Plastic pipeline with controllable strength

By using a combination of PE, micro thermal particles and glass fiber reinforced plastic in plastic pipes, the coextrusion process and external heat source to regulate the solidification of the intermediate layer, the problem of different performance requirements in different environments is solved, and the strength controllable is achieved and corrosion resistance, extending service life.

CN118991192APending Publication Date: 2024-11-22ZHEJIANG AKAN IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411197581.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The performance requirements of existing plastic pipes vary greatly in different construction environments, resulting in inconsistent material selection and increased construction costs and it is difficult to maintain stable performance under extreme conditions.

Method used

Using PE material as the inner layer, thermoplastic elastomer with micro-thermal particles as the intermediate layer and glass fiber reinforced plastic as the outer layer, a plastic pipe with controllable strength is prepared through coextrusion process, and the solidification position of the intermediate layer is adjusted by using an external heat source and to improve anti-hydrostatic strength.

Benefits of technology

It realizes controllability of strength in different scenarios, improves the corrosion resistance, high temperature resistance and aging resistance of the pipeline, reduces wear, extends service life, and maintains stable performance under extreme conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118991192A_ABST
    Figure CN118991192A_ABST
Patent Text Reader

Abstract

The invention relates to a plastic pipeline with controllable strength. The preparation process of the strength-controllable plastic pipeline comprises the following steps: liquid phase purification, preparation of an inner-layer UHMWPE material, preparation of PAn / SiO2 composite microspheres, hot melting blending, cooling and granulation, preparation of a thermoplastic elastomer of middle-layer micro thermosensitive particles, preparation of outer-layer glass fiber reinforced plastic (GFRP), co-extrusion and the like. The strength-controllable plastic pipeline prepared through the method can be selectively heated through an external heat source such as infrared rays under the abnormal construction condition, the solidification position and degree of the middle layer are accurately controlled, the middle layer is solidified, the static hydraulic strength is improved, then the strength is controllable, and the strength-controllable plastic pipeline further has the advantages of being good in corrosion resistance, resistant to high temperature, resistant to acid and alkali and long in service life. And the composite material has a wide application prospect in the fields of buildings, water supply and drainage, chemical engineering, medicines and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a plastic pipe with controllable strength, belonging to the field of building materials. Background Art

[0002] With the continuous advancement of science and technology and the acceleration of the industrialization process, plastic pipes, as a new type of pipe, have gradually occupied an important position in the pipeline industry due to their unique performance and wide application fields. At present, plastic pipe systems are widely used, and the performance requirements of pipes in different scenarios are different. This leads to the selection of pipes of specific materials that meet the requirements due to the purpose and pipe performance. Under specific analysis conditions, even the performance requirements of the same pipe in different construction environments are different. For example, in the case of passing through the road, the ring stiffness needs to be stronger, and the hydrostatic strength needs to be higher around the water pump. If pipes of different materials are selected due to similar differences, the construction cost and material cost will increase. In view of this, a plastic pipe with controllable strength is invented, which can be selectively heated by an external heat source such as infrared rays, and the solidification position and degree of the middle layer can be accurately controlled to solidify the middle layer to increase the hydrostatic strength and thus achieve controllable strength and improve the performance of the pipe, so as to meet the use in different scenarios under abnormal conditions and have very good development prospects.

[0003] Controllable strength plastic pipes can be self-reinforced to significantly improve strength and reliability while maintaining advantages such as light weight and easy installation. This allows the pipe to maintain stable performance under extreme conditions such as high pressure and high temperature, ensuring the safe operation of the project. The self-reinforced plastic pipe system uses special materials and processes to make the pipe more corrosion-resistant. Whether in chemical corrosion, electrochemical corrosion or microbial corrosion, it can maintain good performance and extend the service life of the pipe. Summary of the invention

[0004] In order to overcome the above technical problems existing in the prior art, the object of the present invention is to provide a plastic pipe with controllable strength.

[0005] The present invention provides a process for preparing a plastic pipe with controllable strength, which comprises: A plastic pipe with controllable strength is obtained by co-extrusion using PE material as the inner layer material, thermoplastic elastomer of micro heat-sensitive particles as the middle layer material, and outer glass fiber reinforced plastic as the outer layer material.

[0006] Preferably, the PE material is a high-purity inner layer PE (UHMWPE) material.

[0007] Furthermore, the preparation method of the UHMWPE material comprises: Take pure ethylene monomer as raw material, select suitable saturated hydrocarbon as dispersion medium, add appropriate amount of catalyst and ensure that the catalyst is evenly distributed in the reaction system, carry out polymerization reaction under certain reaction conditions, add appropriate amount of lubricant after a period of time and continue the reaction, continue the reaction for a period of time, then separate the polymerized product from the reaction system, dry it, remove residual water and solvent to obtain UHMWPE material, and then obtain high-purity inner layer UHMWPE material through liquid phase purification.

[0008] Further, the ethylene purity percentage is above 99.9%; Further, the dispersion medium includes at least one of heptane, hexane, petroleum ether or kerosene; Further, the mass ratio of the dispersion medium to the ethylene monomer is: (1-2): 1; Further, the catalyst includes a Ziegler catalyst such as TiCl 3 -Al(C 2 H 5 ) 2 Cl, TiCl 4 -Al(C 2 H 5 ) 2 At least one of Cl or a metallocene catalyst; Furthermore, the mass ratio of ethylene monomer to catalyst is 1: 0.002% to 0.006%. The reaction temperature ranges from 70 to 90°C and the reaction pressure ranges from 1 to 1.5 atmospheres; Furthermore, the lubricant includes at least one of stearate, silicone oil or PTFE micropowder; the mass ratio of the lubricant to the ethylene monomer is: (3%~6%):1; Furthermore, the reaction time before adding the lubricant is 1 to 4 h; Furthermore, the temperature range after separation and drying is 40-60°C, and the drying time is 4-10 hours.

[0009] Preferably, the method for preparing the high-purity inner layer UHMWPE material comprises: Use an appropriate solvent, add UHMWPE material into the solvent in a certain proportion, heat and stir to make it fully dissolved, filter it through a filter after a period of time, and add an appropriate amount of decolorizer for decolorization treatment. After treatment, stir and stand it fully, and cool the solution to make UHMWPE precipitate from the solution. After separation, washing and drying, high-purity inner layer UHMWPE material is obtained.

[0010] Further, the solvent includes at least one of decahydronaphthalene and xylene; Furthermore, the mass ratio of solvent to UHMWPE is: (10-20):1; Further, the heating and stirring temperature range is 100~130℃, and the stirring time is 30~60min; Further, the decolorizing agent includes at least one of activated carbon and white clay; Furthermore, the stirring and standing time is 1 to 2 h; Furthermore, the cooling rate is 2.5~10℃ / min, and the target crystallization temperature range is: 85~100℃ Furthermore, the drying temperature ranges from 40 to 60°C.

[0011] Preferably, the method for preparing a thermoplastic elastomer of micro heat-sensitive particles comprises: Take appropriate amount of TPE matrix, PAn / SiO 2 The composite microspheres and poly (N-isopropylacrylamide) are mixed in a certain proportion, and then ball-milled for a period of time. An appropriate amount of silicon micropowder and benzophenone substances are added and ball-milled for a period of time. After ball-milling, the raw materials are sent to a hot melt blender for hot melt blending at a high temperature. After the mixture is finished, the blended material is cooled by a cooling device, and the cooled material is granulated by a granulator, so as to obtain a thermoplastic elastomer material of intermediate layer micro heat-sensitive particles.

[0012] Furthermore, TPE matrix, PAn / SiO 2 The mass ratio of composite microspheres and poly (N-isopropylacrylamide) is: (4-6): (2-3): 1; Furthermore, the initial ball milling time was 1–4 h; Furthermore, the mass ratios of the added silicon micropowder and benzophenone substances to the mixture are: (1-2): 8 and (1-3): 9 respectively; Further, the benzophenone-type substance includes at least one of benzophenone, 2-hydroxy-4-methoxybenzophenone, and oxybenzone (BP3); Furthermore, the ball milling time after adding silicon micropowder and benzophenone substances is: 1~4h; Furthermore, the temperature of hot melt blending is 150-180°C, and the time of hot melt blending is 8-15 minutes; Further, the cooling temperature range is: 20~40℃; Furthermore, the particle size of the granulation is controlled at 3 to 6 mm.

[0013] Preferably, PAn / SiO 2 The preparation method of composite microspheres comprises: Take appropriate amount of polyaniline (PAn) and initiator to mix, take appropriate amount of SiO2 The nanoparticles are uniformly dispersed in the solvent to obtain SiO 2 Nanoparticle dispersion, SiO 2 The dispersion of nanoparticles is added to the mixture of polyaniline (PAn) and initiator, and a polymerization reaction is carried out under appropriate temperature and stirring conditions to obtain PAn / SiO 2 The composite microspheres are then separated by centrifugation, filtration or precipitation, washed with an appropriate solvent, and then dried to obtain PAn / SiO 2 Composite microspheres.

[0014] Further, the initiator includes at least one of ammonium persulfate, ferric chloride, hydrogen peroxide and cerium ammonium nitrate; Further, the mixing ratio of polyaniline (PAn) and initiator is: (7~10):1; Furthermore, SiO 2 Nanoparticles in the dispersion of SiO 2 The mass ratio of nanoparticles to solvent is: (1-4):1; Furthermore, the preparation of SiO 2 The solvent of the nanoparticle dispersion includes at least one of water or ethanol; Furthermore, the solution of polyaniline (PAn) and initiator is mixed with SiO 2 The mass ratio of the dispersion of nanoparticles is: (1-5): 1; Furthermore, the polymerization reaction temperature is 25-40°C; the reaction time is 6-12 hours; the pH value of the reaction system is 4-6; Further, the washing solvent includes at least one of ethanol, acetone and deionized water; Furthermore, the drying temperature is 30-50°C.

[0015] Preferably, the method for preparing the outer layer of glass fiber reinforced plastic (GFRP) comprises: Take an appropriate amount of high-strength glass fiber and soak it in a resin matrix. After a certain period of time, pour the soaked glass fiber and resin mixture into a mold, and shape it through pressurization, heating and other process means to obtain an outer layer of glass fiber reinforced plastic (GFRP).

[0016] Furthermore, the tensile strength of high-strength glass fiber is 1500~4000MPa and the elastic modulus is 25-500MPa / mm 2 , bending strength is 2000~5000MPa; Furthermore, the mass ratio of glass fiber to resin matrix is: 1:(2~3); Further, the resin matrix includes at least one of epoxy resin, polyester resin, vinyl ester resin and unsaturated polyester resin; Furthermore, the pressure during the molding process is 10-20 MPa, the molding temperature is 150-200° C., and the molding time is 6-9 h.

[0017] Preferably, the method for preparing a plastic pipe with controllable strength comprises: The inner layer UHMWPE material, the middle layer thermoplastic elastomer material of micro-thermosensitive particles, and the outer layer glass fiber reinforced plastic (GFRP) material are placed at the feed port of the extruder in a certain mass ratio, heated and melted respectively, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength.

[0018] Furthermore, the mass ratio of the inner layer UHMWPE material, the middle layer thermoplastic elastomer material of micro thermosensitive particles, and the outer layer glass fiber reinforced plastic (GFRP) material is: (1~3): (6~7): (1~3); Further, the temperature range of the feed port section is: 100~120°C, the temperature range of the feed zone heating section is: 120~150°C, the temperature range of the screw zone heating section is 150~180°C, the temperature range of the barrel zone heating section is 180~200°C, and the temperature range of the die head heating section is 200-220°C; Furthermore, the discharging speed of the co-dose is 2.5~3.5 m / min.

[0019] The present invention prepares a plastic pipe with controllable strength, which has the advantages of controllable strength, good corrosion resistance, high temperature resistance, acid and alkali resistance, strong anti-aging ability, etc., and has broad application prospects in multiple fields such as construction, water supply and drainage, chemical industry, and medicine.

[0020] In summary, the beneficial effects of the present invention are: In this method, UHMWPE material is used as the inner layer material of the plastic pipe with controllable strength. The UHMWPE material has excellent wear resistance, which can significantly reduce wear and extend the service life. The UHMWPE has high impact strength, and its impact resistance enables the pipe to effectively resist damage when it is impacted, thereby ensuring the stability and safety of the pipe. The UHMWPE has an extremely low friction coefficient and excellent self-lubricating property, and its self-lubricating property can reduce the resistance of the pipe when conveying materials and improve the conveying efficiency.

[0021] In this method, a thermoplastic elastomer with micro-thermosensitive particles is used as the main material of the middle layer. The thermoplastic elastomer with micro-thermosensitive particles can be selectively heated by using an external heat source to precisely control the solidification position and degree of the middle layer to solidify the middle layer to increase the hydrostatic strength. The thermoplastic elastomer itself has excellent elasticity, weather resistance and chemical resistance. After combining with micro-thermosensitive particles, these properties can be further enhanced. The addition of micro-thermosensitive particles may also improve the wear resistance, aging resistance and impact resistance of TPE, thereby enhancing the overall performance and service life of the pipeline.

[0022] In this method, glass fiber reinforced plastic (GFRP) material is used as the outer material of the plastic pipe with controllable strength, wherein GFRP combines the high strength and high modulus of glass fiber with the light weight and easy processing of plastic. The addition of glass fiber significantly improves the tensile, compressive and bending strength of the material, allowing the pipe to withstand greater external loads and maintain stable structural performance; the high modulus of GFRP enables the pipe to maintain good shape stability when subjected to stress, reducing the risk of deformation and damage; GFRP has good corrosion resistance and weather resistance, and can maintain stable performance in harsh environments; GFRP also has good thermal insulation and fire resistance, and can effectively prevent the spread of fire; the use of glass fiber reinforced plastic (GFRP) material can effectively protect the inner structure of the pipe, enhance the overall strength, and can increase the service life of the pipe and improve safety performance.

[0023] In this method, a plastic pipe with controllable strength is prepared by using an inner layer of UHMWPE material, a middle layer of thermoplastic elastomer material with micro-thermosensitive particles, and an outer layer of glass fiber reinforced plastic (GFRP). The inner layer of UHMWPE material provides excellent wear resistance and impact resistance, ensuring the durability of the inside of the pipe; the middle layer of thermoplastic elastomer material with micro-thermosensitive particles allows the pipe to adjust its strength according to temperature changes to achieve controllability; the outer layer of GFRP provides high strength and light weight, while ensuring the corrosion resistance and structural stability of the pipe. Both UHMWPE and GFRP have excellent corrosion resistance and can effectively resist chemical corrosion and erosion in harsh environments; the middle layer of thermoplastic elastomer material contains micro-thermosensitive particles, which can respond quickly according to temperature changes, and can achieve comprehensive advantages such as adjustable overall strength of the pipe.

[0024] Therefore, the controllable strength plastic pipe provided by the present invention has the ability to be selectively heated by an external heat source such as infrared rays under abnormal construction conditions, accurately control the solidification position and degree of the middle layer, solidify the middle layer to increase the anti-static hydraulic strength and thus achieve controllable strength, and also has the advantages of good corrosion resistance, high temperature resistance, acid and alkali resistance, strong anti-aging ability, etc., and has broad application prospects in construction, water supply and drainage, chemical industry, medicine and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The present invention is a flow chart for preparing a plastic pipe with controlled strength. DETAILED DESCRIPTION

[0026] To make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0027] The present invention provides a preparation process of a hard carbon composite material, which specifically comprises the following steps: Step (1) Preparation of UHMWPE material S11 Take an appropriate amount of pure ethylene monomer as raw material, take an appropriate amount of hexane as dispersion medium, add an appropriate amount of catalyst TiCl 3 -Al(C 2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 undergoes polymerization reaction at a certain temperature and a certain atmospheric pressure for a certain time; S13 continues to add an appropriate amount of PTFE powder as a lubricant and then continues the reaction for a certain period of time; S14 After the reaction is completed, the polymerized product is separated from the reaction system, and dried to remove residual water and solvent to obtain UHMWPE material; Preferably, step (1) of preparing the UHMWPE material comprises the following steps: S11: taking 10-20 g of pure ethylene monomer as a raw material, taking 20-40 ml of hexane as a dispersion medium, and adding 5-10 mg of a catalyst TiCl 3 -Al(C 2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 performs polymerization reaction at a temperature of 70-90°C and a pressure of 1-1.5 atmospheres for 1-4 hours; S13 continues to add 0.3-0.6 g PTFE micropowder as a lubricant and then continues the reaction for 2-8 hours; S14 separates the polymerized product from the reaction system after the reaction is completed, and dries it at a temperature range of 40-60°C for a drying time of 4-10 hours to remove residual moisture and solvent to obtain UHMWPE material.

[0028] In this method, the UHMWPE material used has excellent wear resistance, can significantly reduce wear and extend service life; the impact strength of UHMWPE is about 2 times that of impact-resistant PC, 5 times that of ABS, and more than 10 times that of POM and PBTP. This impact resistance enables the pipeline to effectively resist damage when it is impacted, ensuring the stability and safety of the pipeline; UHMWPE has an extremely low friction coefficient (0.05~0.11) and excellent self-lubrication. Its lubricity in sliding or rotating form is even better than that of steel and brass with added lubricating oil. This self-lubricity can reduce the resistance of the pipeline when conveying materials and improve the conveying efficiency. The PTFE powder added during the preparation process can further enhance the lubrication effect and form a continuous lubrication layer inside the UHMWPE material, reduce the friction coefficient, and improve the lubrication effect; the wear resistance of PTFE micropowder can significantly improve the wear resistance of UHMWPE material and extend its service life.

[0029] Step (2) Liquid phase purification of UHMWPE materials S21 takes a certain amount of decahydronaphthalene as a solvent, adds a certain amount of UHMWPE material, heats for a certain period of time, stirs to fully dissolve it, and then filters it through a filter; S22 and adding an appropriate amount of decolorizing agent to perform decolorization treatment, and then fully stirring and standing the mixture; S23: cooling the solution so that UHMWPE is precipitated from the solution, and obtaining a high-purity inner layer UHMWPE material after separation, washing and drying; Preferably, the liquid phase purification step of the UHMWPE material in step (2) comprises: S21 taking 100-140 ml of decahydronaphthalene as a solvent, adding 10-14 g of UHMWPE material, heating to 100-130° C., stirring for 1-2 h to fully dissolve it, and then filtering it through a filter; S22 adding 1-5 g of a decolorizing agent for decolorization treatment, and after the treatment, fully stirring and standing for 1-2 h; S23 cooling the solution at a cooling rate of 2.5-10° C. / min in a temperature range of 85-100° C., so that UHMWPE is precipitated from the solution, and after separation, washing and drying, a high-purity inner layer UHMWPE material is obtained.

[0030] In this method, the prepared UHMWPE material is subjected to liquid phase purification to obtain a high-purity inner layer UHMWPE material. Liquid phase purification can remove impurities and unreacted products in the UHMWPE material, thereby improving the purity of the material. This helps to ensure that the UHMWPE material has more stable physical and chemical properties; the crystallinity, tensile strength, impact strength and other properties of the UHMWPE material can be improved; liquid phase purification can change the molecular structure and morphology of the UHMWPE material, thereby optimizing its structure.

[0031] Step (3) PAn / SiO 2 Preparation of composite microspheres S31 Take an appropriate amount of polyaniline (PAn) and ammonium persulfate and mix; S32 Take appropriate amount of SiO 2 The nanoparticles were uniformly dispersed in the ethanol solution to obtain SiO 2 dispersion of nanoparticles; S33 SiO 2 The dispersion of nanoparticles was added to the mixture of polyaniline (PAn) and ammonium persulfate, and the polymerization reaction was carried out for 6-12 hours under certain conditions to obtain PAn / SiO 2 Composite microspheres; S34 was separated by centrifugation, filtration or precipitation, and the composite microspheres were washed with acetone and dried to obtain PAn / SiO 2 Composite microspheres; Preferably, step (3) PAn / SiO 2 The preparation steps of the composite microspheres include: S31 taking 7-10 g of polyaniline (PAn) and 1-2 g of ammonium persulfate and mixing them; S32 taking 15-21 g of SiO 2 The nanoparticles were evenly dispersed in 8-12 ml of ethanol solution to obtain SiO 2 Nanoparticle dispersion; S33 SiO 2 The dispersion of nanoparticles was added to a mixture of polyaniline (PAn) and ammonium persulfate, and the polymerization reaction was carried out at a temperature of 25-40°C and a pH value of 4-6 for 6-12 hours to obtain PAn / SiO 2 The composite microspheres; S34 are separated by centrifugation, filtration or precipitation, washed with 100-200 ml of acetone, and dried at 30-50 °C to obtain PAn / SiO 2 Composite microspheres.

[0032] In this method, PAn / SiO 2 The composite microspheres are the main micro thermosensitive particles in the thermoplastic elastomer of the intermediate layer micro thermosensitive particles. The advantage is that PAn / SiO 2 The composite microspheres can undergo significant changes within a specific temperature range, expanding or contracting in volume, thereby achieving a rapid response to temperature changes. This excellent thermal sensitivity enables the middle layer to quickly adjust its physical properties when the temperature changes to adapt to the use requirements under different environmental conditions; PAn / SiO 2 The composite microspheres themselves have high strength and toughness. Adding them to thermoplastic elastomers can significantly improve the mechanical properties of the middle layer; PAn / SiO 2The composite microspheres have good dispersibility and compatibility in the thermoplastic elastomer and can be evenly distributed in the entire middle layer to avoid the formation of agglomeration or local concentration.

[0033] Step (4) Preparation of thermoplastic elastomer of micro thermosensitive particles S41 Take appropriate amount of TPE matrix, PAn / SiO 2 The composite microspheres and poly (N-isopropylacrylamide) are mixed and ball-milled; S42 continues to add silicon micropowder and benzophenone substances and continue ball milling; S43 After the ball milling treatment, the raw materials are sent to a hot melt blender for hot melt blending at high temperature. After the blending is completed, the blended materials are cooled by a cooling device, and the cooled materials are granulated by a granulator to obtain a thermoplastic elastomer material of intermediate layer micro heat-sensitive particles; Preferably, the step (4) of preparing the thermoplastic elastomer of the micro thermosensitive particles comprises: S41 taking 40-55 g of TPE matrix, 20-28 g of PAn / SiO 2 The composite microspheres are mixed with 10-13g of poly (N-isopropylacrylamide) and ball-milled for 1-4h; S42 continues to add 6-9g of silicon micropowder and 6-9g of 2-hydroxy-4-methoxybenzophenone, and continues ball-milling for 1-4h; S43 after ball-milling, the raw materials are sent to a hot-melt blender for hot-melt blending at a high temperature of 150-180°C for 8-15min. After the blending, the blended material is cooled at 20-40°C by a cooling device, and the cooled material is granulated by a granulator to obtain a thermoplastic elastomer material with 3-6mm intermediate layer micro-thermosensitive particles.

[0034] In this method, the TPE matrix gives the pipeline high elasticity and flexibility, allowing the pipeline to maintain its shape and function under different environmental conditions; poly N-isopropylacrylamide (PNIPAm) is a temperature-responsive polymer that can adjust the strength and elasticity of the pipeline as needed to adapt to different temperature conditions. This thermal sensitivity regulation enables the pipeline to automatically adjust its performance when the temperature changes, enhancing the adaptability and reliability of the pipeline. 2 Thermoplastic elastomers of micro-thermosensitive particles prepared from composite microspheres and poly (N-isopropylacrylamide) can improve the performance, adaptability and reliability of pipelines. This combination of materials not only has excellent physical properties and thermal sensitivity regulation capabilities, but also has controllable strength, which can meet the needs of different application scenarios.

[0035] Step (5) Preparation of outer layer glass fiber reinforced plastic (GFRP) material Take an appropriate amount of high-strength glass fiber and soak it in a resin matrix. After a certain period of time, pour the soaked glass fiber and resin mixture into a mold and shape it by pressurizing, heating and other process means to obtain an outer layer of glass fiber reinforced plastic (GFRP); Preferably, the preparation steps of the outer layer of glass fiber reinforced plastic (GFRP) include: taking 8~14g of high-strength glass fiber, impregnating it in 20~40ml of epoxy resin, pouring the impregnated glass fiber and resin mixture into a mold after 1~4 hours, and molding it by pressurizing 10~20MPa, heating 150~200℃ and other process means to obtain the outer layer of glass fiber reinforced plastic (GFRP).

[0036] This method uses high-strength glass fiber as a reinforcing material, which significantly improves the tensile, compressive and flexural strength of GFRP. This makes GFRP perform well in situations where it needs to withstand large loads; the addition of high-strength glass fiber also increases the modulus of GFRP accordingly. Modulus is the ability of a material to resist deformation when subjected to force; epoxy resin, as a plastic matrix, usually has good corrosion resistance. This allows GFRP to maintain good performance in harsh environments such as moisture, acid and alkali, and extend its service life.

[0037] Step (6) Preparation of plastic pipe with controllable strength S61 takes the inner layer UHMWPE material, the middle layer thermoplastic elastomer material of micro heat-sensitive particles, and the outer layer glass fiber reinforced plastic (GFRP) material and places them at the feed port of the extruder respectively; S62 heats and melts the three layers separately, and then co-extrudes the three layers of material through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength.

[0038] Preferably, the preparation of the controllable strength plastic pipe in step (6) comprises: S61 taking 10-16 g of the inner layer UHMWPE material, 20-32 g of the middle layer thermoplastic elastomer material of micro-thermosensitive particles, and 10-16 g of the outer layer glass fiber reinforced plastic (GFRP) material and placing them at the feed port of the extruder respectively; S62 heating and melting them respectively, and then co-extruding the three layers of materials through a three-layer co-extrusion die to obtain a controllable strength plastic pipe, wherein the feed port section temperature range is: 100-120°C, the feed zone heating section temperature range is: 120-150°C, the screw zone heating section temperature range is: 150-180°C, the barrel zone heating section temperature range is: 180-200°C, and the die head heating section temperature range is 200-220°C.

[0039] In the present method, a co-extrusion method is used to prepare a plastic pipe with controllable strength. The co-extrusion technology allows three different materials to be formed at one time, thereby improving production efficiency and reducing production costs. Through high-temperature heating and extrusion, each layer of material is tightly combined and not easy to be delaminated, thereby ensuring the overall performance of the pipe. By adjusting the ratio and formula of each layer of material, the performance of the pipe, such as strength, toughness, corrosion resistance, etc., can be accurately controlled. Example 1

[0040] The present invention provides a preparation process of a hard carbon composite material, which specifically comprises the following steps: Step (1) Preparation of UHMWPE material S11 Take 10g of pure ethylene monomer as raw material, take 20ml of hexane as dispersion medium, add 5mg of catalyst TiCl 3 -Al(C 2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 was polymerized at 70 °C and 1 atm for 1 h; S13 continued to add 0.3 g PTFE powder as a lubricant and continued the reaction for 2 h; After the reaction is completed, the polymerized product is separated from the reaction system and dried at a temperature of 40° C. for 4 h to remove residual water and solvent to obtain a UHMWPE material. Step (2) Liquid phase purification of UHMWPE materials S21 Take 100 ml of decahydronaphthalene as solvent, add 10 g of UHMWPE material, heat to 100 ° C, stir for 1 hour to make it fully dissolved, and then filter through a filter; S22 and add 1g of decolorizing agent for decolorization, and then stir and stand for 1h; S23: cooling the solution at a rate of 2.5-4°C / min within a temperature range of 85°C, so that UHMWPE is precipitated from the solution, and a high-purity inner layer UHMWPE material is obtained after separation, washing and drying; Step (3) PAn / SiO 2 Preparation of composite microspheres S31 Take an appropriate amount of 7g polyaniline (PAn) and 1g ammonium persulfate and mix them; S32 takes 15gSiO 2 The nanoparticles were evenly dispersed in 8 ml of ethanol solution to obtain SiO 2 dispersion of nanoparticles; S33 SiO 2The dispersion of nanoparticles was added to a mixture of polyaniline (PAn) and ammonium persulfate, and the polymerization reaction was carried out at 25 °C and pH 4 for 6 h to obtain PAn / SiO 2 Composite microspheres; S34 was separated by centrifugation, filtration or precipitation, and the composite microspheres were washed with 100 ml of acetone and dried at 30 °C to obtain PAn / SiO 2 Composite microspheres; Step (4) Preparation of thermoplastic elastomer of micro thermosensitive particles S41 Take appropriate amount of 40g TPE matrix, 20g PAn / SiO 2 The composite microspheres were mixed with 10 g of poly (N-isopropylacrylamide) and ball-milled for 1 h; S42 continued to add 6 g of silicon powder and 6 g of 2-hydroxy-4-methoxybenzophenone, and continued ball milling for 1 h; S43 After the ball milling treatment, the raw materials are sent to a hot melt blender for hot melt blending at a high temperature of 150° C. The hot melt blending time is 8 minutes. After the blending is completed, the blended material is cooled at 20° C. by a cooling device, and the cooled material is granulated by a granulator to obtain a thermoplastic elastomer material with 3 mm intermediate layer micro heat-sensitive particles; Step (5) Preparation of outer layer glass fiber reinforced plastic (GFRP) Take 8g of high-strength glass fiber and soak it in 20ml of epoxy resin. After 1 hour, pour the soaked glass fiber and resin mixture into a mold and mold it by pressurizing it to 10MPa and heating it to 150℃ to obtain an outer layer of glass fiber reinforced plastic (GFRP). Step (6) Preparation method of plastic pipe with controllable strength S61 Take 10g of inner layer UHMWPE material, 20g of middle layer micro thermosensitive particle thermoplastic elastomer material, and 10g of outer layer glass fiber reinforced plastic (GFRP) material and place them at the feed port of the extruder respectively; S62 is heated and melted respectively, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength, wherein the temperature range of the feed port section is: 100°C, the temperature range of the feed zone heating section is: 120°C, the temperature range of the screw zone heating section is: 150°C, the temperature range of the barrel zone heating section is: 180°C, and the temperature range of the die head heating section is 200°C. Example 2

[0041] Step (1) Preparation of UHMWPE material S11 Take 13g of pure ethylene monomer as raw material, take 25ml of hexane as dispersion medium, add 6mg of catalyst TiCl 3 -Al(C2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 was polymerized at 75 °C and 1.1 atm for 2 h; S13 continued to add 0.4 g PTFE powder as a lubricant and continued the reaction for 4 h; After the reaction is completed in S14, the polymerized product is separated from the reaction system, and dried at a temperature range of 45° C. for 6 h to remove residual moisture and solvent to obtain a UHMWPE material; Step (2) Liquid phase purification of UHMWPE materials S21 Take 110 ml of decahydronaphthalene as solvent, add 11 g of UHMWPE material, heat to 110 ° C, stir for 1.3 hours to make it fully dissolved, and then filter through a filter; S22 and add 2g of decolorizing agent for decolorization treatment, and then stir and stand for 1.3h; S23: cooling the solution at a cooling rate of 3°C / min within a temperature range of 90°C, so that UHMWPE is precipitated from the solution, and a high-purity inner layer UHMWPE material is obtained after separation, washing, and drying; Step (3) PAn / SiO 2 Preparation of composite microspheres S31 Take appropriate amount of 8g polyaniline (PAn) and 1.3g ammonium persulfate and mix; S32 takes 17gSiO 2 The nanoparticles were evenly dispersed in 9 ml of ethanol solution to obtain SiO 2 dispersion of nanoparticles; S33 SiO 2 The dispersion of nanoparticles was added to the mixture of polyaniline (PAn) and initiator, and the polymerization reaction was carried out at 30 °C and pH 4.5 for 8 h to obtain PAn / SiO 2 Composite microspheres; S34 was separated by centrifugation, filtration or precipitation, and the composite microspheres were washed with 130 ml of acetone and dried at 35 °C to obtain PAn / SiO 2 Composite microspheres; Step (4) Preparation of thermoplastic elastomer of micro thermosensitive particles S41 Take appropriate amount of 45g TPE matrix, 22g PAn / SiO 2 The composite microspheres were mixed with 11 g of poly (N-isopropylacrylamide) and ball-milled for 2 h; S42 continued to add 7 g of silicon powder and 7 g of 2-hydroxy-4-methoxybenzophenone, and continued ball milling for 2 h; S43 After the ball milling treatment, the raw materials are sent to a hot melt blender for hot melt blending at a high temperature of 160° C. The hot melt blending time is 10 minutes. After the blending is completed, the blended material is cooled at 25° C. by a cooling device, and the cooled material is granulated by a granulator to obtain a thermoplastic elastomer material with a 4 mm intermediate layer micro heat-sensitive particles; Step (5) Preparation of outer layer glass fiber reinforced plastic (GFRP) Take 10g of high-strength glass fiber and soak it in 25ml of epoxy resin. After 2 hours, pour the soaked glass fiber and resin mixture into a mold and form it by pressurizing it to 13MPa and heating it to 160℃ to obtain an outer layer of glass fiber reinforced plastic (GFRP). Step (6) Preparation method of plastic pipe with controllable strength S61 Take 12g of inner layer UHMWPE material, 23g of middle layer micro thermosensitive particle thermoplastic elastomer material, and 12g of outer layer glass fiber reinforced plastic (GFRP) material and place them at the feed port of the extruder respectively; S62 is heated and melted respectively, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength, wherein the temperature range of the feed port section is: 105°C, the temperature range of the feed zone heating section is: 130°C, the temperature range of the screw zone heating section is: 160°C, the temperature range of the barrel zone heating section is 185°C, and the temperature range of the die head heating section is 205°C. Example 3

[0042] Step (1) Preparation of UHMWPE material S11 Take 16g of pure ethylene monomer as raw material, take 30ml of hexane as dispersion medium, add 7mg of catalyst TiCl 3 -Al(C 2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 was polymerized at 80 °C and 1.2 atm for 3 h; S13 continued to add 0.5 g PTFE powder as a lubricant and continued the reaction for 6 h; S14 After the reaction is completed, the polymerized product is separated from the reaction system, and dried at a temperature range of 50° C. for 8 hours to remove residual moisture and solvent to obtain UHMWPE material; Step (2) Liquid phase purification of UHMWPE materials S21 Take 130 ml of decahydronaphthalene as solvent, add 12 g of UHMWPE material, heat to 120 ° C, stir for 1.6 hours to make it fully dissolved, and then filter through a filter; S22 and add 3g of decolorizing agent for decolorization treatment, and then stir and stand for 1.6h; S23: cooling the solution at a cooling rate of 3.5°C / min within a temperature range of 95°C, so that UHMWPE is precipitated from the solution, and a high-purity inner layer UHMWPE material is obtained after separation, washing, and drying; Step (3) PAn / SiO 2 Preparation of composite microspheres S31 Take an appropriate amount of 9g polyaniline (PAn) and 1.6g ammonium persulfate and mix them; S32 takes 19gSiO 2 The nanoparticles were evenly dispersed in 10 ml of ethanol solution to obtain SiO 2 dispersion of nanoparticles; S33 SiO 2 The dispersion of nanoparticles was added to the mixture of polyaniline (PAn) and initiator, and the polymerization reaction was carried out at 35 °C and pH 5 for 10 h to obtain PAn / SiO 2 Composite microspheres; S34 was separated by centrifugation, filtration or precipitation, and the composite microspheres were washed with 160 ml of acetone and dried at 45 °C to obtain PAn / SiO 2 Composite microspheres; Step (4) Preparation of thermoplastic elastomer of micro thermosensitive particles S41 Take appropriate amount of 50g TPE matrix, 26g PAn / SiO 2 The composite microspheres were mixed with 12 g of poly (N-isopropylacrylamide) and ball-milled for 3 h; S42 continued to add 8 g of silicon powder and 8 g of 2-hydroxy-4-methoxybenzophenone, and continued ball milling for 3 h; S43 After the ball milling treatment, the raw materials are sent to a hot melt blender for hot melt blending at a high temperature of 150-180°C for 13 minutes. After the hot melt blending is completed, the blended materials are cooled at 35°C by a cooling device, and the cooled materials are granulated by a granulator to obtain a thermoplastic elastomer material with 5 mm intermediate layer micro heat-sensitive particles; Step (5) Preparation of outer layer glass fiber reinforced plastic (GFRP) Take 12g of high-strength glass fiber and soak it in 35ml of epoxy resin. After 3 hours, pour the soaked glass fiber and resin mixture into a mold and form it by pressurizing it to 16MPa and heating it to 180℃ to obtain an outer layer of glass fiber reinforced plastic (GFRP). Step (6) Preparation method of plastic pipe with controllable strength S61 Take 14g of inner layer UHMWPE material, 28g of middle layer thermoplastic elastomer material of micro heat-sensitive particles, and 15g of outer layer glass fiber reinforced plastic (GFRP) material and place them at the feed port of the extruder respectively; S62 is heated and melted respectively, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength, wherein the temperature range of the feed port section is: 115°C, the temperature range of the feed zone heating section is: 140°C, the temperature range of the screw zone heating section is: 170°C, the temperature range of the barrel zone heating section is 190°C, and the temperature range of the die head heating section is 215°C. Example 4

[0043] Step (1) Preparation of UHMWPE material S11 Take 20g of pure ethylene monomer as raw material, take 40ml of hexane as dispersion medium, add 10mg of catalyst TiCl 3 -Al(C 2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 was polymerized at 90 °C and 1.5 atm for 4 h; S13 continued to add 0.6 g PTFE powder as a lubricant and continued the reaction for 8 h; After the reaction is completed, the polymerized product is separated from the reaction system, and dried at a temperature of 60° C. for 10 h to remove residual water and solvent to obtain a UHMWPE material. Step (2) Liquid phase purification of UHMWPE materials S21 Take 140 ml of decahydronaphthalene as solvent, add 14 g of UHMWPE material, heat to 130 ° C, stir for 2 hours to make it fully dissolved, and then filter through a filter; S22 and add 5g of decolorizing agent for decolorization treatment, and then stir and stand for 2h; S23: cooling the solution at a cooling rate of 4°C / min within a temperature range of 100°C, so that UHMWPE is precipitated from the solution, and a high-purity inner layer UHMWPE material is obtained after separation, washing, and drying; Step (3) PAn / SiO 2Preparation of composite microspheres S31 Take appropriate amount of 10g polyaniline (PAn) and 2g ammonium persulfate and mix them; S32 takes 21gSiO 2 The nanoparticles were evenly dispersed in 12 ml of ethanol solution to obtain SiO 2 dispersion of nanoparticles; S33 SiO 2 The dispersion of nanoparticles was added to the mixture of polyaniline (PAn) and initiator, and the polymerization reaction was carried out at 40 °C and pH 6 for 12 h to obtain PAn / SiO 2 Composite microspheres; S34 was separated by centrifugation, filtration or precipitation, and the composite microspheres were washed with 200 ml of acetone and dried at 50 °C to obtain PAn / SiO 2 Composite microspheres; Step (4) Preparation of thermoplastic elastomer of micro thermosensitive particles S41 Take appropriate amount of 55g TPE matrix, 28g PAn / SiO 2 The composite microspheres were mixed with 13 g of poly (N-isopropylacrylamide) and ball-milled for 4 h; S42 continued to add 9 g of silicon powder and 9 g of 2-hydroxy-4-methoxybenzophenone, and continued ball milling for 4 h; S43 After the ball milling treatment, the raw materials are sent to a hot melt blender for hot melt blending at a high temperature of 180° C. The hot melt blending time is 15 minutes. After the blending is completed, the blended material is cooled at 40° C. by a cooling device, and the cooled material is granulated by a granulator to obtain a thermoplastic elastomer material with 6 mm intermediate layer micro heat-sensitive particles; Step (5) Preparation of outer layer glass fiber reinforced plastic (GFRP) Take 14g of high-strength glass fiber and soak it in 40ml of epoxy resin. After 4 hours, pour the soaked glass fiber and resin mixture into a mold and shape it by pressurizing it to 20MPa and heating it to 200℃ to obtain an outer layer of glass fiber reinforced plastic (GFRP). Step (6) Preparation method of plastic pipe with controllable strength S61 Take 16g of inner layer UHMWPE material, 32g of middle layer micro thermosensitive particle thermoplastic elastomer material, and 16g of outer layer glass fiber reinforced plastic (GFRP) material and place them at the feed port of the extruder respectively; S62 is heated and melted respectively, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength, wherein the temperature range of the feed port section is: 120°C, the temperature range of the feed zone heating section is: 150°C, the temperature range of the screw zone heating section is: 180°C, the temperature range of the barrel zone heating section is 200°C, and the temperature range of the die head heating section is 220°C. Comparative Example 1

[0044] Step (1) Preparation of UHMWPE material S11 Take 10g of pure ethylene monomer as raw material, take 20ml of hexane as dispersion medium, add 5mg of catalyst TiCl 3 -Al(C 2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 was polymerized at 70 °C and 1 atm for 1 h; After the reaction is completed in S13, the polymerized product is separated from the reaction system, and dried at a temperature range of 40° C. for 4 h to remove residual moisture and solvent to obtain a UHMWPE material; Step (2) PAn / SiO 2 Preparation of composite microspheres S21 Take an appropriate amount of 7g polyaniline (PAn) and 1g ammonium persulfate and mix; S22 takes 15gSiO 2 The nanoparticles were evenly dispersed in 8 ml of ethanol solution to obtain SiO 2 dispersion of nanoparticles; S23 SiO 2 The dispersion of nanoparticles was added to a mixture of polyaniline (PAn) and ammonium persulfate, and the polymerization reaction was carried out at 25 °C and pH 4 for 6 h to obtain PAn / SiO 2 Composite microspheres; S24 was separated by centrifugation, filtration or precipitation, and the composite microspheres were washed with 100 ml of acetone and dried at 30 °C to obtain PAn / SiO 2 Composite microspheres; Step (3) Preparation of thermoplastic elastomer of micro thermosensitive particles S31 Take appropriate amount of 40g TPE matrix, 20g PAn / SiO 2 The composite microspheres were mixed with 10 g of poly (N-isopropylacrylamide) and ball-milled for 1 h; S32 After the ball milling treatment, the raw materials are sent to a hot melt blender for hot melt blending at a high temperature of 150°C for 8 minutes. After the hot melt blending is completed, the blended materials are cooled at 20°C by a cooling device, and the cooled materials are granulated by a granulator to obtain a thermoplastic elastomer material with a 3 mm intermediate layer of micro heat-sensitive particles; Step (4) Preparation of outer layer glass fiber reinforced plastic (GFRP) Take 8g of glass fiber and soak it in 20ml of epoxy resin. After 1 hour, pour the soaked glass fiber and resin mixture into a mold and shape it by pressurizing it to 10MPa and heating it to 150℃ to obtain an outer layer of glass fiber reinforced plastic (GFRP). Step (5) Preparation method of plastic pipe with controllable strength S51 takes 10g of inner layer UHMWPE material, 20g of middle layer thermoplastic elastomer material of micro heat-sensitive particles, and 10g of outer layer glass fiber reinforced plastic (GFRP) material and puts them in the feed port of the extruder respectively; S52 is heated and melted respectively, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength, wherein the temperature range of the feed port section is: 100°C, the temperature range of the feed zone heating section is: 120°C, the temperature range of the screw zone heating section is: 150°C, the temperature range of the barrel zone heating section is: 180°C, and the temperature range of the die head heating section is 200°C. Comparative Example 2

[0045] Step (1) Preparation of UHMWPE material S11 Take 20g of pure ethylene monomer as raw material, take 40ml of hexane as dispersion medium, add 10mg of catalyst TiCl 3 -Al(C 2 H 5 ) 2 Cl and ensure that the catalyst is evenly distributed in the reaction system; S12 was polymerized at 90 °C and 1.5 atm for 4 h; After the reaction is completed in S13, the polymerized product is separated from the reaction system, and dried at a temperature range of 60° C. for 10 h to remove residual water and solvent to obtain a UHMWPE material; Step (2) PAn / SiO 2 Preparation of composite microspheres S21 Take appropriate amount of 10g polyaniline (PAn) and 2g ammonium persulfate and mix; S22 takes 21gSiO 2 The nanoparticles were evenly dispersed in 12 ml of ethanol solution to obtain SiO 2dispersion of nanoparticles; S23 SiO 2 The dispersion of nanoparticles was added to the mixture of polyaniline (PAn) and initiator, and the polymerization reaction was carried out at 40 °C and pH 6 for 12 h to obtain PAn / SiO 2 Composite microspheres; S24 was separated by centrifugation, filtration or precipitation, and the composite microspheres were washed with 200 ml of acetone and dried at 50 °C to obtain PAn / SiO 2 Composite microspheres; Step (3) Preparation of thermoplastic elastomer of micro thermosensitive particles S31 Take appropriate amount of 55g TPE matrix, 28g PAn / SiO 2 The composite microspheres were mixed with 13 g of poly (N-isopropylacrylamide) and ball-milled for 4 h; S32 After the ball milling treatment, the raw materials are sent to a hot melt blender for hot melt blending at a high temperature of 180°C for 15 minutes. After the hot melt blending is completed, the blended materials are cooled at 40°C by a cooling device, and the cooled materials are granulated by a granulator to obtain a thermoplastic elastomer material with 6 mm intermediate layer micro heat-sensitive particles; Step (4) Preparation of outer layer glass fiber reinforced plastic (GFRP) Take 14g of glass fiber and soak it in 40ml of epoxy resin. After 4 hours, pour the soaked glass fiber and resin mixture into a mold and shape it by pressurizing it to 20MPa and heating it to 200℃ to obtain an outer layer of glass fiber reinforced plastic (GFRP). Step (5) Preparation method of plastic pipe with controllable strength S51 takes 16g of inner layer UHMWPE material, 32g of middle layer thermoplastic elastomer material of micro heat-sensitive particles, and 16g of outer layer glass fiber reinforced plastic (GFRP) material and puts them in the feed port of the extruder respectively; S52 is heated and melted respectively, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength, wherein the temperature range of the feed port section is: 120°C, the temperature range of the feed zone heating section is: 150°C, the temperature range of the screw zone heating section is: 180°C, the temperature range of the barrel zone heating section is 200°C, and the temperature range of the die head heating section is 220°C.

[0046] The controllable strength plastic pipes obtained in Examples 1-4 and the products of Comparative Examples 1-2 were tested, and the specific testing methods are as follows: Static pressure strength test An SH61-A gas-fired infrared radiator was used to provide a stable external infrared heat source to heat the plastic pipes of Examples 1-4 and Comparative Examples 1-2, and an MPX5700AP pressure sensor was used to record the static pressure resistance during the test.

[0047] Corrosion resistance test The plastic pipes of Examples 1-4 and Comparative Examples 1-2 were subjected to corrosion resistance tests using 30% by mass concentrated sulfuric acid and 4 mol / L sodium hydroxide, and their weight losses were recorded.

[0048] Wear resistance test According to the QB / T 5101-2017 test standard, an M-200 sliding friction and wear tester was used to test the plastic pipes of Examples 1-4 and Comparative Examples 1-2 under a load of 20 N and a sliding speed of 1 m / s for 30 minutes, and the wear quality of the corresponding plastic pipes was recorded.

[0049] Table 1 Static pressure strength test results

[0050] It can be seen from Table 1 that after the pipe is heated by the same external heat source, the anti-static pressure strength of the controllable strength plastic pipes prepared in Examples 1-4 is stronger than that of the plastic pipes prepared in Comparative Examples 1 and 2. In the preparation of the thermoplastic elastomer of the intermediate layer micro-thermosensitive particles, silicon micropowder and 2-hydroxy-4-methoxybenzophenone are creatively added, which has the advantages of high thermal conductivity and good suspension performance, can absorb more heat energy under the same conditions, and can also improve the thermal stability and thermal conductivity of the thermoplastic elastomer, so as to have a solidification effect that is beneficial to the phase change of the intermediate layer.

[0051] Table 2 Corrosion resistance test results

[0052] As can be seen from Table 2, the corrosion resistance of the controlled strength plastic pipes prepared in Examples 1-4 is stronger than that of the plastic pipes prepared in Comparative Examples 1 and 2. This is because the inner layer UHMWPE material is subjected to liquid phase purification to improve the purity in the examples. The improvement of the material purity helps to reduce the erosion of the corrosive medium on the pipeline material, because impurities are often the starting point of corrosion. Through the purification process, the catalyst residues, unreacted monomers, oligomers and other impurities in the UHMWPE material can be effectively removed, which greatly improves the corrosion resistance of the product.

[0053] Table 3 Wear resistance test results

[0054] As can be seen from Table 2, the wear resistance of the controlled strength plastic pipes prepared in Examples 1-4 is stronger than that of the plastic pipes prepared in Comparative Examples 1 and 2. Only glass fibers were used in the preparation process of the comparative examples, while high-strength glass fibers were used in the preparation of the comparative examples. The high-strength glass fibers can significantly resist external wear sources due to their high hardness and strength. The high-strength glass fibers are tightly combined with the resin matrix, and the GFRP material structure formed is uniform and stable, which can effectively prevent the expansion of cracks and the aggravation of wear. Due to the improvement of wear resistance, the GFRP material using high-strength glass fibers can also significantly improve the service life of the controlled strength plastic pipe.

[0055] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to the present embodiment as needed, but they are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A plastic pipe with controllable strength, characterized in that The preparation process includes: A plastic pipe with controllable strength is obtained by co-extrusion using PE material as the inner layer material, thermoplastic elastomer with micro heat-sensitive particles as the middle layer material, and glass fiber reinforced plastic as the outer layer material.

2. The plastic pipe with controllable strength according to claim 1, characterized in that: The preparation method of the PE material comprises: Take pure ethylene monomer as raw material, select suitable saturated hydrocarbon as dispersion medium, add appropriate amount of catalyst and ensure that the catalyst is evenly distributed in the reaction system, carry out polymerization reaction under certain reaction conditions, add appropriate amount of lubricant after a period of time and continue the reaction, continue the reaction for a period of time, then separate the polymerized product from the reaction system and dry it to remove residual moisture and solvent to obtain PE material, and then obtain high-purity inner layer PE material through liquid phase purification.

3. The controllable strength plastic pipe according to claim 3, characterized in that: Contains at least one of the following characteristics (1) to (11): (1) The purity percentage of ethylene used should be above 99.9%; (2) The dispersion medium comprises at least one of heptane, hexane, petroleum ether, or kerosene; (3) The mass ratio of the dispersion medium to the ethylene monomer is: (1~2):1; (4) The catalyst comprises at least one of a Ziegler catalyst such as TiCl3-Al(C2H5)2Cl, TiCl4-Al(C2H5)2Cl or a metallocene catalyst; (5) The mass ratio of ethylene monomer to catalyst is 1: 0.002%~0.006%; (6) The reaction temperature range is 70~90℃; (7) The reaction pressure is 1 to 1.5 atmospheres; (8) The lubricant includes at least one of stearate, silicone oil or PTFE powder; (9) The mass ratio of lubricant to ethylene monomer is: (3%~6%):1; (10) The reaction time before adding lubricant is 1~4h; (11) The temperature range after separation and drying is 40~60℃, and the drying time is 4~10h.

4. The plastic pipe with controllable strength according to claim 1, characterized in that: The preparation method of the thermoplastic elastomer of the micro-thermosensitive particles comprises: Take an appropriate amount of TPE matrix, PAn / SiO2 composite microspheres and poly N-isopropylacrylamide and mix them in a certain proportion, then perform ball milling for a period of time, continue to add an appropriate amount of silicon micropowder and dibenzophenone substances and continue ball milling for a period of time. After ball milling, the raw materials are sent to a hot melt blender and hot melt blended at high temperature. After the end, the blended material is cooled by a cooling device, and the cooled material is granulated by a granulator to obtain a thermoplastic elastomer material with intermediate layer micro heat-sensitive particles.

5. The plastic pipe with controllable strength according to claim 4, characterized in that: Contains at least one of the following characteristics (1) to (8): (1) The mass ratio of TPE matrix, PAn / SiO2 composite microspheres and poly (N-isopropylacrylamide) is: (4-6): (2-3): 1; (2) The initial ball milling time is 1 to 4 hours; (3) The mass ratios of added silica powder and benzophenone to the mixture are: (1-2):8 and (1-3):9 respectively; (4) Benzophenone substances include at least one of benzophenone, 2-hydroxy-4-methoxybenzophenone, and oxybenzone (BP3); (5) The ball milling time after adding silica powder and benzophenone is: 1~4h; (6) The temperature of hot melt blending is: 150~180℃, and the time of hot melt blending is: 8~15min; (7) Cooling temperature range: 20~40℃; (8) The particle size of granulation is controlled at 3~6 mm.

6. The controllable strength plastic pipe according to claim 5, characterized in that: The preparation of the PAn / SiO2 composite microspheres comprises: Take an appropriate amount of polyaniline (PAn) and an initiator and mix them, take an appropriate amount of SiO2 nanoparticles and evenly disperse them in a solvent to obtain a dispersion of SiO2 nanoparticles, add the dispersion of SiO2 nanoparticles to the mixture of polyaniline (PAn) and the initiator, and carry out a polymerization reaction under suitable temperature and stirring conditions to obtain PAn / SiO2 composite microspheres, which are then separated by centrifugation, filtration or precipitation, and the composite microspheres are washed with an appropriate solvent and then dried to obtain PAn / SiO2 composite microspheres.

7. The controllable strength plastic pipe according to claim 1, characterized in that: The preparation of the outer layer of glass fiber reinforced plastic comprises: Take an appropriate amount of high-strength glass fiber and soak it in a resin matrix. After a certain period of time, pour the soaked glass fiber and resin mixture into a mold, and shape it through pressurization, heating and other process means to obtain an outer layer of glass fiber reinforced plastic.

8. The controllable strength plastic pipe according to claim 7, characterized in that: The preparation of the outer layer of glass fiber reinforced plastic includes at least one of the following features (1) to (4): (1) The tensile strength of high-strength glass fiber is 1500~4000MPa and the elastic modulus is 25-500MPa / mm 2 , bending strength is 2000~5000MPa; (2) The mass ratio of glass fiber to resin matrix is: 1:(2~3); (3) The resin matrix includes at least one of epoxy resin, polyester resin, vinyl ester resin and unsaturated polyester resin; (4) The pressure during the molding process is 10~20MPa, the molding temperature is 150~200℃, and the molding time is 6~9h.

9. The controllable strength plastic pipe according to claim 1, characterized in that: The preparation of the controllable strength plastic pipe includes: The inner layer PE material, the middle layer thermoplastic elastomer material of micro heat-sensitive particles, and the outer layer glass fiber reinforced plastic (GFRP) material are placed at the feed port of the extruder in a certain mass ratio, heated and melted separately, and then the three layers of materials are co-extruded through a three-layer co-extrusion die to obtain a plastic pipe with controllable strength.

10. The controllable-strength plastic pipe according to claim 9, characterized in that: The preparation of the controllable strength plastic pipe includes at least one of the following features (1) to (3): (1) The mass ratio of the inner layer PE material, the middle layer thermoplastic elastomer material of micro heat-sensitive particles, and the outer layer glass fiber reinforced plastic (GFRP) material is: (1-3): (6-7): (1-3); (2) The temperature range of the feed port section is: 100~120℃, the temperature range of the feed zone heating section is: 120~150℃, the temperature range of the screw zone heating section is 150~180℃, the temperature range of the barrel zone heating section is 180~200℃, and the temperature range of the die head heating section is 200-220℃; (3) The speed of discharging the co-dose is: 2.5~3.5 m / min.

Citation Information

Patent Citations

  • Novel all-plastic heat-insulation pressure-resistant conveying pipeline and preparation method thereof

    CN108943881A

  • Yolk-shell structure carbon ball@polyaniline composite microsphere and preparation method thereof

    CN109810269A

  • Corrosion-resistant PE drain pipe preparation process

    CN113337026A

  • Low-heat-conduction heat-preservation composite plastic pipeline and preparation method thereof

    CN116006785A

  • Abrasion restistant pipe

    US20020004116A1