A method for improving infrared laser absorptivity of spherical copper powder for selective laser melting

By adding nano-copper powder to the surface of spherical copper powder and performing ball milling and controlled atmosphere treatment, the problem of low absorption rate of copper powder to 1064nm infrared laser was solved, achieving high absorption rate and good thermal and electrical conductivity of copper powder, thus improving the quality of copper parts formed by selective laser melting.

CN115740438BActive Publication Date: 2024-11-15KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211487424.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-11-15
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

Copper has an extremely low absorption rate to the 1064nm infrared laser commonly used in selective laser melting, which makes it difficult to melt copper powder. This results in low density and performance of the formed parts, limiting its application in complex parts such as cooling walls for aerospace engines.

Method used

By adding nano-copper powder to the surface of spherical copper powder and ball milling it, followed by treatment under a controlled atmosphere, a nano-scale oxide layer is formed to improve laser absorption rate and avoid affecting thermal and electrical conductivity.

Benefits of technology

The infrared laser absorption rate of copper powder was significantly increased to over 35%, improving the density and performance of copper parts formed by selective laser melting, and meeting the requirements for thermal and electrical conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 221125114458
    Figure 221125114458
  • Figure 221125114503
    Figure 221125114503
  • Figure 221125114507
    Figure 221125114507
Patent Text Reader

Abstract

The invention discloses a method for improving the infrared laser absorption rate of spherical copper powder for selective laser melting, comprising the following steps: adding nano copper powder to spherical copper powder; adding the spherical copper powder with the nano copper powder added to a pure copper grinding tank of a planetary ball mill for grinding; placing the ball-milled powder in an atmosphere protection furnace for controlled atmosphere treatment, and obtaining spherical copper powder for selective laser melting with high infrared laser absorption rate after the treatment. The invention can obtain high-quality copper powder for selective laser melting with an infrared laser absorption rate of more than 35%, and greatly improve the density of selective laser melted copper formed parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a method for improving the infrared laser absorptivity of spherical copper powder for selective laser melting, belonging to the field of 3D printing and additive manufacturing. Background Art

[0002] Selective laser melting is a method that uses a focused high-energy laser as a heat source, scans a specific area of ​​the molten powder bed according to the scanning path obtained after the digital model of the formed part is discretized, and accumulates and manufactures parts layer by layer. Compared with traditional processes, laser selective melting has the advantages of direct forming, no need for molds, high precision, and direct manufacturing of complex structures. Selective laser melting usually uses an infrared laser with a wavelength of 1064nm to melt spherical powder with a diameter of 15~53 microns to ensure the forming quality.

[0003] Copper has good electrical and thermal conductivity, and is an ideal material for complex parts such as aerospace engine cooling walls. However, copper has an extremely low absorption rate for infrared lasers with a wavelength of 1064nm, which is commonly used in selective laser melting. This makes it difficult to melt the powder during selective laser melting, and it is difficult to increase the density of the formed parts, resulting in poor performance, which greatly limits the application of selective laser melting copper. Improving the absorption rate of spherical copper powder for selective laser melting to infrared lasers with a wavelength of 1064nm is the key to improving the quality and performance of selective laser melted copper parts.

[0004] Alloying can improve the laser absorption rate of powder to a certain extent; adding alloying elements to copper will form a copper alloy with a higher laser absorption rate for pure copper; adding alloying elements to pre-alloy during smelting and then using methods such as atomization can obtain copper alloy powder with relatively high laser absorption rate, but this method cannot be used to process pure copper powder. After the alloying elements are added, the thermal conductivity and electrical conductivity of copper will be greatly reduced, affecting the performance and application of the formed parts. Summary of the invention

[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for improving the infrared laser absorptivity of spherical copper powder for selective laser melting; according to the absorption characteristics of the material to the infrared laser and the characteristics of the selective laser melting copper forming process, the method uses homogeneous nano-copper particles to modify the surface of the micron-sized spherical copper powder, and combines the controlled atmosphere treatment to effectively improve the infrared laser absorptivity of the selective laser copper powder, with little effect on the thermal and electrical conductivity; the method of the present invention specifically comprises the following steps:

[0006] (1) Add nano copper powder to spherical copper powder.

[0007] (2) Add the spherical copper powder added with nano copper powder into the pure copper grinding tank of the planetary ball mill for grinding.

[0008] (3) The ball-milled powder is placed in an atmosphere protection furnace for controlled atmosphere treatment. After the treatment, spherical copper powder with high infrared laser absorption rate for selective laser melting can be obtained.

[0009] Preferably, the size of the nano copper powder in step (1) of the present invention is 10-100 nm, and the addition ratio of the nano copper powder is 1-5 g of 10-100 nm nano copper powder per kilogram of spherical copper powder for selective laser melting.

[0010] Preferably, in step (2) of the present invention, a pure copper grinding jar and pure copper grinding balls are used, and pure copper grinding balls with a diameter of 10 to 20 mm are added at a ratio of 2 to 3 kg of grinding balls per kg of powder; the grinding jar is sealed, and vacuum is drawn to maintain a vacuum degree of 1.0×10 -2 ~2.0×10 -2 Pa.

[0011] Preferably, the specific process of grinding in step (2) of the present invention is: start the planetary ball mill, at a speed of 200-500 rpm, ball mill for 4-8 minutes, pause for 2-4 minutes, then ball mill for another 4-8 minutes, pause for 2-4 minutes, and repeat this process 3-5 times.

[0012] Preferably, the specific process of the controlled atmosphere treatment of the powder in step (3) of the present invention is: placing the ball-milled powder in an atmosphere protection furnace, heating it to 150-300° C. under an oxygen partial pressure of 0.02-0.05 MPa, keeping it warm for 30-120 minutes, and then cooling it to room temperature with the furnace.

[0013] The principle of the present invention is as follows: nano copper powder can be adsorbed on the surface of micron spherical copper powder particles used for selective laser melting through ball milling to improve the absorption rate of the spherical copper powder; then the surface of the spherical copper powder particles is treated through controlled atmosphere treatment to further improve the laser absorption rate of the spherical copper powder; the nano copper powder used in this process is homogeneous particles, and the nano-level oxide layer formed on the surface of the copper powder after the controlled atmosphere treatment is mostly decomposed and precipitated during the selective laser melting process, and will not affect the thermal conductivity and electrical conductivity of the formed part.

[0014] The beneficial effects of the present invention are as follows: the infrared laser absorptivity of the copper powder for selective laser melting is increased to more than 35%, and other alloy elements and impurities are not introduced, the thermal conductivity and electrical conductivity of copper are not affected, and the density and performance of selective laser melted copper formed parts are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 Morphology of copper powder before treatment;

[0016] Figure 2 Morphology of copper powder after treatment;

[0017] Figure 3 Comparison of the reflectivity of the powder before and after treatment. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the described contents.

[0019] Example 1

[0020] Take 1 kg of spherical copper powder for selective laser melting, add 1 g of 10 nm nano copper powder, add it into the pure copper grinding jar of the planetary ball mill, add 2 kg of pure copper grinding balls with a diameter of 10 mm; after sealing, evacuate the grinding jar to keep the vacuum degree in the grinding jar at 1.0×10 -2 Pa; then start the planetary ball mill, at a speed of 200 rpm, ball mill for 4 minutes, pause for 2 minutes, and repeat the above steps 3 times.

[0021] The ball-milled powder was placed in an atmosphere protection furnace, heated to 150° C. under an oxygen partial pressure of 0.05 MPa, kept warm for 120 minutes, and then cooled to room temperature with the furnace to obtain the processed spherical copper powder for selective laser melting.

[0022] Figure 1 This is the morphology of copper powder before treatment. Figure 2 This is the morphology of the spherical copper powder prepared in this example. Figure 2 It can be seen that a nanostructure conducive to infrared laser absorption is formed on the surface of the treated copper powder. Figure 3 To compare the reflectivity of the powder before and after treatment, Figure 3 It can be seen that the reflectivity of the copper powder to the 1064nm infrared laser before treatment is 79%, and the corresponding laser absorption rate is 21%; after treatment, the reflectivity of the copper powder to the 1064nm infrared laser drops to 30%, and the corresponding laser absorption rate increases to 70%.

[0023] In summary, the infrared laser absorption rate of the spherical copper powder prepared by the method described in this embodiment is 70%; the infrared laser absorption rate of the spherical copper powder before treatment is 21%. The method described in the present invention can greatly improve the infrared laser absorption rate of the spherical copper powder.

[0024] Example 2

[0025] Take 1 kg of spherical copper powder for selective laser melting, add 5 g of 100 nm nano copper powder, add it into the pure copper grinding jar of the planetary ball mill, add 3 kg of pure copper grinding balls with a diameter of 20 mm; after sealing, evacuate the grinding jar to maintain a vacuum degree of 2.0×10 -2 Pa; then start the planetary ball mill, at a speed of 500 rpm, ball mill for 8 minutes, pause for 4 minutes, and repeat the above steps 5 times.

[0026] The ball-milled powder was placed in an atmosphere protection furnace, heated to 300° C. under an oxygen partial pressure of 0.03 MPa, kept warm for 30 minutes, and then cooled to room temperature with the furnace to obtain the processed spherical copper powder for selective laser melting.

[0027] The infrared laser absorption rate of the spherical copper powder prepared by the method described in this embodiment is 60%; the infrared laser absorption rate of the spherical copper powder before treatment is 21%. The method described in the present invention can greatly improve the infrared laser absorption rate of the spherical copper powder.

[0028] Example 3

[0029] Take 1 kg of spherical copper powder for selective laser melting, add 3 g of 50 nm nano copper powder, add it into the pure copper grinding jar of the planetary ball mill, add 2.5 kg of pure copper grinding balls with a diameter of 15 mm; after sealing, evacuate the grinding jar to maintain a vacuum degree of 1.5×10 -2 Pa; then start the planetary ball mill, at a speed of 300 rpm, ball mill for 6 minutes, pause for 3 minutes, and repeat the above steps 4 times.

[0030] The ball-milled powder was placed in an atmosphere protection furnace, heated to 200° C. under an oxygen partial pressure of 0.02 MPa, kept warm for 90 minutes, and then cooled to room temperature with the furnace to obtain the processed spherical copper powder for selective laser melting.

[0031] The infrared laser absorption rate of the spherical copper powder prepared by the method described in this embodiment is 40%; the infrared laser absorption rate of the spherical copper powder before treatment is 21%. The method described in the present invention can greatly improve the infrared laser absorption rate of the spherical copper powder.

Claims

1. A method for improving the infrared laser absorptivity of spherical copper powder for selective laser melting, characterized in that: The specific steps include: (1) Adding nano copper powder to spherical copper powder; (2) adding the spherical copper powder added with the nano copper powder and a certain weight of grinding balls into the grinding jar of the planetary ball mill, sealing the jar and grinding the jar under vacuum; (3) Placing the ball-milled powder in an atmosphere protection furnace for controlled atmosphere treatment, and obtaining spherical copper powder for selective laser melting with high infrared laser absorption rate after the treatment; The size of the nano copper powder in step (1) is 10-100 nm; The addition ratio of the nano copper powder is 1-5 grams of 10-100 nm nano copper powder per kilogram of spherical copper powder for selective laser melting.

2. The method for improving infrared laser absorptivity of spherical copper powder for selective laser melting according to claim 1, characterized in that: In step (2), a pure copper grinding jar and pure copper grinding balls are used, and pure copper grinding balls with a diameter of 10 to 20 mm are added at a ratio of 2 to 3 kg of grinding balls per kg of powder; then the grinding jar is sealed and evacuated to maintain a vacuum degree of 1.0 × 10 -2 ~2.0×10 -2 Pa.

3. The method for improving infrared laser absorptivity of spherical copper powder for selective laser melting according to claim 2, characterized in that: The specific process of grinding in step (2) is: turn on the planetary ball mill, at a rotation speed of 200-500 rpm, ball mill for 4-8 minutes, pause for 2-4 minutes, then ball mill for another 4-8 minutes, pause for 2-4 minutes, and repeat this process 3-5 times.

4. The method for improving infrared laser absorptivity of spherical copper powder for selective laser melting according to claim 1, characterized in that: The specific process of the controlled atmosphere treatment of the powder in step (3) is: the ball-milled powder is placed in an atmosphere protection furnace, heated to 150-300°C under an oxygen partial pressure of 0.02-0.05 MPa, kept warm for 30-120 minutes, and then cooled to room temperature with the furnace.