Oil storage cotton and preparation method thereof and atomizer for electronic cigarette
By attaching cellulose fibers containing hydroxyl groups to the oil storage cotton and using pressure reduction filtration technology, the oil storage capacity and oil locking ability of the oil storage cotton are improved, solving the problem of insufficient oil storage capacity of the existing oil storage cotton, and realizing Higher oil storage capacity and longer service life.
Patent Information
- Application Number
- CN202211336626.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-28
AI Technical Summary
The existing oil storage cotton has not yet been able to meet the needs of electronic cigarettes for miniaturization design and service life in terms of oil storage capacity and oil locking capacity. In particular, the oil storage capacity of PA+PET material is only 15g/g, which cannot meet the needs of e-cigarettes. Required standards.
Cellulose fibers containing hydroxyl groups are attached to the fiber cotton, and the cellulose fiber solution is passed through the fiber cotton through reduced pressure filtration technology, so that the cellulose fibers are intercepted and attached to the fiber cotton, thereby increasing the polar group content of the surface layer of the fiber cotton. Thereby improving the oil storage capacity and oil locking ability.
The oil storage capacity of the oil storage cotton prepared by this method is significantly increased, reaching about 26g/g, which meets the oil storage needs of electronic cigarettes and extends the service life of the oil storage cotton.
Smart Images

Figure CN115787296B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic cigarettes, and in particular to an oil storage cotton and a preparation method thereof, and an atomizer for electronic cigarettes. Background Art
[0002] Electronic cigarettes, also known as virtual cigarettes, steam cigarettes, aerosol generating devices, etc., are mainly used to simulate the feeling of smoking without affecting health, for the purpose of quitting smoking or replacing cigarettes.
[0003] The electronic cigarette atomizer is the core component of the electronic cigarette, and the oil storage cotton is one of the important components of the electronic cigarette atomizer. The main function of the oil storage cotton is to store the smoke oil. The oil storage capacity and oil locking capacity of the oil storage cotton are closely related to the service life of the oil storage cotton and the taste of the electronic cigarette. The stronger the oil storage capacity and oil locking capacity of the oil storage cotton, the longer the service life of the oil storage cotton (no need to frequently replace the oil storage cotton or frequently refill the smoke oil), the larger the amount of smoke of the electronic cigarette, and the better the taste of smoking. At the same time, it is also conducive to the miniaturization design of the electronic cigarette (for the same amount of smoke oil storage, the stronger the oil storage capacity of the oil storage cotton, the smaller the volume required for the oil storage cotton).
[0004] Existing oil storage cotton mainly adopts PP+PE material, or PET material, or PA+PET material. In terms of oil storage capacity and oil locking capacity, since PA is added to PA+PET material, PA contains amide bonds, and the amide bonds match the smoke oil in polarity, it can have a strong adsorption effect with the smoke oil, thereby improving the oil storage capacity and oil locking capacity of the oil storage cotton. According to tests, the oil storage capacity of the oil storage cotton using PA+PET material is about 15g / g (that is, each gram of oil storage cotton stores 15 grams of smoke oil), but this oil storage capacity has not yet been able to meet the existing demand. In order to meet the needs of miniaturized design of electronic cigarettes and the service life of oil storage cotton, it is urgent to improve the oil storage capacity and oil locking capacity of oil storage cotton. Summary of the invention
[0005] The object of the present invention is to provide an oil storage cotton and a preparation method thereof and an atomizer for an electronic cigarette, wherein the oil storage cotton has good oil storage capacity and oil locking capacity.
[0006] The invention provides an oil storage cotton, comprising fiber cotton, on which cellulose fibers containing hydroxyl groups are attached.
[0007] In one achievable manner, the cellulose fiber is at least one of natural cotton fiber, wood fiber, bamboo fiber, jute fiber, ramie fiber, flax fiber, hemp fiber, sisal fiber and mulberry silk fiber.
[0008] In a feasible manner, the width of the cellulose fiber is 5-20 μm, and the length of the cellulose fiber is 0.2-5 mm.
[0009] In an achievable manner, the density of the fiber cotton is 0.03-0.1 g / cm 3 .
[0010] The present invention also provides a method for preparing oil storage cotton, which is used to prepare the above-mentioned oil storage cotton. The method for preparing the oil storage cotton comprises the following steps:
[0011] S10: Provide fiber cotton;
[0012] S20: adding cellulose fibers containing hydroxyl groups into the dispersion to prepare a cellulose fiber solution;
[0013] S30: allowing the cellulose fiber solution to pass through the fiber cotton, so that the cellulose fibers in the cellulose fiber solution are retained and attached to the fiber cotton;
[0014] S40: Drying the fiber cotton to obtain oil storage cotton.
[0015] In one achievable manner, the step S20 specifically includes:
[0016] The fiber cotton is placed in a vacuum filtration device, and the cellulose fiber solution is passed through the fiber cotton using a vacuum filtration method, so that the cellulose fibers in the cellulose fiber solution are retained and attached to the fiber cotton.
[0017] In one achievable manner, when performing reduced pressure filtration, the pressure set by the reduced pressure filtration device is -60 kPa to -20 kPa.
[0018] In one achievable manner, the cellulose fibers are insoluble in the dispersion.
[0019] In one achievable manner, the dispersion liquid is an ethanol solution.
[0020] In one achievable manner, the cellulose fiber is at least one of natural cotton fiber, wood fiber, bamboo fiber, jute fiber, ramie fiber, flax fiber, hemp fiber, sisal fiber and mulberry silk fiber.
[0021] In one achievable manner, the content of cellulose fibers in the cellulose fiber solution is 50-500 g / L.
[0022] In a feasible manner, the width of the cellulose fiber is 5-20 μm, and the length of the cellulose fiber is 0.2-5 mm.
[0023] In an achievable manner, the density of the fiber cotton is 0.03-0.1 g / cm 3 .
[0024] The present invention also provides an atomizer for electronic cigarettes, comprising the oil storage cotton described above.
[0025] The oil storage cotton provided by the present invention contains abundant hydroxyl groups in the molecular structure of cellulose fiber, and attaching cellulose fiber to fiber cotton can increase the content of polar groups on the surface of fiber cotton, thereby achieving the purpose of improving the oil storage capacity and oil locking capacity of fiber cotton. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the production process of oil storage cotton in an embodiment of the present invention.
[0027] Figure 2 Schematic diagram of the structure of the pressure reducing filtration device in an embodiment of the present invention. DETAILED DESCRIPTION
[0028] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0029] The terms "first", "second", "third", "fourth" and the like (if any) in the description and claims of the present invention are used to distinguish similar objects and are not necessarily used to describe a particular sequence or order.
[0030] The directional words such as up, down, left, right, front, back, top, bottom, etc. (if any) involved in the specification and claims of the present invention are defined by the positions of the structures in the drawings and the positions of the structures relative to each other, and are only for the clarity and convenience of expressing the technical solution. It should be understood that the use of directional words should not limit the scope of protection claimed in the present invention.
[0031] The embodiment of the present invention provides an oil storage cotton, including fiber cotton, on which cellulose fibers containing hydroxyl groups are attached. Since the molecular structure of cellulose fibers contains abundant hydroxyl groups, attaching cellulose fibers to the fiber cotton can increase the content of polar groups on the surface of the fiber cotton, thereby achieving the purpose of improving the oil storage capacity and oil locking capacity of the fiber cotton.
[0032] As an embodiment, the cellulose fiber is at least one of natural cotton fiber, wood fiber, bamboo fiber, jute fiber, ramie fiber, flax fiber, hemp fiber, sisal fiber and mulberry silk fiber.
[0033] As an embodiment, the width of the cellulose fiber is 5-20 micrometers, and the length of the cellulose fiber is 0.2-5 millimeters.
[0034] As an embodiment, the density of the fiber cotton is 0.03-0.1 g / cm 3 .
[0035] As an implementation method, the material of the fiber cotton can be a skin-core structure material such as PE (polyethylene) + PP (polypropylene), PET (polyethylene terephthalate) or PA (polyamide) + PET. When the fiber cotton is a skin-core structure material of PE + PP, PE is used as the skin layer and PP is used as the core layer; when the fiber cotton is a skin-core structure material of PET, PET with a low melting point is used as the skin layer and PET with a high melting point is used as the core layer (that is, the PET skin-core structure is composed of two PET materials with different melting points); when the fiber cotton is a skin-core structure material of PA + PET, PA is used as the skin layer and PET is used as the core layer. Preferably, the fiber cotton adopts the skin-core structure material of PA + PET. Since PA contains amide bonds, the amide bonds match the smoke oil in polarity, so it can have a strong adsorption effect with the smoke oil, thereby improving the oil storage capacity and oil locking capacity of the oil storage cotton.
[0036] Figure 1 Schematic diagram of the production process of oil storage cotton in an embodiment of the present invention. Figure 1 As shown, an embodiment of the present invention further provides a method for preparing oil storage cotton, which is used to prepare the above-mentioned oil storage cotton. The method for preparing the oil storage cotton comprises the following steps:
[0037] S10: Provide fiber cotton, which can be made of commonly used oil storage cotton;
[0038] S20: adding cellulose fibers containing hydroxyl groups into the dispersion and stirring evenly, so that the cellulose fibers are evenly dispersed in the dispersion and the cellulose fibers are at least partially insoluble in the dispersion, to prepare a cellulose fiber solution;
[0039] S30: passing the cellulose fiber solution through the fiber cotton, so that the cellulose fibers in the cellulose fiber solution are retained and attached to the fiber cotton;
[0040] S40: Drying the fiber cotton (for example, drying it at 60° C.) to obtain oil storage cotton.
[0041] Specifically, the preparation method of the oil storage cotton provided in this embodiment allows the cellulose fiber solution to pass through the fiber cotton, so that the cellulose fibers in the cellulose fiber solution are intercepted and attached to the fiber cotton. Since the molecular structure of the cellulose fiber contains abundant hydroxyl groups, the cellulose fibers attached to the fiber cotton can increase the content of polar groups on the surface of the fiber cotton, thereby achieving the purpose of improving the oil storage capacity and oil locking capacity of the fiber cotton. The preparation method is not only simple in process, but also enables the cellulose fibers to be evenly attached to the fiber cotton. The oil storage cotton prepared by the preparation method has good oil storage capacity and oil locking capacity.
[0042] like Figure 1 As shown, as an implementation manner, the above step S20 specifically includes:
[0043] The fiber cotton is placed in a vacuum filtration device, and the cellulose fiber solution is passed through the fiber cotton by vacuum filtration (suction filtration) to intercept and attach the cellulose fibers in the cellulose fiber solution to the fiber cotton. Preferably, when performing vacuum filtration, the pressure set in the vacuum filtration device is -60kPa to -20kPa. At the same time, the cellulose fiber solution can also be subjected to multiple vacuum filtrations to increase the number of cellulose fibers attached to the fiber cotton.
[0044] Specifically, the reduced pressure filtration method can not only increase the rate at which the cellulose fibers in the cellulose fiber solution adhere to the fiber cotton, but also make the cellulose fibers adhere to the fiber cotton more evenly. Figure 2 As shown, in this embodiment, the vacuum filtration device 1 can be a commonly used suction filtration device, which includes a funnel 11 (Buchner funnel), a suction filter bottle 12 and an exhaust device 13. The liquid outlet end of the funnel 11 is plugged into the suction filter bottle 12, and the exhaust device 13 is connected to the suction filter bottle 12. The fiber cotton 2 and the cellulose fiber solution 3 are both placed in the funnel 11 (the cellulose fiber solution 3 is located on the upper layer of the fiber cotton 2); during suction filtration, the exhaust device 13 is turned on, and the air in the suction filter bottle 12 is sucked by the exhaust device 13 to form a negative pressure of -60kPa to -20kPa in the suction filter bottle 12. Under the action of the negative pressure in the suction filter bottle 12, the cellulose fiber solution 3 in the funnel 11 passes through the fiber cotton 2, the cellulose fibers in the cellulose fiber solution 3 are retained and attached to the fiber cotton 2, and the solvent in the cellulose fiber solution 3 passes through the fiber cotton 2 and flows into the suction filter bottle 12.
[0045] Preferably, the dispersion liquid is an ethanol solution (of course, the dispersion liquid may also be other dispersion liquids such as water), and the cellulose fibers are insoluble in the dispersion liquid. Of course, in other embodiments, the cellulose fibers may also be slightly soluble in the dispersion liquid (in fact, the smaller the solubility of the cellulose fibers in the dispersion liquid, the better, so that the amount of cellulose fibers attached to the fiber cotton can be increased without destroying the original structure and morphology of the cellulose fibers).
[0046] As an embodiment, the cellulose fiber is at least one of natural cotton fiber, wood fiber, bamboo fiber, jute fiber, ramie fiber, flax fiber, hemp fiber, sisal fiber and mulberry silk fiber.
[0047] As an embodiment, the width of the cellulose fiber is 5-20 microns, preferably 8-15 microns. The length of the cellulose fiber is 0.2-5 mm, preferably 0.5-2 mm. Specifically, if the length of the cellulose fiber is too long, it is easy to block the capillary pores of the fiber cotton; if the length of the cellulose fiber is too short, it is not easy to be adsorbed and trapped on the fiber cotton when passing through the fiber cotton.
[0048] As an embodiment, the content of cellulose fiber in the cellulose fiber solution is 50-500 g / L, preferably 100-300 g / L. Specifically, if the content of cellulose fiber in the cellulose fiber solution is too high, it is easy to block the capillary channels of the fiber cotton; if the content of cellulose fiber in the cellulose fiber solution is too low, it is not easy to be adsorbed and trapped on the fiber cotton.
[0049] As an embodiment, the density of the fiber cotton is 0.03-0.1 g / cm 3 Preferably, the density of the fiber cotton is 0.03-0.07 g / cm 3 .
[0050] An embodiment of the present invention further provides an atomizer for an electronic cigarette, comprising the oil storage cotton described above.
[0051] The method for preparing the oil storage cotton provided in the embodiment of the present invention uses a vacuum filtration method to make a cellulose fiber solution pass through the fiber cotton, so that the cellulose fibers in the cellulose fiber solution are intercepted and attached to the fiber cotton. Since the molecular structure of the cellulose fibers contains abundant hydroxyl groups, the cellulose fibers attached to the fiber cotton can increase the content of polar groups on the surface of the fiber cotton, thereby achieving the purpose of improving the oil storage capacity and oil locking capacity of the fiber cotton. The preparation method is not only simple in process, but also can make the cellulose fibers evenly attached to the fiber cotton. The oil storage cotton prepared by the preparation method has good oil storage capacity and oil locking capacity.
[0052] First embodiment
[0053] The preparation method of the oil storage cotton provided in this embodiment comprises the following steps:
[0054] Control the humidity of the production environment to 30%-50%;
[0055] Select cellulose fibers, the width of the cellulose fibers is 10 microns and the length is 1 millimeter;
[0056] Adding cellulose fibers into an ethanol solution to prepare a cellulose fiber solution with a concentration of 200 g / L;
[0057] Perform vacuum filtration under a negative pressure of -40 kPa to allow the cellulose fiber solution to pass through the fiber cotton;
[0058] The fiber cotton is dried to obtain the oil storage cotton.
[0059] The oil storage cotton prepared as above was subjected to an oil absorption test, and it was measured that the oil storage capacity of the oil storage cotton reached 26g / g (that is, each gram of oil storage cotton stored 26g of e-liquid), and the oil storage capacity of the oil storage cotton was significantly improved.
[0060] Second embodiment
[0061] The preparation method of the oil storage cotton provided in this embodiment comprises the following steps:
[0062] Control the humidity of the production environment to 30%-50%;
[0063] Select cellulose fibers, the width of the cellulose fibers is 8 microns and the length is 1.5 millimeters;
[0064] Adding cellulose fibers into an ethanol solution to prepare a cellulose fiber solution with a concentration of 150 g / L;
[0065] Perform vacuum filtration under negative pressure of -50 kPa to allow the cellulose fiber solution to pass through the fiber cotton;
[0066] The fiber cotton is dried to obtain the oil storage cotton.
[0067] The oil absorption test was carried out on the oil storage cotton prepared as above, and it was measured that the oil storage capacity of the oil storage cotton reached 22g / g, and the oil storage capacity of the oil storage cotton was significantly improved.
[0068] Third embodiment
[0069] The preparation method of the oil storage cotton provided in this embodiment comprises the following steps:
[0070] Control the humidity of the production environment to 30%-50%;
[0071] Select cellulose fibers, the width of the cellulose fibers is 12 microns and the length is 2 millimeters;
[0072] Adding cellulose fibers into an ethanol solution to prepare a cellulose fiber solution with a concentration of 100 g / L;
[0073] Perform vacuum filtration under negative pressure of -30 kPa to allow the cellulose fiber solution to pass through the fiber cotton;
[0074] The fiber cotton is dried to obtain the oil storage cotton.
[0075] The oil absorption test was carried out on the oil storage cotton prepared as above, and it was measured that the oil storage capacity of the oil storage cotton reached 25g / g, and the oil storage capacity of the oil storage cotton was significantly improved.
[0076] Comparative Example 1
[0077] The preparation method of the oil storage cotton provided in this comparative example comprises the following steps:
[0078] Control the humidity of the production environment to 30%-50%;
[0079] Select cellulose fibers, the width of the cellulose fibers is 22 microns and the length is 3 millimeters;
[0080] Adding cellulose fibers into an ethanol solution to prepare a cellulose fiber solution with a concentration of 50 g / L;
[0081] Perform vacuum filtration under a negative pressure of -10 kPa to allow the cellulose fiber solution to pass through the fiber cotton;
[0082] The fiber cotton is dried to obtain the oil storage cotton.
[0083] The oil storage cotton prepared as above was subjected to an oil absorption test, and the oil storage capacity of the oil storage cotton was measured to be 17 g / g.
[0084] Comparative Example 2
[0085] The preparation method of the oil storage cotton provided in this comparative example comprises the following steps:
[0086] Control the humidity of the production environment to 30%-50%;
[0087] Select cellulose fibers, the width of the cellulose fibers is 3 microns and the length is 0.3 millimeters;
[0088] Adding cellulose fibers into an ethanol solution to prepare a cellulose fiber solution with a concentration of 500 g / L;
[0089] Perform vacuum filtration under a negative pressure of -70 kPa to allow the cellulose fiber solution to pass through the fiber cotton;
[0090] The fiber cotton is dried to obtain the oil storage cotton.
[0091] The oil storage cotton prepared as above was subjected to an oil absorption test, and the oil storage capacity of the oil storage cotton was measured to be 15 g / g.
[0092] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. An oil storage cotton, comprising fiber cotton, characterized in that: The fiber cotton is attached with cellulose fibers containing hydroxyl groups, and the cellulose fibers are retained and attached to the fiber cotton after a cellulose fiber solution passes through the fiber cotton; the width of the cellulose fibers is 5-20 microns, and the length of the cellulose fibers is 0.2-5 millimeters.
2. The oil storage cotton according to claim 1, characterized in that: The cellulose fiber is at least one of natural cotton fiber, wood fiber, bamboo fiber, jute fiber, ramie fiber, flax fiber, hemp fiber and sisal fiber.
3. The oil storage cotton according to claim 1, characterized in that: The density of the fiber cotton is 0.03-0.1g / cm 3 .
4. A method for preparing oil storage cotton, characterized in that: Used to prepare the oil storage cotton according to any one of claims 1 to 3, the preparation method of the oil storage cotton comprises the following steps: S10: Provide fiber cotton; S20: adding cellulose fibers containing hydroxyl groups to the dispersion to prepare a cellulose fiber solution; the width of the cellulose fibers is 5-20 μm, and the length of the cellulose fibers is 0.2-5 mm; S30: allowing the cellulose fiber solution to pass through the fiber cotton, so that the cellulose fibers in the cellulose fiber solution are retained and attached to the fiber cotton; S40: Drying the fiber cotton to obtain oil storage cotton.
5. The method for preparing the oil storage cotton according to claim 4, characterized in that: The step S20 specifically includes: The fiber cotton is placed in a vacuum filtration device, and the cellulose fiber solution is passed through the fiber cotton using a vacuum filtration method, so that the cellulose fibers in the cellulose fiber solution are retained and attached to the fiber cotton.
6. The method for preparing the oil storage cotton according to claim 5, characterized in that: When performing reduced pressure filtration, the pressure set in the reduced pressure filtration device is -60 kPa to -20 kPa.
7. The method for preparing the oil storage cotton according to claim 4, characterized in that: The cellulose fibers are insoluble in the dispersion.
8. The method for preparing the oil storage cotton according to claim 4, characterized in that: The dispersion liquid is an ethanol solution.
9. The method for preparing the oil storage cotton according to claim 4, characterized in that: The content of cellulose fibers in the cellulose fiber solution is 50-500 g / L.
10. An atomizer for electronic cigarette, characterized in that: It comprises the oil storage cotton as described in any one of claims 1-3.