from plants.
8. The adhesive tape according to claim 7, wherein The plant-derived tackifier is terpene resin.
9. The adhesive tape according to claim 1 or 2, wherein The tackifier is composed of one or more tackifiers having a softening point in the range of 70°C to 150°C.
10. The adhesive tape according to claim 1 or 2, wherein The plant-derived fiber of the substrate is rayon.
11. The adhesive tape according to claim 1 or 2, wherein The olefin resin is a bio-based polyolefin.
12. The adhesive tape according to claim 11, wherein The bio-based polyolefin is bio-based polyethylene.
13. The adhesive tape according to claim 1 or 2, wherein The olefin resin is provided on one side of the substrate, and the adhesive layer is provided on one side of the substrate.
14. The adhesive tape according to claim 13, wherein The olefin resin and the adhesive layer are provided on different surfaces of the substrate.
15. An adhesive tape comprising: a substrate obtained by forming a plant-derived fiber into a woven fabric and laminating an olefin resin on one or both sides of the woven fabric; and An adhesive layer is provided on one or both sides of the substrate, The adhesive layer comprises natural rubber, a wood-based filler, a plant-derived plasticizer, and a tackifier. The plant-derived plasticizer is liquid natural rubber.
16. The adhesive tape according to claim 15, characterized in that An olefin resin is laminated on one surface of the woven fabric, and an adhesive layer is provided on the other surface of the woven fabric.