Glass composition having nickel to reduce energy consumption during its melting step

By adding nickel to the low-iron glass composition to reduce its thermal radiation conductivity, the problem of high energy consumption in the glass industry is solved, cost-effective energy reduction is achieved, and the mechanical and chemical properties of the glass are maintained.

CN115784606BActive Publication Date: 2024-11-26AGC GLASS EUROPE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211571810.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-02-28
Filing Date
2019-02-15
Publication Date
2024-11-26
Estimated Expiration
2039-02-15

AI Technical Summary

Technical Problem

The existing glass industry medium and low iron glass compositions are difficult to reduce energy consumption at high temperatures, and the modification components are costly, which affects industrial applications.

Method used

Adding 0.0001% to 0.0020% nickel to the low-iron glass composition reduces its thermal radiation conductivity, thereby reducing the energy consumption of the melting step and maintaining the mechanical and chemical properties of the glass.

Benefits of technology

By increasing the absorption coefficient of the glass and reducing the radiation conductivity, the energy consumption of the glass melting process is significantly reduced, and it is cost-effective and does not damage the characteristics of the glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115784606B_ABST
    Figure CN115784606B_ABST
Patent Text Reader

Abstract

The present invention relates to a glass composition having nickel to reduce the energy consumption during its melting step, a glass composition having low thermal radiation conductivity at high temperature. In particular, the present invention relates to a glass composition comprising the following components expressed in weight percentage relative to the total weight of the glass composition: SiO 2 50%‑85%; Al 2 O 3 0%‑30%, B 2 O 3 0%‑20%; Na 2 O 0%‑25%; CaO 0%‑25%; MgO 0%‑15%; K 2 O 0%‑20%; BaO 0%‑20%; total Fe 2 O 3 The present invention relates to a glass having a content of 0.002% to 0.1% and further comprises NiO at a level of 0.0001% to 0.0020% by weight of the total glass composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an invention patent application with an application date of February 15, 2019, an application number of 201980015939.6 and an invention name of “Glass composition having nickel to reduce energy consumption during its melting step”. Technical Field

[0002] The present invention relates to a glass composition comprising nickel to reduce energy consumption during its melting step. Background Art

[0003] Reducing the energy consumption in melting furnaces in the glass industry is a major issue both from an economic and an environmental point of view. Improvements in the industrial production process steps have been developed, such as further furnace insulation, optimization of combustion, ... However, further improvements in the process steps would require significantly more expensive investments. Another way to reduce the energy consumption is to process the glass composition itself by reducing its melting temperature. The melting temperature is defined as the temperature at which the glass viscosity is 10 PaS. Therefore, the melting temperature is reduced by reducing the viscosity of the glass composition at high temperatures. Thereby, the energy to be supplied to the furnace can be reduced.

[0004] Recently, "ultra-white" or "ultra-clear" glasses have tended to be preferred in the solar or architectural fields due to their high light transmittance and / or energy transmittance. These glasses contain low amounts of iron and are therefore often also referred to as "low-iron glasses". For industrial soda-lime glasses, low-iron glasses are characterized by a total iron content (expressed as total Fe2O3) of less than about 0.1 wt%, typically less than 600 ppm. However, these low-iron glass compositions are characterized by a high radiative thermal conductivity and are therefore difficult to heat by radiation of the wavelengths emitted inside a glass furnace. For these low-iron glass compositions, increasing the radiation absorption of the molten glass at high temperatures would be highly beneficial in terms of energy consumption.

[0005] Lowering the melting temperature of glass compositions has been considered in the art: US 5,071,796 discloses window glass compositions in which SiO2 has been partially replaced by Na2O and Al2O3, resulting in a reduction in high temperature viscosity. WO 2014 / 128714 proposes replacing about half of the silica content, and part or all of the calcium oxide content, with a boron component. However, it is difficult to maintain the glass properties of such highly modified compositions, such as the fining temperature, glass transition temperature, glass durability or optical properties. In addition, some alternative components may be quite expensive, and thus limit their industrial application.

[0006] Glass compositions containing nickel are known in the art. See, for example, US 2013 / 0316162, US 2014 / 0017500, US 3,881,905, which describe glass or tempered glass for display panels; and US 5,888,917, which discloses transparent non-fogging colored glass.

[0007] It is therefore an object of the present invention to provide a low iron glass composition having low radiative thermal conductivity at high temperatures in a cost-effective manner to reduce the energy consumption of the production process without compromising the properties of the glass composition. Summary of the invention

[0008] The present invention relates to a glass composition comprising the following components expressed in weight percentage relative to the total weight of the glass composition:

[0009]

[0010]

[0011] Wherein the glass composition further comprises nickel expressed as NiO at a level of 0.0001% to 0.0020% by weight.

[0012] The present invention further relates to a glass product made of the glass composition, in particular a glass product in the form of a glass sheet, a hollow glass product or a glass fiber.

[0013] The invention also relates to the use of nickel for reducing the energy consumption during the melting step of the glass composition according to the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 A shows the absorption coefficient (κ) of the glass composition of the prior art (XCL) and the composition of the invention (XCL-Ni) as a function of wavelength at room temperature. λ ). Figure 1 B shows the absorption coefficient (κ) of the same prior art glass composition (XCL) and the composition of the invention (XCL-Ni) at 1200°C as a function of wavelength. λ ). Figure 1 B further shows the emissivity gradient (dE) of the black body at 1200°C as a function of the same wavelength. λ / dT).

[0015] Figure 2 The addition of nickel to a low iron composition to reduce the relative radiant thermal conductivity (Rk) is graphically illustrated. r ). Used to normalize (Rk r=1) has a glass composition of 1000 ppm Fe2O3 (total iron content) and 0 ppm NiO.

[0016] Figure 3 The increase in specific energy consumption (in %) obtained with glass compositions enriched with iron or nickel, starting from a base glass with 670 ppm Fe2O3, is shown. The black dots are industry data, which record the increase in specific energy consumption with stepwise additions of Fe2O3, starting from 670 ppm Fe2O3. The dashed line above the black dots is the calculated specific energy increase for glasses containing a nickel component (NiO at levels of 5, 10 and 15 ppm), the calculated specific energy increase for glass compositions having a total iron content ranging between 670 and 870 ppm. DETAILED DESCRIPTION

[0017] The object of the present invention is to provide a low iron glass composition having low thermal radiative conductivity to reduce energy consumption during the production process. It has surprisingly been found that the addition of small amounts of nickel to a low iron glass composition in a cost-effective manner allows a significant reduction in thermal radiative conductivity while maintaining the mechanical properties, viscosity and chemical durability of the glass composition.

[0018] Throughout this document, when a range is indicated, the endpoints are included. In addition, all integers and sub-domain values ​​within the numerical range are expressly included as if explicitly written. Also throughout this document, the values ​​of the content are expressed as weight percentages, that is, relative to the total weight of the glass, unless otherwise explicitly specified (e.g., in ppm). Throughout this document, unless otherwise explicitly specified, the iron content is total and expressed as Fe2O3.

[0019] The glass compositions of the present invention comprise nickel, expressed as NiO, at a level of 0.0001% to 0.0020% by weight.

[0020] In a preferred embodiment, the glass composition of the present invention comprises nickel expressed as NiO at a level of ≤ 0.0018%, preferably ≤ 0.0015%, more preferably ≤ 0.0010%, ideally ≤ 0.0008% by weight.

[0021] In another preferred embodiment, the glass composition of the present invention comprises nickel expressed as NiO at a level of ≥ 0.0002%, more preferably ≥ 0.0003% or even > 0.0005% by weight.

[0022] The glass composition of the present invention comprises total iron (expressed as Fe2O3) at a level of 0.002% to 0.1% by weight. In a preferred embodiment, the glass composition comprises total iron (expressed as Fe2O3) at a level of 0.002% to 0.06%, preferably 0.002% to 0.04%, more preferably 0.002% to 0.02% by weight.

[0023] The present invention solves the following technical challenges: by reducing the radiative conductivity (k) of the glass composition in the wavelength corresponding to the energy radiated in the melting furnace at the temperature reached in the furnace. r ) and thus increase the absorption coefficient (κ λ ), formulating a glass composition with low radiative thermal conductivity at high temperatures. It has been surprisingly found that the addition of low amounts of nickel to a glass composition with a relatively low amount of total iron provides such low radiative thermal conductivity. Moreover, this technical solution (by which the composition is only slightly modified) allows the mechanical and chemical properties of the glass composition to be maintained.

[0024] The radiative transport in molten glass compositions can be estimated by the Rosseland approximation based on the following assumptions: Photon propagation can be modeled by the diffusion law, i.e., according to Eq. 1, the energy flux F is related to the thermal gradient is proportional to, where z is the glass height and the proportionality factor k r is the radiation heat transfer coefficient.

[0025]

[0026] Radiative heat transfer coefficient k r The emissivity gradient can be calculated at all wavelengths by following Equation II (the rate of change of emissivity with temperature) and the absorption coefficient κ λ For the purpose of this invention, the emissivity E emitted in the furnace is calculated by summing the reciprocals of λ Absorbed into black body.

[0027]

[0028] It has been found that to improve heat transfer from the low iron glass composition to the molten glass, the thermal gradient in Equation 1 is increased, This can be achieved by reducing the radiative thermal conductivity k of the glass composition. r and thus by increasing its absorption coefficient κ λ Furthermore, it has been found that the absorption curve of the glass composition must match as much as possible the emissivity gradient of the energy radiation emitted in the furnace in order to have a significant effect on the radiative thermal conductivity.

[0029] The absorption coefficients κ of the compositions of the prior art and the compositions of the invention (according to Table 1 below) were measured at room temperature and at elevated temperature. λ The high temperatures correspond to the temperatures typically achieved in glass furnaces.

[0030] Table 1 Compositions of the prior art Compositions of the present invention refer to XCL XCL-Ni <![CDATA[SiO2(wt%)]]> 73.0 73.0 <![CDATA[Al2O3(wt%)]]> 0.03 0.03 CaO (wt%) 8.25 8.25 MgO (wt%) 4.5 4.5 <![CDATA[Na2O(wt%)]]> 13.9 13.9 <![CDATA[K2O(wt%)]]> 0.01 0.01 <![CDATA[SO3(wt%)]]> 0.32 0.32 <![CDATA[Fe2O3 tot(wt%)]]> 0.0102 0.0102 Ni(ppm) 0 19

[0031] The absorption coefficient is measured in the laboratory according to the following method: a specific spectrometer is designed to measure the transmittance from 250 to 2800 nm at high temperature. A temperature of 1200°C is chosen as representative of the temperatures reached in the furnace. The radiation sources are xenon and halogen lamps (from 250 to 2000 nm) and ceramic elements (for wavelengths above 2000 nm). The radiation is modulated and divided into two beams entering the laboratory furnace. The optical path of one beam is dedicated to measuring the transmittance of the glass sample, the other beam does not pass through the sample and is used as a blank. The transmittance detector is a photomultiplier tube or a semiconductor. The glass sample holder is an alumina ring with two sapphire windows. Measurements are performed at two different thicknesses of 1 mm and 2 mm. Therefore, the absorption coefficient is calculated from the two recorded transmission spectra.

[0032] The absorption coefficients (κ) of the two low iron glass compositions, namely, XCL without nickel component (composition of the prior art) and XCL-Ni with low level of nickel (composition of the present invention) are shown in Table 1. λ ) is measured at wavelengths from 250nm to 2800nm. According to the above method, at room temperature ( Figure 1 A) and 1200℃( Figure 1 B), the absorption coefficient is measured as a function of wavelength. Figure 1 B further shows the emissivity gradient (dE) of a black body at the same temperature of 1200°C as a function of the same wavelength. λ / dT). For illustration purposes, only the shape of this latter curve is important, and Figure 1 The values ​​in B are normalized to the function dE λ / The maximum value of dT.

[0033] exist Figure 1 A (where the absorption coefficient of the glass composition is measured at room temperature at different wavelengths) shows that due to Fe 2+ , the prior art composition XCL exhibits a strong absorption band centered at 1000 nm. The XCL-Ni composition of the present invention exhibits several strong absorption bands in the visible range, and also exhibits several peaks centered at 1000 and 2000 nm in the infrared spectrum. These peaks explain the slightly higher IR absorption of the nickel-containing glass composition at room temperature compared to the prior art composition.

[0034] Figure 1B illustrates the surprising benefit of the composition of the invention. Compared to the reference (XCL, composition of the prior art), the absorption in the visible range of the composition of the invention (XCL-Ni) decreases at high temperatures, but increases strongly in the infrared (above 1700 nm), which is highly beneficial for improving the absorption of radiation emitted in the furnace.

[0035] As follows Figure 1 As described in A and 1B, it has surprisingly been found that the compositions of the present invention advantageously absorb the radiation emitted by the flame and the radiation re-emitted by the refractory materials in the furnace. In fact, the compositions of the present invention containing low amounts of nickel exhibit absorption bands in the infrared wavelengths at high temperatures that match the emissivity gradient of the energy furnace absorbed to a black body herein ( Figure 1 B).

[0036] Using Equation II and from Figure 1 The absorption coefficient κ obtained in B λ The radiative thermal conductivity k has been calculated for low iron glass compositions characterized by different levels of iron content and different levels of nickel content. r .

[0037] The relative radiative thermal conductivity Rk has been calculated using Equation II (above): r The absorption coefficients of iron and nickel are κ λ From to Figure 1 The optical model is calibrated based on the measured absorption curves at room temperature and 1200 °C in A and 1B. r The values ​​are normalized to glass containing 1000 ppm Fe2O3 and no nickel to obtain the relative radiative thermal conductivity Rk r .

[0038] Figure 2 The addition of nickel to low iron compositions is shown to reduce the relative radiative thermal conductivity (Rk r ) benefits. Figure 2 It is demonstrated that the effect of adding nickel to the glass composition on radiative conductivity is stronger for compositions with lower iron content. It is further demonstrated that the first few ppm of nickel are most effective in reducing the relative radiative thermal conductivity. Increasing the nickel level above 0.002% by weight of the total glass composition does not provide significant incremental benefit.

[0039] Computational fluid dynamics models of glass furnaces usually use the radiative thermal conductivity approximation calculated in this paper. Therefore, glass technicians can use the Figure 2 The data were used to estimate the energy increase as a function of the amount of nickel added to the melt for a given amount of iron. Figure 3 An alternative estimate based on industry data is shown, reporting the change in specific consumption (in percent) / amount of iron.

[0040] Industrial data have been collected on the energy gain of silicate based glass compositions at different levels of iron content: please refer to Figure 3 These industrial data report an initial content of 670 ppm Fe2O3 tot The composition starts with Fe2O3 tot The increase in the content of iron increases the specific energy consumption (i.e., energy reduction). From these industrial data obtained at different iron contents, the thermal conductivity k can be calculated. r , and thus obtain k r The function f that relates the decrease in specific consumption to the increase in specific consumption. In addition, based on Figure 2 The measurement of κ λ , the k of a glass composition containing both nickel and iron can be calculated r , and apply the same function f to the k values ​​of these glass compositions r Converted into an increase in specific energy consumption, such as Figure 3 In fact, Figure 3 The energy gain obtained using glass compositions containing various nickel additions (5, 10 and 15 ppm NiO) is shown, calculated for glass compositions having a total iron content ranging between 670 and 870 ppm. tot In a glass composition of 5 ppm NiO will reduce the specific energy consumption by about 1%, which is indeed significant in the current glass melting field. Adding 10 ppm to 15 ppm NiO to the same glass composition will provide an increase in specific energy consumption of 1.7% and 2.2%, respectively. For glass compositions with higher iron content, the increase per ppm NiO is lower, but still significant. In a glass composition containing 870 ppm Fe2O3 tot Adding 5 ppm to 15 ppm NiO to the glass composition will give an increase in specific energy consumption of 0.7% to 1.5%, respectively.

[0041] In a preferred embodiment, the glass composition of the present invention further comprises cobalt, expressed as CoO, at a level of preferably 0.00005% to 0.0020%, more preferably 0.00005% to 0.0015% by weight. In practice, it has been found that the addition of nickel, even at the low levels required by the present invention, may slightly affect the optical properties, such as the color of the final product. Depending on the target application / use, this may or may not be a problem. The yellow color imparted by nickel can be easily neutralized by cobalt additions, if desired.

[0042] In another embodiment, the glass composition of the present invention further comprises chromium expressed as Cr2O3 at a level of preferably 0.0001% to 0.0025%, more preferably 0.0001% to 0.002% by weight. In fact, it has been found that the addition of chromium to the glass composition of the present invention can provide similar benefits as the addition of nickel, in that it allows the radiant thermal conductivity of the corresponding glass composition to be reduced, but in a less effective manner compared to nickel.

[0043] In a preferred embodiment, the glass composition of the present invention is free of selenium. Free of selenium in this context means a glass composition having <3 ppm, preferably <2 ppm of selenium (expressed as Se). In a more preferred embodiment, the glass composition of the present invention does not contain a combination of selenium and cobalt.

[0044] The glass composition according to the invention is made of glass that can belong to various categories. The glass can be, for example, soda-lime-silica, aluminosilicate or borosilicate type glass, among others.

[0045] In addition to iron and nickel, the glass composition of the present invention comprises the following components expressed in weight percentage relative to the total weight of the glass composition:

[0046] <![CDATA[SiO2]]> 50%-85% <![CDATA[Al2O3]]> 0%-30% <![CDATA[B2O3]]> 0%-20% <![CDATA[Na2O]]> 0%-25% CaO 0%-25% MgO 0%-15% <![CDATA[K2O]]> 0%-20% BaO 0%-20%

[0047] In a preferred embodiment, the glass composition of the present invention comprises the following components expressed in weight percentage relative to the total weight of the glass composition:

[0048] More preferably <![CDATA[SiO2]]> 50%-78% 55%-78% <![CDATA[Al2O3]]> 0%-18% 0%-18% <![CDATA[B2O3]]> 0%-18% 0%-18% <![CDATA[Na2O]]> 0%-20% 5%-20% CaO 0%-25% 0%-15% MgO 0%-10% 0%-10% K2O 0%-10% 0%-10% BaO 0%-5% 0%-5%

[0049] The preferred composition of the invention, which can be used in particular for glass sheets and insulating glass products, is of the soda-lime-silica type. Advantageously, according to this preferred embodiment, the composition comprises the following components expressed in weight percentage relative to the total weight of the glass composition:

[0050] <![CDATA[SiO2]]> 60%-75% <![CDATA[Al2O3]]> 0%-6% <![CDATA[B2O3]]> 0%-4% <![CDATA[Na2O]]> 5%-20% CaO 0%-15% MgO 0%-10% <![CDATA[K2O]]> 0%-10% BaO 0%-5%

[0051] Other preferred glass compositions of the present invention, particularly useful for glass fiber applications, comprise the following components expressed in weight percentage relative to the total weight of the glass composition:

[0052] <![CDATA[SiO2]]> 50%-75% <![CDATA[Al2O3]]> 10%-30% <![CDATA[B2O3]]> 0%-20% <![CDATA[Na2O]]> 0%-5% CaO 0%-25% MgO 0%-15% <![CDATA[K2O]]> 0%-5% BaO 0%-5%

[0053] Descriptions of glass compositions according to the invention which are considered suitable for use in glass fibers are shown in the following table:

[0054] Description 1 Note 2 Note 3 <![CDATA[SiO2(%)]]> 59-61 52-56 64-66 <![CDATA[B2O3(%)]]> - 5-10 - <![CDATA[TiO2(%)]]> - 0-0.8 - <![CDATA[Fe2O3(%)]]> 0.05-0.1 0.05-0.1 0.002-0.1 <![CDATA[Al2O3(%)]]> 12.5-13.5 12-16 24-26 CaO(%) 21.5-22.5 16-25 0-0.3 MgO(%) 2.7-3.3 0-5 9-11 <![CDATA[Na2O(%)]]> 0.03-0.05 0-2 0-0.3 <![CDATA[K2O(%)]]> 0.25-0.60 <![CDATA[Including in Na2O]]> <![CDATA[Including in Na2O]]>

[0055] The glass composition of the present invention is particularly interesting when used to make glass products, especially hollow glass products, glass sheets and / or glass fibers. Hollow glass products can be glass bottles, glass flasks, glass jars, etc. Glass fibers are glass in the form of fibers used to make various products (such as glass wool for insulation), and are generally composed of matte fine glass fibers.

[0056] In a preferred embodiment, the present invention relates to a hollow glass product made from the composition of the present invention.

[0057] In an alternative preferred embodiment, the present invention is directed to a glass fiber made from the glass composition of the present invention.

[0058] Typically, the method for making glass comprises the following steps: (i) melting a starting material batch including a mixture of glass starting materials and / or cullets in a glass melting furnace / tank; and then forming the molten glass into a desired shape. The melting step comprises providing heat to the starting materials or cullets by radiation transfer to achieve melting / melting. Typically, the heat is generated by burning a burner using a fossil fuel (i.e., natural gas) together with preheated air.

[0059] For example, in order to form a fiber, the molten glass can be continuously drawn from a sleeve. In order to form a hollow glass like a bottle, the molten glass is placed in a mold, and then the glass is molded into a glass bottle body by a blow molding technique. The glass sheet can be obtained by a float process, a drawing process, a rolling process, or any other process known to manufacture a glass sheet starting from a molten glass composition. In an embodiment according to the present invention, the glass sheet is a float glass sheet. The term "float glass sheet" should be understood to mean a glass sheet formed by a float glass process, which consists in pouring molten glass on a bath of molten tin under reducing conditions.

[0060] The invention also relates to the use of nickel for reducing the energy consumption during the melting step of the glass composition according to the invention.

[0061] Embodiments of the present invention will now be further described by way of examples.The following examples are provided for illustrative purposes and are not intended to limit the scope of the present invention.

[0062] Examples

[0063] Preparation of glass compositions for the examples: According to each composition specified below, powder raw materials were mixed together and placed in a melting crucible. The raw material mixture was then heated in an electric furnace to a temperature that allowed the raw materials to completely melt.

[0064] According to the present invention, the following glass compositions are produced. These glass compositions are particularly suitable for use as glass sheets or insulating glass products.

[0065] 1 2 3 4 5 6 7 8 <![CDATA[SiO2(%)]]> 72.2 72.2 72.3 72.2 72.2 72.2 72.2 72.3 <![CDATA[Al2O3(%)]]> 0.62 0.63 0.61 0.62 0.62 0.61 0.62 0.61 <![CDATA[Fe2O3(%)]]> 0.075 0.077 0.074 0.074 0.074 0.074 0.074 0.073 CaO(%) 8.89 8.91 8.85 8.87 8.84 8.87 8.86 8.67 MgO(%) 4.28 4.26 4.29 4.30 4.30 4.29 4.30 4.21 <![CDATA[Na2O(%)]]> 13.50 13.53 13.46 13.48 13.50 13.50 13.52 13.44 <![CDATA[K2O(%)]]> 0.06 0.06 0.06 0.06 0.06 0.06 0.06 0.06 Ni(ppm) 4 5 9 13 3 6 6 8 Co(ppm) - - - - 0.75 1.5 2.5 3.5

Claims

1. A glass sheet comprising a glass composition, the glass composition comprising the following components expressed in weight percentage relative to the total weight of the glass composition: It is characterized in that The glass composition further comprises nickel expressed as NiO at a level of >0.0005% to 0.0018% by weight.

2. The glass sheet comprising the glass composition according to claim 1, characterized in that: The glass composition comprises total Fe2O3 at a level of 0.002% to 0.06%.

3. The glass sheet comprising the glass composition according to claim 1, characterized in that: The glass composition comprises total Fe2O3 at a level of 0.002% to 0.04%.

4. The glass sheet comprising the glass composition according to claim 1, characterized in that: The glass composition comprises total Fe2O3 at a level of 0.002% to 0.02%.

5. The glass sheet comprising the glass composition according to any one of claims 1 to 4, characterized in that The glass composition comprises the following components expressed in weight percentage relative to the total weight of the glass composition: 。 6. The glass sheet comprising the glass composition according to claim 5, characterized in that: The glass composition comprises the following components expressed in weight percentage relative to the total weight of the glass composition: 。 7. The glass sheet comprising the glass composition according to any one of claims 1 to 4, characterized in that The glass composition further comprises cobalt.

8. The glass sheet comprising the glass composition according to claim 7, characterized in that: The glass composition comprises cobalt, expressed as CoO, at a level of 0.00005% to 0.0020% by weight.

9. The glass sheet comprising the glass composition according to claim 7, characterized in that: The glass composition comprises cobalt, expressed as CoO, at a level of 0.00005% to 0.0015% by weight.

10. The glass sheet comprising the glass composition according to any one of claims 1 to 4, characterized in that The glass composition further comprises chromium.

11. The glass sheet comprising the glass composition according to claim 10, characterized in that: The glass composition comprises chromium, expressed as Cr2O3, at a level of 0.0001% to 0.0025% by weight.

12. The glass sheet comprising the glass composition according to claim 10, characterized in that: The glass composition comprises chromium, expressed as Cr2O3, at a level of 0.0001% to 0.002% by weight.

13. Use of nickel expressed as NiO at a level of 0.0001% to 0.0020% by weight for reducing energy consumption during the melting process of a glass composition comprising, in weight percentage, the following components: