Sacrificial anode protection device and method for concrete pipe piles in saline-alkali areas
By using sacrificial anode protection devices in foundation concrete pipe piles in saline-alkali areas and designing sacrificial anodes based on soil corrosiveness levels and characteristics of concrete pipe piles, the corrosion problem of foundation concrete pipe piles in saline-alkali areas in high chloride environments has been solved, and a comprehensive solution has been achieved. Covered for corrosion protection and extended service life.
Patent Information
- Application Number
- CN202211270778.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-10-17
AI Technical Summary
Existing technology cannot effectively solve the corrosion problem of foundation concrete pipe piles in saline-alkali areas in high chloride environments, and anti-corrosion measures lack personalized design for different soil corrosion levels and reinforced concrete structures.
The sacrificial anode protection device is used to provide full coverage anti-corrosion protection by evaluating the soil corrosion level and selecting suitable sacrificial anode materials, combined with the analytical hierarchy process to determine the specific shape, quantity and installation location of the sacrificial anodes.
The sacrificial anode protection device designed according to different soil corrosion levels and characteristics of concrete pipe piles has been realized to effectively prevent corrosion, extend the service life of pipe piles, and improve corrosion control capabilities during the construction and operation phases.
Smart Images

Figure CN115747809B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a protective device for concrete pipe piles in saline-alkali areas, and in particular to a sacrificial anode protective device and method for concrete pipe piles in saline-alkali areas. Background Art
[0002] Prestressed concrete pipe piles have become the preferred pile type for many projects due to their low comprehensive cost, fast construction speed, easy control of construction quality, low impact on the environment, and high cost performance. At present, in addition to being widely used in inland areas with normal soil conditions, they are widely used in coastal areas (such as Shandong, Fujian, Zhejiang, Shanghai, etc.), inland saline-alkali areas (such as the eastern part of Inner Mongolia) and other corrosive environments. In a high chloride environment, due to the strong permeability of chloride ions, they can penetrate the sheath of concrete and reach the surface of steel in concrete, causing corrosion damage; sometimes there are cracks in the concrete sheath, and the corrosive medium can directly reach the surface of the steel embedded in the concrete, causing corrosion. At present, a series of specifications have been promulgated in China for the anti-corrosion work of reinforced concrete pipe piles. These specifications have a comprehensive classification of environmental categories and influencing factors, but they do not take into account the unique environmental factors in each place and the uses of different reinforced concrete structures. As a result, the current anti-corrosion work of pipe piles is rather chaotic. For example, some projects are located in moderately corrosive environments or above, but the pipe piles are not treated with anti-corrosion and ordinary pipe piles are still used. Some only have anti-corrosion coatings on the outer surfaces, and the pile body concrete does not meet the requirements of the specifications. Some outer surface coatings are not cured for long enough, and the protective layer is destroyed during piling construction. Some pipe pile end pads are not thickened, etc.
[0003] From the perspective of system engineering, cathodic protection is the main means of protecting concrete pipe piles in a strong corrosive environment. First, the soil corrosiveness is evaluated according to the soil environment where the foundation concrete pipe piles are located. The material of the sacrificial anode is selected according to the metal material of the protected concrete pipe piles and the characteristics of various anode materials, and the specific number and installation location of the required sacrificial anodes are determined before installation. However, there is no relevant description in the existing technology. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a sacrificial anode protection device and method for foundation concrete piles in saline-alkali areas, which can be used to manufacture foundation concrete pile protection devices according to different soil corrosion levels in order to overcome the shortcomings of the prior art.
[0005] The technical solution adopted by the present invention is: a sacrificial anode protection device for concrete pipe piles in saline-alkali areas, comprising a concrete pipe pile consisting of a pile body and a lower pile head, wherein the lower pile head is composed of a connecting piece and an end plate fixedly arranged on the upper end of the connecting piece, and is also provided with a sacrificial anode, one end of the sacrificial anode is fixedly connected to the end plate of the lower pile head by welding, and the other end of the sacrificial anode extends into the pile body.
[0006] A method for selecting a sacrificial anode in a sacrificial anode protection device for a concrete pipe pile in a saline-alkali area comprises the following steps:
[0007] 1) According to the soil environment of the foundation concrete pile in the saline-alkali area, five influencing factors affecting soil resistivity are determined, soil corrosivity is evaluated, and soil grade is determined; the five influencing factors affecting soil resistivity are: soil salt content, soil moisture, soil porosity, soil pH value and soil temperature;
[0008] 2) Select the material of the sacrificial anode according to the protection potential required by the metal material of the concrete pile to be protected and the metal material of the concrete pile welding, the soil resistivity in the area where the concrete pile is located, and the characteristics of different sacrificial anode materials;
[0009] 3) Determine the specific shape and quantity of the sacrificial anode according to the shape of the concrete pile to be protected, the metal material of the concrete pile, the metal material of the concrete pile welding, the soil resistivity of the area where the concrete pile is located, and the design life of the sacrificial anode protection device;
[0010] 4) Select the installation location of the sacrificial anode according to the shape of the concrete pipe pile to be protected and install it.
[0011] The sacrificial anode protection device and method for foundation concrete pipe piles in saline-alkali areas of the present invention is based on the anti-corrosion problem of foundation concrete pipe piles, using a large amount of construction data, combined with practical experience, and formulated scoring rules for limiting factors affecting the soil environment, determining the soil corrosion level, and using the hierarchical analysis method to score various factors of the sacrificial anode material to select suitable sacrificial anode materials. According to the shape of the protected concrete pipe piles, the metal material of the concrete pipe piles, the metal material of the concrete pipe piles, the soil resistivity of the area where the piles are located, and the design life of the sacrificial anode protection device, the specific shape of the sacrificial anode is determined, the specific number of sacrificial anodes required, and the appropriate installation location is selected for installation. The method is reasonably designed and highly operable, and provides a good method and means for the anti-corrosion protection of foundation concrete pipe piles. The present invention can use the hierarchical analysis method to integrate multiple evaluation indicators, combined with the formulated scoring rules, and use the sacrificial anode method to effectively protect the foundation concrete pipe piles in saline-alkali areas from corrosion. It has the following advantages:
[0012] 1. By analyzing the influencing factors of the soil environment, the hierarchical analysis method is used to determine the weight of each factor and score it, the soil corrosion level is determined, and the appropriate sacrificial anode material is selected according to the comprehensive evaluation score. This method is simple, reasonable and easy to use.
[0013] 2. This method can be used for corrosion control of concrete pipe piles in saline-alkali areas during the design and manufacturing stages. It can lay a solid foundation for concrete pipe piles in saline-alkali areas at the initial stage of their life and provide strong support for corrosion control during the operation stage.
[0014] 3. The sacrificial anode protection device and method for foundation concrete pipe piles moves the anti-corrosion checkpoint forward, which not only highlights the management focus, but also achieves full coverage control in the design, manufacturing, and operation stages, and rationally allocates management resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Schematic diagram of the assembly of the sacrificial anode protection device of the present invention, in which:
[0016] 1: Pile 2: Sacrificial anode
[0017] 3: Lower pile head 3.1: Connectors
[0018] 3.2: End plate;
[0019] Figure 2 The present invention is a flow chart of a method for selecting a sacrificial anode in a sacrificial anode protection device for concrete pipe piles in saline-alkali areas. DETAILED DESCRIPTION
[0020] The sacrificial anode protection device and method for concrete pipe piles in saline-alkali areas of the present invention are described in detail below in conjunction with the embodiments and drawings.
[0021] The sacrificial anode protection device and method for foundation concrete pipe piles in saline-alkali areas of the present invention is based on the anti-corrosion problem of foundation concrete pipe piles, uses a large amount of construction data, combines practical experience, formulates scoring rules for limiting factors affecting soil environment, determines the soil corrosion level, and uses the hierarchical analysis method to score various factors of sacrificial anode materials to select suitable sacrificial anode materials. According to the shape of the protected concrete pipe pile, the metal material of the concrete pipe pile, the metal material of the concrete pipe pile welding, the soil resistivity of the area where the concrete pipe pile is located, and the design life of the sacrificial anode protection device, the specific shape and specific number of the sacrificial anodes are determined, and a suitable installation position is selected for installation.
[0022] like Figure 1The invention shown in the figure is a sacrificial anode protection device for concrete pipe piles in saline-alkali areas, comprising a concrete pipe pile consisting of a pile body 1 and a lower pile head 3, wherein the lower pile head 3 is composed of a connecting member 3.1 and an end plate 3.2 fixedly arranged on the upper end of the connecting member 3.1, and is also provided with a sacrificial anode 2, one end of the sacrificial anode 2 is fixedly connected to the end plate 3.2 of the lower pile head 3 by welding, and the other end of the sacrificial anode 2 extends into the pile body 1.
[0023] like Figure 2 As shown, the method for selecting the sacrificial anode in the sacrificial anode protection device for concrete pipe piles in saline-alkali areas of the present invention comprises the following steps:
[0024] 1) According to the soil environment of the foundation concrete piles in saline-alkali areas, the five factors affecting soil resistivity are determined, the soil corrosivity is evaluated, and the soil grade is determined;
[0025] The corrosion of foundation concrete piles in the soil environment belongs to the category of electrochemical corrosion. Soil resistivity is an indicator of soil conductivity and is used as a basic parameter to judge soil corrosiveness. The five factors that affect soil resistivity are: soil salt content, soil moisture (water content), soil porosity (tightness), soil pH (acidity and alkalinity) and soil temperature;
[0026] (1) The weights of the five factors affecting soil resistivity were determined by using the analytic hierarchy process, which are:
[0027] The soil salt content level weight b1 is 0.26;
[0028] The soil moisture (water content) level weight b2 is 0.21;
[0029] The soil porosity (looseness) grade weight b3 is 0.08;
[0030] The soil pH (acidity) level weight b4 is 0.3;
[0031] The soil temperature grade weight b5 is 0.15;
[0032] (2) Determine the scoring criteria for each factor affecting soil resistivity
[0033] (2.1) Soil salt content scoring standard: the lower the score, the more corrosive the soil is:
[0034] Usually the soil contains various salts. The Cl — with SO 4 2- However, it can cause relatively serious metal corrosion. The higher the salt content, the more corrosive the soil is.
[0035] Soil salt content is greater than or equal to 100mmol / kg, 1 point;
[0036] 2 points if the soil salt content is greater than or equal to 30mmol / kg and less than 100mmol / kg;
[0037] 3 points if the soil salt content is greater than or equal to 10mmol / kg and less than 30mmol / kg;
[0038] 4 points if the soil salt content is greater than or equal to 3mmol / kg and less than 10mmol / kg;
[0039] Soil salt content is less than 3mmol / kg, 5 points;
[0040] (2.2) Soil moisture (water content) scoring criteria: the lower the score, the more corrosive the soil is:
[0041] The soil liquid content is divided into surface water and groundwater. Usually, as the soil moisture increases, O 2 and CO 2 The content of will also increase, resulting in a more significant effect on the potential of the metal electrode. The higher the humidity, the more corrosive the soil will be.
[0042] Soil moisture (water content) greater than or equal to 80% is 1 point;
[0043] Soil moisture (water content) greater than or equal to 50% and less than 80% is 2 points;
[0044] Soil moisture (water content) greater than or equal to 20% and less than 50% is 3 points;
[0045] Soil moisture (water content) greater than or equal to 10% and less than 20% is 4 points;
[0046] Soil moisture (water content) is less than 10%, which is 5 points;
[0047] (2.3) Soil porosity (looseness) scoring standard: the lower the score, the more corrosive the soil is:
[0048] The porosity of soil usually determines the air permeability of the soil. Usually the size of the porosity indicates the looseness and air capacity of the soil. The higher the porosity, the weaker the soil corrosiveness.
[0049] Soil porosity (looseness) is less than or equal to 30%, with 1 point;
[0050] Soil porosity (looseness) greater than 30% and less than or equal to 40% is 2 points;
[0051] Soil porosity (looseness) greater than 40% and less than or equal to 50% is 3 points;
[0052] Soil porosity (looseness) greater than 50% and less than or equal to 60% is 4 points;
[0053] Soil porosity (looseness) greater than 60% is 5 points;
[0054] (2.4) Soil pH (acidity and alkalinity) scoring standard: the lower the score, the more corrosive the soil:
[0055] Soil with a lower pH value is more susceptible to corrosion.
[0056] The soil pH value (acidity and alkalinity) is less than or equal to 4, which is 1 point;
[0057] If the soil pH value (acidity and alkalinity) is greater than 4 and less than or equal to 5.5, it is 2 points;
[0058] The soil pH value (acidity and alkalinity) is greater than 5.5 and less than or equal to 7.5, which is 3 points;
[0059] The soil pH value (acidity and alkalinity) is greater than 7.5 and less than or equal to 8.5, which is 4 points;
[0060] The soil pH value (acidity and alkalinity) is greater than 8.5, which is 5 points;
[0061] (2.5) Soil temperature scoring criteria: the lower the score, the more corrosive the soil:
[0062] The temperature of the soil affects the solubility of gases in the soil liquid phase, and the degree of influence involves the effect of oxygen content on the cathode and anode. The higher the soil temperature, the faster the diffusion rate of metal corrosion controlled by the diffusion process.
[0063] 1 point if the soil temperature is greater than or equal to 30°C;
[0064] 2 points if the soil temperature is greater than or equal to 20°C and less than 30°C;
[0065] 3 points if the soil temperature is greater than or equal to 15°C and less than 20°C;
[0066] 4 points if the soil temperature is greater than or equal to 10°C and less than 15°C;
[0067] If the soil temperature is less than 10℃, it is 5 points;
[0068] (3) Calculate the soil resistivity correction factor and determine the soil corrosion level
[0069] The comprehensive calculation formula of soil resistivity correction factor K is as follows:
[0070] K=b 1 ×Soil salt content score + b 2× soil moisture score + b 3 ×Soil porosity score + b 4 ×Soil pH score + b 5 ×Soil temperature score;
[0071] When the soil resistivity correction coefficient K is greater than or equal to 1 and less than 2.2, the soil is extremely corrosive, the probability of local corrosion or pitting corrosion is extremely high, the probability of uniform corrosion is moderate, and the soil grade is IV;
[0072] When the soil resistivity correction coefficient K is greater than or equal to 2.2 and less than 3.2, the soil is highly corrosive, the probability of local corrosion or pitting corrosion is moderate, the probability of uniform corrosion is slight, and the soil grade is III;
[0073] When the soil resistivity correction coefficient K is greater than or equal to 3.2 and less than 4.2, the soil is less corrosive, the probability of local corrosion or pitting corrosion is slight, the probability of uniform corrosion is extremely slight, and the soil grade is II;
[0074] When the soil resistivity correction coefficient K is greater than or equal to 4.2 and less than or equal to 5, the soil is extremely weakly corrosive, the probability of local corrosion or pitting corrosion is extremely slight, the probability of uniform corrosion is extremely slight, and the soil grade is Grade I.
[0075] 2) Select the material of the sacrificial anode according to the required protection potential of the metal material of the concrete pile to be protected and the metal material of the concrete pile welding, the soil resistivity of the area where the concrete pile is located and the characteristics of different sacrificial anode materials; including:
[0076] (1) Determine the factor weight vectors of the three factors for selecting sacrificial anode materials and score the three factors
[0077] The selection of sacrificial anode materials is affected by many factors. The three factors for selecting sacrificial anode materials are: soil resistivity, the metal material of the protected concrete pile and the protection potential required by the welded metal material of the concrete pile, and the open circuit potential of the sacrificial anode material;
[0078] (1.1) The weights of each factor in selecting sacrificial anode materials are obtained by applying the hierarchical analysis method, which are:
[0079] The soil resistivity grade weight h1 is 0.528;
[0080] The required protection potential level weight h2 of the protected concrete pipe pile metal material and the concrete pipe pile welding metal material is 0.332;
[0081] The open circuit potential grade weight h3 of the sacrificial anode material is 0.140;
[0082] The grade weights of the three factors form the weight vector H:
[0083]
[0084] (1.2) The three factors for selecting sacrificial anode materials are graded, each factor is divided into 3 levels, and each factor is scored separately:
[0085] Soil resistivity rating:
[0086] The resistivity of the soil is greater than or equal to 1Ω·m and less than or equal to 5Ω·m, and the score is 1;
[0087] The resistivity of the soil is greater than 5Ω·m and less than or equal to 8Ω·m, and the score is 2;
[0088] The resistivity of the soil is greater than 8Ω·m and less than or equal to 10Ω·m, and the score is 3;
[0089] Under the copper-copper sulfate reference electrode, the protection potential grade rating required for the protected concrete pipe pile metal material and the concrete pipe pile welding metal material is:
[0090] The protection potential is greater than or equal to -1.5V and less than or equal to -1.2V, and the score is 1;
[0091] The protection potential is greater than -1.2V and less than or equal to -1.1V, and the score is 2;
[0092] The protection potential is greater than -1.1V and less than or equal to -0.85V, and the score is 3;
[0093] The open circuit potential rating of sacrificial anode materials under the calomel reference electrode is:
[0094] The open circuit potential is greater than or equal to -1.7V and less than or equal to -1.5V, and the score is 1;
[0095] The open circuit potential is greater than -1.5V and less than or equal to -1.3V, and the score is 2;
[0096] The open circuit potential is greater than -1.3V and less than or equal to -1.0V, and the score is 3.
[0097] (2) Comprehensive evaluation calculation method and selection criteria for sacrificial anode material selection
[0098] The sacrificial anode material is scored according to the three factors in step (1) to obtain the scoring vector F of the sacrificial anode material:
[0099] F=[F 1 ,F 2 ,F 3 ]
[0100] Among them, F 1 、F 2、F 3 The scoring values of the three factors for selecting sacrificial anode materials;
[0101] Comprehensive evaluation score K for sacrificial anode material selection sam Calculate as follows:
[0102] K sam =H T ·F T
[0103] The selection criteria for sacrificial anode materials are:
[0104] Comprehensive evaluation score K sam ≤1.2, it is recommended to select a high potential pure magnesium or magnesium-manganese magnesium anode as the sacrificial anode;
[0105] Comprehensive evaluation score K sam >1.2 and ≤2.2, it is recommended to select magnesium anode of magnesium-aluminum-zinc-manganese system as sacrificial anode;
[0106] Comprehensive evaluation score K sam >2.2 and ≤3, it is recommended to choose a magnesium anode or a zinc alloy anode of the magnesium-aluminum-zinc-manganese system as a sacrificial anode.
[0107] 3) Determine the specific shape and quantity of the sacrificial anode according to the shape of the protected concrete pile, the metal material of the concrete pile, the metal material of the concrete pile welding, the soil resistivity of the area where the concrete pile is located, and the design life of the sacrificial anode protection device; including:
[0108] In order to adapt to the geological differences in my country, most of the pipe piles currently used in my country are prestressed concrete pipe piles. According to the different concrete strength grades, prestressed pipe piles can be divided into prestressed concrete pipe piles (PC piles) and prestressed high-strength concrete pipe piles (PHC piles). The metal inside the protected concrete pipe pile is a steel cage, and the end plate and connectors are generally cast steel parts.
[0109] (1) Determine the specific shape of the sacrificial anode based on the determined sacrificial anode material and the internal space of the concrete pile;
[0110] (2) Number of sacrificial anodes required
[0111]
[0112] Where: N is the number of sacrificial anodes, unit:
[0113] I s is the required protection current, in A;
[0114] I a It is the output current of a single sacrificial anode, in A;
[0115] f is the reserve coefficient. Since the foundation concrete pipe piles are buried structures, it is taken as 1.7.
[0116] (2.1) Calculate the total protection current I required for the protected concrete piles s :
[0117] I s =I A ×S Total
[0118] S 总 =N×πDL
[0119] Where: I A For protection current density, unit is mA / m 2 ;
[0120] S 总 is the total area of steel bars inside the concrete pile, in m 2 ;
[0121] N is the number of steel bars inside the concrete pile, in pieces;
[0122] D is the diameter of a single steel bar, in m;
[0123] L is the length of a single steel bar, in m;
[0124] When the soil resistivity correction coefficient K is greater than or equal to 1 and less than 2.2, the soil grade is IV, the soil is extremely corrosive, and I A Take 60~100mA / m 2 ;
[0125] When the soil resistivity correction coefficient K is greater than or equal to 2.2 and less than 3.2, the soil grade is Grade III, the soil is highly corrosive, and Grade I A Take 30~60mA / m 2 ;
[0126] When the soil resistivity correction coefficient K is greater than or equal to 3.2 and less than 4.2, the soil grade is II, the soil corrosiveness is weak, and I A Take 10~30mA / m 2 ;
[0127] When the soil resistivity correction coefficient K is greater than or equal to 4.2 and less than or equal to 5, the soil grade is Grade I, the soil corrosiveness is extremely weak, and Grade I A Take 5~10mA / m 2 ;
[0128] (2.2) Output current of a single sacrificial anode
[0129]
[0130] Where: ΔU is the driving voltage, unit V;
[0131] When a high-potential pure magnesium or magnesium-manganese magnesium anode is selected as a sacrificial anode, ΔU is 0.18V;
[0132] When a magnesium anode or zinc alloy anode of the magnesium-aluminum-zinc-manganese system is selected as a sacrificial anode, ΔU is 0.2V;
[0133] R is the total resistance of the loop, which is approximately equal to the sacrificial anode grounding resistance R A , unit Ω;
[0134] (2.3) Calculate the sacrificial anode grounding resistance:
[0135] Since the concrete piles are below the ground and in a water environment, the grounding resistance R A Calculated according to water connection resistance:
[0136]
[0137]
[0138] Where: R A is the sacrificial anode grounding resistance, unit: Ω;
[0139] l is the length of the sacrificial anode, in cm;
[0140] ρ is the resistivity of the medium, in Ω·cm;
[0141] t 1 is the equivalent substitution coefficient;
[0142] r is the equivalent radius of the sacrificial anode, Unit: cm;
[0143] A is the cross-sectional area of the sacrificial anode cross section, in cm 2 .
[0144] (3) Sacrificial anode service life
[0145] When designing a sacrificial anode protection device, the total number of sacrificial anodes output current and sacrificial anode consumption rate are used to calculate the service life of the sacrificial anodes. After installing the sacrificial anodes, the total number of sacrificial anodes output current I is measured. a Total sacrificial anode consumption rate, verify the sacrificial anode working life,
[0146]
[0147] Where: T is the sacrificial anode service life, unit is a;
[0148] W is the net mass of the sacrificial anode, in kg;
[0149] ω is the sacrificial anode consumption rate, kg / (A·a);
[0150] When a high potential pure magnesium or magnesium-manganese magnesium anode is selected as a sacrificial anode, ω is taken as 7.5kg / (A·a)
[0151] When magnesium anode or zinc alloy anode of magnesium-aluminum-zinc-manganese system is used as sacrificial anode, ω is taken as 5kg / (A·a)
[0152] I a总 Output current for the total number of sacrificial anodes, unit A.
[0153] 4) Select the installation location of the sacrificial anode according to the shape of the concrete pile to be protected and install it; including:
[0154] First, determine the electrical connection status of the steel cage inside the concrete pipe pile. If the electrical connection is normal, choose to install the sacrificial anode; if the electrical connection is abnormal, repair the steel bars by welding to ensure effective electrical connection between the steel cages inside the concrete pipe pile, and then choose to install the sacrificial anode.
Claims
1. A method for selecting sacrificial anodes in a sacrificial anode protection device for concrete pipe piles in saline-alkali areas, the sacrificial anode protection device for concrete pipe piles in saline-alkali areas comprising a concrete pipe pile consisting of a pile body (1) and a lower pile head (3), wherein: The lower pile head (3) is composed of a connecting piece (3.1) and an end plate (3.2) fixedly arranged on the upper end of the connecting piece (3.1), and is also provided with a sacrificial anode (2), one end of the sacrificial anode (2) is fixedly connected to the end plate (3.2) of the lower pile head (3) by welding, and the other end of the sacrificial anode (2) extends into the pile body (1); the method for selecting the sacrificial anode comprises the following steps: 1) According to the soil environment of the foundation concrete pile in the saline-alkali area, five influencing factors affecting soil resistivity are determined, soil corrosivity is evaluated, and soil grade is determined; the five influencing factors affecting soil resistivity are: soil salt content, soil moisture, soil porosity, soil pH value and soil temperature; the evaluation of soil corrosivity and determination of soil grade include: (1) The weights of the five factors affecting soil resistivity were determined by using the analytic hierarchy process, which are: The soil salt content level weight b1 is 0.26; The soil moisture level weight b2 is 0.21; The soil porosity grade weight b3 is 0.08; The soil pH level weight b4 is 0.3; The soil temperature grade weight b5 is 0.15; (2) Determine the scoring criteria for each factor affecting soil resistivity (2.1) Soil salt content scoring standard: the lower the score, the more corrosive the soil is: Soil salt content is greater than or equal to 100mmol / kg, 1 point; 2 points if the soil salt content is greater than or equal to 30mmol / kg and less than 100mmol / kg; 3 points if the soil salt content is greater than or equal to 10mmol / kg and less than 30mmol / kg; 4 points if the soil salt content is greater than or equal to 3mmol / kg and less than 10mmol / kg; Soil salt content is less than 3mmol / kg, 5 points; (2.2) Soil moisture rating standard: the lower the rating, the more corrosive the soil is: 1 point if soil moisture is greater than or equal to 80%; Soil moisture is greater than or equal to 50% and less than 80%, 2 points; Soil moisture is greater than or equal to 20% and less than 50%, 3 points; Soil moisture is greater than or equal to 10% and less than 20%, which is 4 points; If the soil moisture is less than 10%, it is 5 points; (2.3) Soil porosity scoring standard: the lower the score, the more corrosive the soil is: Soil porosity is less than or equal to 30%, with a score of 1; Soil porosity greater than 30% and less than or equal to 40% is 2 points; Soil porosity greater than 40% and less than or equal to 50% is 3 points; Soil porosity greater than 50% and less than or equal to 60% is 4 points; Soil porosity greater than 60% is 5 points; (2.4) Soil pH rating standard: the lower the rating, the more corrosive the soil: If the soil pH is less than or equal to 4, it is 1 point; If the soil pH value is greater than 4 and less than or equal to 5.5, it is 2 points; The soil pH value is greater than 5.5 and less than or equal to 7.5, which is 3 points; The soil pH value is greater than 7.5 and less than or equal to 8.5, which is 4 points; The soil pH value is greater than 8.5, which is 5 points; (2.5) Soil temperature scoring criteria: the lower the score, the more corrosive the soil: 1 point if the soil temperature is greater than or equal to 30°C; 2 points if the soil temperature is greater than or equal to 20°C and less than 30°C; 3 points if the soil temperature is greater than or equal to 15°C and less than 20°C; 4 points if the soil temperature is greater than or equal to 10°C and less than 15°C; If the soil temperature is less than 10℃, it is 5 points; (3) Calculate the soil resistivity correction factor and determine the soil corrosion level The comprehensive calculation formula of soil resistivity correction factor K is as follows: K = b1 × soil salt content score + b2 × soil moisture score + b3 × soil porosity score + b4 × soil pH score + b5 × soil temperature score; When the soil resistivity correction coefficient K is greater than or equal to 1 and less than 2.2, the soil is extremely corrosive, the probability of local corrosion or pitting corrosion is extremely high, the probability of uniform corrosion is moderate, and the soil grade is IV; When the soil resistivity correction coefficient K is greater than or equal to 2.2 and less than 3.2, the soil is highly corrosive, the probability of local corrosion or pitting corrosion is moderate, the probability of uniform corrosion is slight, and the soil grade is III; When the soil resistivity correction coefficient K is greater than or equal to 3.2 and less than 4.2, the soil is less corrosive, the probability of local corrosion or pitting corrosion is slight, the probability of uniform corrosion is extremely slight, and the soil grade is II; When the soil resistivity correction coefficient K is greater than or equal to 4.2 and less than or equal to 5, the soil is extremely weakly corrosive, the probability of local corrosion or pitting corrosion is extremely slight, and the probability of uniform corrosion is extremely slight. The soil grade is Grade I. 2) Select the material of the sacrificial anode according to the required protection potential of the metal material of the concrete pile to be protected and the metal material of the concrete pile welding, the soil resistivity of the area where the concrete pile is located and the characteristics of different sacrificial anode materials; including: (1) Determine the factor weight vectors of the three factors for selecting sacrificial anode materials and score the three factors The three factors for selecting sacrificial anode materials are: soil resistivity, the required protection potential of the metal material of the concrete pile to be protected and the metal material of the concrete pile welding, and the open circuit potential of the sacrificial anode material; (1.1) The weights of each factor in selecting sacrificial anode materials are obtained by applying the hierarchical analysis method, which are: The soil resistivity grade weight h1 is 0.528; The required protection potential level weight h2 of the protected concrete pipe pile metal material and the concrete pipe pile welding metal material is 0.332; The open circuit potential grade weight h3 of the sacrificial anode material is 0.140; The grade weights of the three factors form the weight vector H: (1.2) The three factors for selecting sacrificial anode materials are graded, each factor is divided into 3 levels, and each factor is scored separately: Soil resistivity rating: The soil resistivity is greater than or equal to 1Ω·m and less than or equal to 5Ω·m, and the score is 1; The resistivity of the soil is greater than 5Ω·m and less than or equal to 8Ω·m, and the score is 2; The resistivity of the soil is greater than 8Ω·m and less than or equal to 10Ω·m, and the score is 3; Under the copper-copper sulfate reference electrode, the protection potential grade rating required for the protected concrete pipe pile metal material and the concrete pipe pile welding metal material is: The protection potential is greater than or equal to -1.5V and less than or equal to -1.2V, and the score is 1; The protection potential is greater than -1.2V and less than or equal to -1.1V, and the score is 2; The protection potential is greater than -1.1V and less than or equal to -0.85V, and the score is 3; The open circuit potential rating of sacrificial anode materials under the calomel reference electrode is: The open circuit potential is greater than or equal to -1.7V and less than or equal to -1.5V, and the score is 1; The open circuit potential is greater than -1.5V and less than or equal to -1.3V, and the score is 2; The open circuit potential is greater than -1.3V and less than or equal to -1.0V, and the score is 3; (2) Comprehensive evaluation calculation method and selection criteria for sacrificial anode material selection The sacrificial anode material is scored according to the three factors in step (1) to obtain the scoring vector F of the sacrificial anode material: F=[F1,F2,F3] Among them, F1, F2, and F3 are the scoring values of the three factors for selecting sacrificial anode materials; Comprehensive evaluation score K for sacrificial anode material selection sam Calculate as follows: K sam =H T ·F T The selection criteria for sacrificial anode materials are: Comprehensive evaluation score K sam ≤1.2, it is recommended to select a high potential pure magnesium or magnesium-manganese magnesium anode as the sacrificial anode; Comprehensive evaluation score K sam >1.2 and ≤2.2, it is recommended to select magnesium anode of magnesium-aluminum-zinc-manganese system as sacrificial anode; Comprehensive evaluation score K sam >2.2 and ≤3, it is recommended to select magnesium anode or zinc alloy anode of magnesium-aluminum-zinc-manganese system as sacrificial anode 3) According to the shape of the concrete pile to be protected, the metal material of the concrete pile, the metal material of the concrete pile welding, the soil resistivity of the area where the concrete pile is located, and the design life of the sacrificial anode protection device, determine the specific shape and quantity of the sacrificial anode; including: (1) Determine the specific shape of the sacrificial anode based on the determined sacrificial anode material and the internal space of the concrete pile; (2) Number of sacrificial anodes required Where: N is the number of sacrificial anodes, unit: I s is the required protection current, in A; I a It is the output current of a single sacrificial anode, in A; f is the reserve coefficient, which is 1.7 because the foundation concrete piles belong to buried structures; (2.1) Calculate the total protection current I required for the protected concrete piles s : I s =I A ×S 总 S 总 =N×πDL Where: I A For protection current density, unit is mA / m 2 ; S 总 is the total area of steel bars inside the concrete pile, in m 2 ; N is the number of steel bars inside the concrete pile, in pieces; D is the diameter of a single steel bar, in m; L is the length of a single steel bar, in m; When the soil resistivity correction coefficient K is greater than or equal to 1 and less than 2.2, the soil grade is IV, the soil is extremely corrosive, and I A Take 60~100mA / m 2 ; When the soil resistivity correction coefficient K is greater than or equal to 2.2 and less than 3.2, the soil grade is Grade III, the soil is highly corrosive, and Grade I A Take 30~60mA / m 2 ; When the soil resistivity correction coefficient K is greater than or equal to 3.2 and less than 4.2, the soil grade is II, the soil corrosiveness is weak, and I A Take 10~30mA / m 2 ; When the soil resistivity correction coefficient K is greater than or equal to 4.2 and less than or equal to 5, the soil grade is Grade I, the soil corrosiveness is extremely weak, and Grade I A Take 5~10mA / m 2 ; (2.2) Output current of a single sacrificial anode Where: ΔU is the driving voltage, unit V; When a high-potential pure magnesium or magnesium-manganese magnesium anode is selected as a sacrificial anode, ΔU is 0.18V; When a magnesium anode or zinc alloy anode of the magnesium-aluminum-zinc-manganese system is selected as a sacrificial anode, ΔU is 0.2V; R is the total resistance of the loop, which is approximately equal to the sacrificial anode grounding resistance R A , unit Ω; (2.3) Calculate the sacrificial anode grounding resistance: Since the concrete piles are below the ground and in a water environment, the grounding resistance R A Calculated according to water connection resistance: Where: R A is the sacrificial anode grounding resistance, unit: Ω; l is the length of the sacrificial anode, in cm; ρ is the resistivity of the medium, in Ω·cm; t1 is the equivalent substitution coefficient; r is the equivalent radius of the sacrificial anode, Unit: cm; A is the cross-sectional area of the sacrificial anode cross section, in cm 2 ; (3) Sacrificial anode service life When designing a sacrificial anode protection device, the total number of sacrificial anodes output current and sacrificial anode consumption rate are used to calculate the service life of the sacrificial anodes. After installing the sacrificial anodes, the total number of sacrificial anodes output current I is measured. a总 and sacrificial anode consumption rate to verify the sacrificial anode service life. Where: T is the sacrificial anode service life, unit is a; W is the net mass of the sacrificial anode, in kg; ω is the sacrificial anode consumption rate, kg / (A·a); When a high potential pure magnesium or magnesium-manganese magnesium anode is used as a sacrificial anode, ω is taken as 7.5kg / (A·a) When magnesium anode or zinc alloy anode of magnesium-aluminum-zinc-manganese system is used as sacrificial anode, ω is taken as 5kg / (A·a) I a总 Output current for the total number of sacrificial anodes, unit A 4) Select the installation location of the sacrificial anode according to the shape of the concrete pipe pile to be protected and install it.
2. The method for selecting a sacrificial anode according to claim 1, characterized in that: Step 4) includes: First, determine the electrical connection status of the steel cage inside the concrete pipe pile. If the electrical connection is normal, choose to install the sacrificial anode; if the electrical connection is abnormal, repair the steel bars by welding to ensure effective electrical connection between the steel cages inside the concrete pipe pile, and then choose to install the sacrificial anode.
Citation Information
Patent Citations
Anti-corrosion protection system for spiral ground piles and application method of anti-corrosion protection system
CN109097782A
PHC pipe pile bottom end plate cathodic protection anticorrosion system and method
CN111270245A
Sacrificial anode protect pile
CN205205232U
Method for electrolytic protecting of concrete pile reinforcing rods
KR1019980009522A