A fast baking method for battery
By using the combination of activation gas and carrier gas in the battery baking process, the existence form of water molecules is changed, and the problems of low baking efficiency and difficulty in removing combined water in the prior art are solved, efficient water removal is achieved, and battery is improved Quality and safety performance.
Patent Information
- Application Number
- CN202211332746.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-10-28
AI Technical Summary
In the existing battery manufacturing process, rapid baking efficiency is low and bound water cannot be effectively removed. Especially for materials with strong water absorption, the moisture cannot be reduced below 700ppm, affecting battery quality and safety performance.
Using the combination of activated gases such as ammonia, carbon dioxide and formaldehyde, as well as carrier gases such as nitrogen, argon and helium, the presence form of water molecules is changed through chemical methods, and the combination of ammonia and water molecules is used to significantly reduce the boiling point of the mixture. This enables efficient removal of moisture at low energy consumption.
It achieves efficient removal of moisture at lower energy consumption, improves baking efficiency, and ensures the product quality and safe use of the battery.
Smart Images

Figure CN115763986B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a rapid baking method for batteries. Background Art
[0002] The gradual depletion of fossil energy and the increasingly serious greenhouse effect have prompted researchers to continuously explore sustainable and clean energy. Since Sony first commercialized lithium-ion batteries in 1991, lithium-ion batteries have been widely used in 3C digital products and power batteries. Since lithium-ion batteries have advantages over traditional lead-acid batteries in cycle life, volume energy density, and mass energy density, many technicians have been committed to the commercialization of lithium-ion batteries in the past 20 years. Due to the supply shortage of lithium elements, researchers regard sodium-ion batteries as an important direction to supplement lithium-ion batteries. In 2021, Contemporary Amperex Technology Co., Ltd. launched its first sodium-ion battery, which opened the prelude to the industrialization of sodium-ion batteries.
[0003] In the battery manufacturing process, baking is a crucial step to ensure the product quality and safety of the battery. Many steps in the battery cell production process require baking, such as pole piece baking, cell baking, positive electrode active material, conductive agent, binder baking, etc. The most critical one is the vacuum baking before liquid injection, and the moisture content is generally required to be less than 300ppm.
[0004] In order to achieve fast baking and meet the moisture content standard, the industry currently generally adopts high vacuum heating to 80-120℃ baking. The heating methods include heat radiation, heat conduction and heat convection. Through the optimization of baking equipment and processes, the baking efficiency can be achieved 4 to 7 hours per batch. For example, patent CN112864463B uses gradient vacuuming to improve baking efficiency.
[0005] The positive and negative electrodes of lithium-ion batteries and sodium-ion batteries are typical porous electrodes with a porosity of 20%-40% and a high pore tortuosity. The active material is a micro-nano material with a large specific surface area and easy water absorption. Existing process methods and equipment are all centered around how to quickly heat and reduce pressure to improve efficiency. Such methods can only accelerate the baking rate of unbound water to a certain extent, but have no effect on bound water. Since baking is usually carried out in the presence of a diaphragm, it is impossible to remove bound water by increasing the temperature. For some materials with strong water absorption, when the moisture content is baked to 700ppm, even if the baking time is delayed, the water content cannot be further reduced. Summary of the invention
[0006] The object of the present invention is to provide a rapid baking method for a battery. The rapid baking method of the present invention can achieve efficient removal of moisture with lower energy consumption.
[0007] The invention provides a rapid baking method for a battery. During the baking process, an activated gas and a carrier gas are introduced. The activated gas comprises one or more of ammonia, carbon dioxide and formaldehyde; the carrier gas is one or more of nitrogen, argon and helium; and the volume fraction of the activated gas is 0.1-5%.
[0008] Preferably, the rapid baking method comprises the following steps:
[0009] A) placing the battery cell in a baking device, evacuating the battery cell, introducing an activated gas and a carrier gas for preheating;
[0010] B) vacuuming and heat-insulating the preheated battery cells;
[0011] C) repeating steps A) and B) at least once;
[0012] D) Fill the baking equipment with nitrogen to normal pressure, perform nitrogen cooling cycle, and complete the baking.
[0013] Preferably, the absolute gas pressure during preheating is 30000-99000 Pa.
[0014] Preferably, the preheating temperature is 80-115°C.
[0015] Preferably, the total preheating time is 10 to 120 minutes.
[0016] Preferably, the vacuum degree of the heat preservation and pressure preservation is 10-100 Pa.
[0017] Preferably, the temperature of the heat preservation and pressure preservation is 80-115°C.
[0018] Preferably, the heat preservation and pressure preservation time is 10 to 120 minutes.
[0019] Preferably, the nitrogen cooling cycle is performed at least twice.
[0020] Preferably, in each nitrogen cooling cycle, the normal pressure is first maintained for 0.1 to 10 min, and then the vacuum is evacuated and maintained at a vacuum degree of 10 to 200 Pa for 0.1 to 10 min.
[0021] The present invention provides a rapid baking method for a battery, comprising the following steps: A) placing a battery cell in a baking device, introducing an activated gas and a carrier gas after vacuuming for preheating; the activated gas includes one or more of ammonia, carbon dioxide and formaldehyde; the carrier gas is one or more of nitrogen, argon and helium; the volume fraction of the activated gas is 0.1-5%; B) keeping the preheated battery cell warm and pressurized; C) repeating steps A) and B) at least once; D) filling the baking device with nitrogen to normal pressure, performing a nitrogen cooling cycle, and completing the baking. The method changes the existing form of water molecules by a chemical method, and by introducing ammonia at any time during the baking process, the ammonia molecules are combined with bound water and / or unbound water through hydrogen bonds or chemical bonds, and the ammonia molecules can significantly reduce the boiling point of the mixture after combining with water, so that the efficient removal of water can be achieved with lower energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0023] Figure 1 The figure is a schematic diagram of the process flow of the rapid baking method of the present invention. DETAILED DESCRIPTION
[0024] The present invention provides a rapid baking method for a battery, comprising the following steps:
[0025] A) placing the battery cell in a baking device, evacuating the battery cell, introducing an activated gas and a carrier gas for preheating;
[0026] The activation gas includes one or more of ammonia, carbon dioxide and formaldehyde; the carrier gas is one or more of nitrogen, argon and helium; the volume fraction of the activation gas is 0.1-5%;
[0027] B) Keeping the preheated battery cell warm and pressurized;
[0028] C) repeating steps A) and B) at least once;
[0029] D) Fill the baking equipment with nitrogen to normal pressure, perform nitrogen cooling cycle, and complete the baking.
[0030] Preparation
[0031] Place the cells in the baking apparatus.
[0032] In the present invention, the battery cell can be a lithium ion battery cell or a sodium ion battery cell, and the present invention does not specifically limit this. In the present invention, the baking equipment is a baking equipment commonly used by those skilled in the art.
[0033] Introducing activation gas and carrier gas
[0034] The box containing the battery cells is evacuated, and then activated gas and carrier gas are introduced.
[0035] In the present invention, the activated gas is a small molecule that can combine with water molecules through hydrogen bonds or chemical bonds to form a low-boiling substance, preferably one or more of ammonia, carbon dioxide and formaldehyde; the carrier gas is one or more of nitrogen, argon and helium; the volume fraction of the activated gas in the total amount of the activated gas and the carrier is preferably 0.1-5%, more preferably 1-4%, such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, preferably a range value with any of the above values as the upper or lower limit.
[0036] Warm-up phase
[0037] Heat the box containing the battery cells for preheating.
[0038] In the present invention, during the preheating process, the temperature is raised to 80-115°C, preferably 85-110°C, such as 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, preferably a range value with any of the above values as the upper or lower limit; the total time of the preheating process is preferably 10-120min, more preferably 20-100min, such as 10min, 20min, 30min, 40min, 50min, 60min, 70min, 80min , 90min, 100min, 110min, 120min, preferably a range value with any of the above values as the upper or lower limit; the absolute gas pressure in the preheating process is preferably 30000-99000Pa, more preferably 50000-80000Pa, such as 30000Pa, 40000Pa, 50000Pa, 60000Pa, 70000Pa, 80000Pa, 90000Pa, 99000Pa, preferably a range value with any of the above values as the upper or lower limit.
[0039] Heat preservation and pressure holding stage
[0040] After preheating, the present invention evacuates and maintains a vacuum degree of 10-200 Pa, and maintains the temperature and pressure inside the box at 80-115° C.
[0041] In the present invention, the vacuum degree of the heat preservation and pressure holding is preferably 10-200Pa, more preferably 50-150Pa, such as 10Pa, 20Pa, 30Pa, 40Pa, 50Pa, 60Pa, 70Pa, 80Pa, 90Pa, 100Pa, 110Pa, 120Pa, 130Pa, 140Pa, 150Pa, 160Pa, 170Pa, 180Pa, 190Pa, 200Pa, preferably a range value with any of the above values as the upper or lower limit; the temperature of the heat preservation and pressure holding is preferably 80-115°C, preferably 8 The temperature of the mixture is preferably 5 to 110°C, such as 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, preferably a range value with the above arbitrary numerical values as the upper or lower limit; the time for heat preservation and pressure holding is preferably 10 to 120min, more preferably 20 to 100min, such as 10min, 20min, 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min, 120min, preferably a range value with the above arbitrary numerical values as the upper or lower limit.
[0042] Cycle Phase
[0043] The present invention preferably repeats the above-mentioned activation gas and carrier introduction stage - preheating stage - heat and pressure maintenance stage at least once.
[0044] Nitrogen cooling cycle stage
[0045] Nitrogen is filled into the baking equipment to normal pressure, and first maintained at normal pressure for 0.1 to 10 minutes, and then evacuated, and maintained at a vacuum degree of 10 to 200 Pa for 0.1 to 10 minutes to complete a nitrogen cooling cycle. The present invention preferably repeats the nitrogen cooling cycle at least once, that is, performs at least two nitrogen cooling cycles.
[0046] In the present invention, the time maintained at normal pressure is preferably 0.1 to 10 min, more preferably 1 to 8 min, such as 0.1 min, 0.5 min, 1 min, 1.5 min, 2 min, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min, 5 min, 5.5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min, 9.5 min, 10 min, preferably a range value with any of the above values as the upper or lower limit.
[0047] The vacuum degree is preferably 10-200 Pa, more preferably 50-150 Pa, such as 10 Pa, 20 Pa, 30 Pa, 40 Pa, 50 Pa, 60 Pa, 70 Pa, 80 Pa, 90 Pa, 100 Pa, 110 Pa, 120 Pa, 130 Pa, 140 Pa, 150 Pa, 160 Pa, 170 Pa, 180 Pa, 190 Pa, 200 Pa, preferably a range value with any of the above values as the upper or lower limit; the time maintained under the above vacuum degree The time interval is preferably 0.1-10 min, more preferably 1-8 min, such as 0.1 min, 0.5 min, 1 min, 1.5 min, 2 min, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min, 5 min, 5.5 min, 6 min, 6.5 min, 7 min, 7.5 min, 8 min, 8.5 min, 9 min, 9.5 min, 10 min, preferably with any of the above values as the upper or lower limit of the range value.
[0048] The present invention provides a rapid baking method for a battery, comprising the following steps: A) placing a battery cell in a baking device, introducing an activated gas and a carrier gas after vacuuming for preheating; the activated gas includes one or more of ammonia, carbon dioxide and formaldehyde; the carrier gas is one or more of nitrogen, argon and helium; the volume fraction of the activated gas is 0.1-5%; B) keeping the preheated battery cell warm and pressurized; C) repeating steps A) and B) at least once; D) filling the baking device with nitrogen to normal pressure, performing a nitrogen cooling cycle, and completing the baking. The method changes the existing form of water molecules by a chemical method, and by introducing ammonia at any time during the baking process, the ammonia molecules are combined with bound water and / or unbound water through hydrogen bonds or chemical bonds, and the ammonia molecules can significantly reduce the boiling point of the mixture after combining with water, so that the efficient removal of water can be achieved with lower energy consumption.
[0049] In order to further illustrate the present invention, a rapid baking method of a battery provided by the present invention is described in detail below in conjunction with embodiments, but it should not be construed as limiting the scope of protection of the present invention.
[0050] Example 1
[0051] (1) Preparation stage: put the assembled lithium iron phosphate battery into the baking box;
[0052] (2) Introduction of activation gas and carrier gas: The box containing the battery cells is evacuated to 50 Pa, and then filled with nitrogen and ammonia until the absolute pressure is 65000 Pa; preferably, the ammonia system fraction is 2%;
[0053] (3) Preheating stage: The box containing the battery cells is heated to 95°C and the total preheating time is 30 minutes;
[0054] (4) Insulation and pressure holding stage: the preheated battery is evacuated and the vacuum degree is maintained at 100 Pa, and the temperature inside the box is maintained at 95°C for 60 min;
[0055] (5) Cycle stage: repeat the above steps (2) to (4) for 6 cycles;
[0056] (6) Nitrogen cooling cycle stage: nitrogen is filled into the baking device to normal pressure and maintained at normal pressure for 5 min, then vacuum is evacuated and maintained at a vacuum degree of 100 Pa for 5 min;
[0057] (7) Repeat the above step (6) and cycle cooling ventilation twice.
[0058] The positive and negative electrodes of the battery cell were tested for water content using a Karl Fischer titrator at a test temperature of 170°C.
[0059] Example 2
[0060] Compared with Example 1, the activated gas is changed to carbon dioxide, and the others remain the same.
[0061] Example 3
[0062] Compared with Example 1, the activated gas is changed to formaldehyde, and the others remain the same.
[0063] Example 4
[0064] The volume fraction of the activated gas was changed to 0.2% relative to Example 1, and the others remained the same.
[0065] Example 5
[0066] The volume fraction of the activated gas is changed to 4% relative to Example 1, and the others remain the same.
[0067] Example 6
[0068] Compared with Example 1, the lithium iron phosphate battery cell is changed to a sodium ion battery cell, wherein the positive electrode of the sodium ion battery cell uses Prussian white, and the rest remains the same.
[0069] Comparative Example 1
[0070] The volume fraction of the activated gas is changed to 0% relative to Example 1, and the others remain the same.
[0071] Comparative Example 2
[0072] The volume fraction of the activated gas is changed to 0% relative to Example 6, and the others remain the same.
[0073] The moisture content of the battery cells after baking in the embodiment and the comparative example is shown in Table 1:
[0074] Table 1 Water content of the battery cells after baking in the embodiments and comparative examples
[0075]
[0076]
[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A rapid baking method for a battery, comprising the following steps: A) Place the battery cell in a baking device, evacuate the battery cell, and introduce activation gas and carrier gas for preheating. The activation gas includes one or more of ammonia, carbon dioxide and formaldehyde; the carrier gas is one or more of nitrogen, argon and helium; the volume fraction of the activation gas is 0.1-5% B) Evacuate the preheated battery cells to keep them warm and pressurized; C) Repeat steps A) and B) at least once; D) Fill the baking equipment with nitrogen to normal pressure, perform nitrogen cooling cycle, and complete the baking.
2. The rapid baking method according to claim 1, characterized in that: The absolute air pressure during the preheating is 30000~99000Pa.
3. The rapid baking method according to claim 2, characterized in that: The preheating temperature is 80-115°C.
4. The rapid baking method according to claim 3, characterized in that: The total preheating time is 10~120min.
5. The rapid baking method according to claim 1, characterized in that: The vacuum degree of the heat preservation and pressure preservation is 10~100pa.
6. The rapid baking method according to claim 5, characterized in that: The temperature of the heat preservation and pressure preservation is 80-115°C.
7. The rapid baking method according to claim 6, characterized in that: The time of heat preservation and pressure preservation is 10 to 120 minutes.
8. The rapid baking method according to claim 1, characterized in that: The nitrogen cooling cycle was performed at least twice.
9. The rapid baking method according to claim 8, characterized in that: In each nitrogen cooling cycle, first maintain normal pressure for 0.1~10 minutes, then evacuate and maintain the vacuum degree at 10~200Pa for 0.1~10 minutes.
Citation Information
Patent Citations
A rapid baking method for square lithium-ion batteries
CN112864463B
Method of drying electrode assemblies
CN107871853A
Electrode wetting method, electrode and battery
CN112736287A
Rapid baking method for square lithium ion battery
CN112864463A
Battery cell baking method
CN113363409A