A kind of hot-adhesive modified asphalt waterproof coating and its preparation method and application

Through the combination of room temperature solid hot-adhesive modified asphalt waterproofing coating and modified asphalt waterproofing membrane, the existing hot-melt modified asphalt waterproofing membrane laying process solves the problems of many overlapping seams, low reliability and safety hazards of open flame baking. problem, achieving no smoke emissions and efficient waterproof performance, improving the waterproof durability of concrete pavements and bridge decks.

CN115772368BActive Publication Date: 2024-10-18BEIJING RAILWELD NEW MATERIAL TECH CO LTD +4
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202211510463.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2024-10-18
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

The existing hot-melt modified asphalt waterproofing membrane laying process has many overlapping seams, low reliability, and poor edge sealing effect, and the open flame baking process has safety hazards and environmental pollution problems.

Method used

Provides a room temperature solid hot-adhesive modified asphalt waterproof coating. The formula includes asphalt, modifier, binder, softener, plasticizer, bonding compensator and filler, and is prepared by low-temperature heating treatment (not higher than 160°C) , applied on the concrete base by spraying or scraping, and paved in combination with modified asphalt waterproofing membrane.

Benefits of technology

It achieves open flame-free construction, improves the reliability and durability of the waterproofing system, enhances the adhesion between the membrane and the base surface, reduces smoke emissions, and ensures the adhesion, airtightness and weather resistance of the composite waterproofing system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003968922640000051
    Figure BDA0003968922640000051
  • Figure BDA0003968922640000061
    Figure BDA0003968922640000061
  • Figure BDA0003968922640000062
    Figure BDA0003968922640000062
Patent Text Reader

Abstract

The present invention provides a hot-adhesive modified asphalt waterproof coating and a preparation method thereof, as well as an application in a concrete pavement and a bridge deck waterproof system. The hot-adhesive modified asphalt waterproof coating is solid at room temperature and is composed of: 40-55% asphalt, 5-15% modifier, 11-19% binder, 1-6% bonding compensator, 12-21% softener, 1-5% plasticizer and 3-8% filler by mass percentage. The working temperature of the asphalt waterproof coating of the present invention is lower than 160°C and does not generate smoke; in addition to having excellent impermeability, low-temperature flexibility (-30°C) and fatigue resistance, it also has a high elongation at break and bonding strength, is fully bonded to the base surface and the coiled material, and does not solidify for a long time, so that the overlapping joints of the coiled material are reliably bonded, thereby improving the reliability and durability of the waterproof system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymers, and in particular relates to a hot-adhesive modified asphalt waterproof coating for a waterproof system of a concrete pavement or bridge deck and a preparation method thereof. Background Art

[0002] Concrete pavement, especially the bridge deck waterproofing system of concrete bridges (including highway bridges and railway bridges) is an important technical means to improve the durability of the structure. The waterproofing system of concrete roads generally adopts the method of first laying a hot-melt modified asphalt waterproofing membrane layer on the concrete base, and then pouring a certain thickness of concrete or asphalt as a protective layer. The waterproof performance of the bridge deck depends on whether the membrane can be completely bonded to the base and whether the membranes are firmly overlapped without gaps. When laying hot-melt modified asphalt waterproofing membranes, the membranes are arranged first, cut to the exact size, and each roll is rolled back from the end to the middle. The isolation film is melted with flames, and then rolled forward immediately to make the membrane completely bonded to the base, and then the other half of the membrane is repeated. The subsequent membranes are staggered at the end overlap. Such a laying process results in more overlaps of the membranes and relatively low reliability; and the edge sealing effect of waterproof walls and drainage holes is not easy to guarantee. At the same time, the open flame baking process has certain safety hazards and is also prone to environmental pollution. Summary of the invention

[0003] In view of the deficiencies of the prior art, the present invention provides a hot-adhesive modified asphalt waterproof coating. The asphalt waterproof coating of the present invention is solid at room temperature and is easy to store and transport. The asphalt waterproof coating and the modified asphalt waterproof coiled material thereon replace the traditional hot-melt modified asphalt waterproof coiled material, and no open flame is required at the construction site; the solid asphalt waterproof coating in the prior art needs to be heated to above 180°C during construction, while the heating temperature of the asphalt waterproof coating of the present invention is not higher than 160°C during construction. Therefore, the asphalt waterproof coating of the present invention does not generate smoke during construction. In addition to excellent impermeability, low-temperature flexibility (-30°C) and fatigue resistance, the asphalt waterproof coating of the present invention also has a higher elongation at break and bonding strength, is fully bonded to the base surface and the coiled material, and does not solidify for a long time, so that the overlapping joints of the coiled material are reliably bonded, thereby improving the reliability and durability of the waterproof system.

[0004] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0005] A hot-adhesive modified asphalt waterproof coating, which is solid at room temperature and consists of the following components by mass percentage:

[0006] Asphalt 40-55%, modifier 5-15%, binder 11-19%, binder compensator 1-6%, softener 12-21%, plasticizer 1-5% and filler 3-8%;

[0007] Wherein, the modifier is selected from one or more of flexible epoxy resin, polyisocyanate, chloroprene rubber, waste rubber powder, polyethylene resin, polypropylene resin, phenolic resin, SBR, SBS, polyethylene terephthalate (PET), ethylene vinyl acetate (EVA) and coumarone resin;

[0008] The binder is selected from one or more of rosin resin, terpene resin, petroleum resin, medium molecular weight polyisobutylene with a viscosity average molecular weight of 35000-55000, T612 viscosity index improver, T613 viscosity index improver and T614 viscosity index improver;

[0009] The softener is selected from one or more of turpentine, chlorinated paraffin, white oil, furfural-reduced oil, naphthenic oil and vegetable oil;

[0010] The plasticizer is selected from one or more of cobalt naphthenate, diisobutyl cyclohexanedicarboxylate (DIBCH), trioctyl trimellitate (TOTM), environmentally friendly tributyl citrate (TBC), dioctyl phthalate (DOP) and dioctyl adipate (DOA);

[0011] The bonding compensator is selected from one or more of alicyclic epoxysilane SCA-E86E, bis(acetylacetonato)diisopropyl titanate, 3-aminopropyltriethoxysilane and diisopropoxy acetoacetic acid oleate aluminate;

[0012] The filler is selected from one or more of talc powder, light calcium carbonate and mica powder.

[0013] Preferably, the asphalt is selected from one or both of heavy traffic road petroleum asphalt 70# and 90#.

[0014] More preferably, the asphalt has a needle penetration (25°C, 100g, 5s, 0.1mm) of 60-100 and a softening point of 45-55°C.

[0015] Preferably, the modifier is selected from one or more of flexible epoxy resin, chloroprene rubber, polypropylene resin, phenolic resin, SBR, SBS, ethylene vinyl acetate (EVA) and coumarone resin.

[0016] Preferably, the binder is selected from one or both of medium molecular weight polyisobutylene with a viscosity average molecular weight of 35,000-55,000 and T612 viscosity index improver.

[0017] Preferably, the softener is selected from one or both of naphthenic oil and white oil.

[0018] Preferably, the plasticizer is selected from one or both of dioctyl phthalate and diisobutyl cyclohexanedicarboxylate.

[0019] Preferably, the adhesion compensating agent is selected from one or both of alicyclic epoxysilane SCA-E86 and diisopropoxy acetoacetic acid oleate aluminate.

[0020] Preferably, the filler is selected from one or both of light calcium carbonate and talc.

[0021] Another object of the present invention is to provide a method for preparing the hot melt modified asphalt coating, comprising the following steps:

[0022] a) Prepare the components according to the ratio;

[0023] b) Place the asphalt in a constant temperature oven at 120-140°C, heat it until it becomes fluid, and continue to keep it warm. The heating and insulation time should be at least 2 hours;

[0024] c) weighing the asphalt in a flowing state obtained in step b), transferring it into a container equipped with a heat preservation and stirring device, slowly adding a modifier, a softener and a plasticizer, stirring at a low speed at 140 to 160° C. for 1 to 2 hours, keeping the temperature constant, and using a high-speed shearing machine to continuously shear for 1 to 2 hours;

[0025] d) Add the binder, filler and binder compensator to the mixed system of step c), keep the temperature constant, continue to use the high-speed shearing machine, continue shearing for 1 to 2 hours, cool, cut into blocks, seal and insulate for storage, and obtain the product.

[0026] Preferably, in step c), the rotation speed of the low-speed stirring is 50 to 200 r / min.

[0027] Preferably, in steps c) and d), the high-speed shear rate is 1000-2000 rpm.

[0028] The third object of the present invention is to provide the use of the hot melt modified asphalt coating or the hot melt modified asphalt coating prepared by the above preparation method in concrete pavement and bridge deck waterproofing systems, comprising the following steps:

[0029] I. heating the hot-adhesive modified asphalt waterproof coating to a fluid state, the heating temperature is 150-160° C., and the discharge temperature is 150-160° C.;

[0030] II. Spray or scrape the flowing hot-adhesive modified asphalt waterproof coating on the upper surface of the concrete base and the lower surface of the modified asphalt waterproof membrane, and immediately lay the modified asphalt waterproof membrane on the concrete base, spraying, laying, rolling and venting at the same time to achieve a full adhesion effect; the thickness of the hot-adhesive modified asphalt waterproof coating on the concrete base is 0.8 to 1.5 mm.

[0031] The hot melt modified asphalt waterproof coating provided by the present invention has various components that work together. Among them:

[0032] The binder improves the bonding degree between asphalt and modifier, and at the same time increases the bonding force between the hot-adhesive modified asphalt waterproof coating and the roll material and the base surface, thereby improving the extensibility of the material.

[0033] The softener is used to dissolve the modifier, so that its chain segments are fully opened and the fusion with asphalt is promoted.

[0034] The plasticizer is an asphalt additive that can effectively improve the flexibility and tensile properties of the material and enhance its impact resistance while improving the low temperature resistance and high temperature viscosity of asphalt. In addition, the plasticizer also has a certain improvement effect on the temperature sensitivity of asphalt.

[0035] The bonding compensator further improves the interfacial bonding strength between the material and the waterproof membrane and the concrete base surface, thereby ensuring the integrity and water penetration resistance of the composite waterproof system.

[0036] The filler further improves the high temperature resistance of the material, absorbs small molecule oil substances, and reduces the oil permeability of the material.

[0037] In summary, the hot melt modified asphalt waterproof coating provided by the present invention has a solid content of ≥98%, a hot melt temperature of less than 160°C, and no smoke is generated during the heating process. Replacing the traditional hot melt asphalt waterproof membrane with the hot melt modified asphalt waterproof coating and modified asphalt waterproof membrane of the present invention can achieve construction without open flames and no smoke emission during construction. The hot-adhesive modified asphalt waterproof coating of the present invention can fully coat and level the rough concrete base surface below it, fully adhere to and penetrate the waterproof membrane thereon, and ensure that the composite waterproof system has good adhesion, airtightness, weather resistance, elongation and crack tracking. DETAILED DESCRIPTION

[0038] The present invention is described below with reference to specific examples. It will be appreciated by those skilled in the art that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention in any way.

[0039] The experimental methods in the following examples are all conventional methods unless otherwise specified. The raw materials, reagents, etc. used in the following examples are all commercially available products unless otherwise specified. The purchase of some raw materials is as follows:

[0040] Alicyclic epoxysilane SCA-E86E, diisopropoxy acetoacetic acid oleate aluminate: purchased from Nanjing Nengde New Materials Technology Co., Ltd.;

[0041] Flexible epoxy resin YP-50: purchased from Wuhan Yipeng Material Technology Co., Ltd.;

[0042] SBR1502: PetroChina Company Limited;

[0043] SBS2336: Guangzhou Xinnuo New Material Technology Co., Ltd.;

[0044] Polypropylene resin GM750E: Ningbo Chaowang New Materials Co., Ltd.

[0045] Tert-butyl phenolic resin 2402: Shandong Maofa Chemical Co., Ltd.;

[0046] Neoprene SN244X: Guangzhou Qianyiyuan Synthetic Material Technology Co., Ltd.;

[0047] Ethylene vinyl acetate: Shandong Kejian Chemical Co., Ltd.;

[0048] HRD550 medium molecular weight polyisobutylene: viscosity average molecular weight 35000-55000, Jinan Xinhou Trading Co., Ltd.;

[0049] Coumarone resin: Shandong Xiangzhao New Materials Co., Ltd.

[0050] The hot-adhesive modified asphalt waterproof coatings of the following examples and comparative examples are prepared by the following steps:

[0051] a) Prepare the components according to the ratio;

[0052] b) Place the asphalt in a constant temperature oven at 120-140°C, heat it until it becomes fluid, and continue to keep it warm. The heating and insulation time should be at least 2 hours;

[0053] c) weighing the asphalt in a flowing state obtained in step b), transferring it into a container with a heat preservation and stirring device, slowly adding a modifier, a softener and a plasticizer, stirring at 50-200 rpm at 140-160° C. for 1-2 hours, keeping the temperature constant, using a high-speed shearing machine, with a shear rate of 1000-2000 rpm, and continuously shearing for 1-2 hours;

[0054] d) Add the binder, filler and binder compensator to the mixed system of step c), keep the temperature unchanged, continue to use the high-speed shearing machine, the shear rate is 1000-2000rpm, continue shearing for 1-2h, cool, cut into blocks, seal and store in a heat-insulated manner, and obtain.

[0055] The specific construction steps of the hot-adhesive modified asphalt waterproof coatings of the following embodiments and comparative examples when applied to the waterproof system are as follows:

[0056] I. heating the hot-adhesive modified asphalt waterproof coating to a fluid state, the heating temperature is 150-160° C., and the discharge temperature is 150-160° C.;

[0057] II. Spray or scrape the flowing hot-adhesive modified asphalt waterproof coating on the upper surface of the concrete base and the lower surface of the modified asphalt waterproof membrane, and immediately lay the modified asphalt waterproof membrane on the concrete base, spraying, laying, rolling and venting at the same time to achieve a full adhesion effect; the thickness of the hot-adhesive modified asphalt waterproof coating on the concrete base is 0.8 to 1.5 mm.

[0058] Embodiments 1 to 7 A hot-adhesive modified asphalt waterproof coating

[0059] The raw material ratios of the hot-adhesive modified asphalt waterproof coatings of Examples 1 to 7 are shown in Table 1, and they were prepared and applied according to the above method. The physical and mechanical properties are shown in Table 2.

[0060] Comparative Examples 1 to 3: A hot-adhesive modified asphalt waterproof coating

[0061] The raw material ratios of the hot-adhesive modified asphalt waterproof coatings of Comparative Examples 1 to 3 are shown in Table 3, and they were prepared and constructed according to the above method. The physical and mechanical properties are shown in Table 4.

[0062] Table 1 Formulation of the hot-adhesive modified asphalt waterproof coating of Examples 1 to 7 (unit: kg)

[0063]

[0064] Table 2 Physical and mechanical properties of Examples 1 to 7

[0065]

[0066] Table 3 Formula of hot-adhesive modified asphalt waterproof coating of comparative example 1 to 2 (unit: kg)

[0067]

[0068] Table 4 Physical and mechanical properties of hot melt modified asphalt coatings of comparative examples 1 to

[0069]

[0070] In Examples 1-7 of the present invention, the impermeability, low-temperature flexibility and elongation at break of the material are greatly improved by compounding modified asphalt and plasticizer with resin and rubber, and the elongation at break is more than 650%; the cohesion of the material, the bonding strength with the coiled material, and the bonding strength with the concrete are greatly improved by the binder and the bonding compensator. In particular, the aluminate coupling agent reacts with the filler or the surface of the substrate through a protonation reaction, and there is no need for hydroxyl groups on the surface of the filler, nor does it require pre-hydrolysis or residual moisture on the surface of the filler, and it has good bonding with asphalt and modifiers.

[0071] In Comparative Example 1, the amount of filler is relatively small, only 1%, and the heat resistance and low temperature resistance of the coating are greatly reduced; in Comparative Example 2, the amount of filler is large, up to 15%, which affects the elongation at break and bonding strength of the coating; in Comparative Example 3, the amount of bonding compensator is 0.1%, and the bonding strength and impermeability of the coating are low; in Comparative Example 4, the amount of asphalt is only 30%, the high temperature resistance and low temperature resistance of the coating are poor, the elongation at break is small, and the ductility of the coating is poor, which is manifested as poor bonding strength with concrete.

Claims

1. A hot-adhesive modified asphalt waterproof coating, which is solid at room temperature and consists of the following components by mass percentage: 70# heavy road petroleum asphalt 40%, flexible epoxy resin YP-50 14%, SBR2336 1%, HRD550 medium molecular weight polyisobutylene 18%, naphthenic oil 17%, dioctyl phthalate 4%, alicyclic epoxy silane SCA-E86E 3% and light calcium carbonate 3%; in, Flexible epoxy resin and SBR2336 are modifiers, HRD550 medium molecular weight polyisobutylene is a binder, naphthenic oil is a softener, dioctyl phthalate is a plasticizer, alicyclic epoxy silane SCA-E86E is a bonding compensator, and light calcium carbonate is a filler.

2. A hot-adhesive modified asphalt waterproof coating, which is solid at room temperature and consists of the following components by mass percentage: 70# heavy road petroleum asphalt 50%, SBR2336 1%, polypropylene resin GM750E 14%, HRD550 medium molecular weight polyisobutylene 15%, naphthenic oil 15%, dioctyl phthalate 1%, diisopropoxy acetoacetic acid oleate aluminate 1% and light calcium carbonate 3%; in, SBR2336 and polypropylene resin GM750E are modifiers, HRD550 medium molecular weight polyisobutylene is a binder, cyclohexane oil is a softener, dioctyl phthalate is a plasticizer, diisopropoxy acetoacetic acid oleate aluminate is a bonding compensator, and light calcium carbonate is a filler.

3. A hot-adhesive modified asphalt waterproof coating, which is solid at room temperature and consists of the following components by mass percentage: 70# heavy-duty road petroleum asphalt 55%, tert-butyl phenolic resin 5%, T612 viscosity index improver 19%, naphthenic oil 12%, diisobutyl cyclohexanedicarboxylate 2%, alicyclic epoxy silane SCA-E86E 2% and talc 5%; in, Tert-butyl phenolic resin is a modifier, T612 viscosity index improver is a binder, naphthenic oil is a softener, diisobutyl cyclohexanedicarboxylate is a plasticizer, alicyclic epoxy silane SCA-E86E is a bonding compensator, and talc is a filler.

4. The method for preparing the hot-adhesive modified asphalt waterproof coating according to any one of claims 1 to 3 comprises the following steps: a) Prepare the components according to the ratio; b) Place the asphalt in a constant temperature oven at 120-140°C, heat it until it becomes fluid, and continue to keep it warm. The heating and insulation time should be at least 2 hours; c) weighing the asphalt in a flowing state obtained in step b), transferring it into a container equipped with a heat preservation and stirring device, slowly adding a modifier, a softener and a plasticizer, stirring at a low speed at 140 to 160° C. for 1 to 2 hours, keeping the temperature constant, and using a high-speed shearing machine to continuously shear for 1 to 2 hours; d) Add the binder, filler and bonding compensator to the mixed system of step c), keep the temperature constant, continue to use the high-speed shearing machine, continue shearing for 1 to 2 hours, cool, cut into blocks, seal and store insulated, and obtain.

5. The preparation method according to claim 4, characterized in that: In the step c), the rotation speed of the low-speed stirring is 50 to 200 r / min.

6. The preparation method according to claim 4, characterized in that: In the steps c) and d), the high-speed shear rate is 1000-2000 rpm.

Citation Information

Patent Citations

  • Asphalt waterproof paint for building and preparation method thereof

    CN101921545A

  • Hot melt type modified asphalt waterproof paint and preparation method thereof

    CN102408829A

  • Functional hot melting modified asphalt waterproof roll material and preparation method thereof

    CN106758313A

  • Rubber asphalt-based material used for concrete structured expansion joints, and preparation method thereof

    CN106947273A

  • Room-temperature non-cured rubber modified asphalt waterproof coating and preparation method thereof

    CN107779098A