A polyimide nanofiber / carbon nanotube composite conductive aerogel and preparation method thereof
The conditions of traditional conductive aerogels during preparation are solved by blending carbon nanotubes in polyamic acid solution and preparing polyimide nanofiber/carbon nanotube composite conductive aerogels using electrospinning and freeze-drying techniques. The problems of harshness and performance degradation have achieved high conductivity and flexibility aerogels, suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202211511511.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-11-29
AI Technical Summary
The existing conductive aerogels are harsh in the preparation process and cannot be mass-produced. Their performance after high-temperature carbonization is also degraded, which cannot meet the application requirements of piezoresistive sensors with high sensitivity, fast response and long cycle cycles.
Polyimide nanofiber/carbon nanotube composite conductive aerogel was prepared by synthesizing and mixing carbon nanotubes with electrospinning and freeze-drying. This method provides gentle process conditions, is easy to replicate at scale, and improves the conductivity and flexibility of the aerogel through winding of carbon nanotubes and cross-linking of PI nanofibers.
It realizes the high conductivity, good flexibility and compression elasticity of aerogel. It is suitable for flexible wearable devices and piezoresistive sensors in high temperature environments, and has a wide range of application prospects.
Smart Images

Figure CN115819969B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer nanomaterials and strain sensing, and in particular relates to a method for preparing a polyimide nanofiber / carbon nanotube composite conductive aerogel with flexible resilience. Background Art
[0002] Aerogel is an excellent solid material with a nano three-dimensional porous network structure. It has the characteristics of low density, high porosity, large specific surface area and low thermal conductivity. It has broad application prospects in flame retardant insulation, filtration adsorption, energy storage devices, and military and civilian fields such as aerospace. Conductive aerogel not only has the characteristics of the above-mentioned aerogel, but also has excellent conductive properties, making it have broad application prospects in flexible wearables, battery negative electrodes, supercapacitors, sensors and other fields. At present, the traditional preparation method of conductive aerogel is to obtain carbon-based aerogel by high-temperature carbonization of organic aerogel. Although it has excellent conductive properties, the conditions in the preparation process are harsh (high temperature, high pressure, oxygen-free, etc.), and it cannot be mass-produced. In addition, the performance of traditional carbon-based aerogels is reduced after high-temperature carbonization treatment (lower mechanics, lower compression rebound and brittleness), so traditional aerogels cannot meet the application requirements of high-sensitivity, fast response and long cycle piezoresistive sensors. Therefore, designing a new conductive aerogel with excellent mechanical properties, good thermal stability, flexibility and resilience is still a challenging problem in this field.
[0003] Polyimide (PI) is a type of polymer containing an imide ring on the main chain. Since the imide ring has a rigid aromatic ring stable structure, and the conjugation effect of its aromatic heterocyclic structure enhances the main chain bond energy and intermolecular forces, PI has good mechanical properties and thermal stability, and has been widely used in military applications and space flight. Since the first linear PI aerogel was produced by Aspen Aerogels in the United States in 2006, this material has attracted many domestic and foreign researchers to engage in related work. PI aerogel overcomes the brittleness of traditional inorganic oxide aerogels and the poor temperature resistance of organic aerogels, but there are still deficiencies in the field of conductivity, so it is necessary to improve the conductivity of PI aerogel in order to obtain better performance and wider applications. Patent CN 111218112 (application number 202010164170.9) proposes a method of preparing conductive PI aerogel by introducing graphene oxide into a polyamic acid aqueous solution and vacuum freeze drying. The aerogel prepared by this method has a large hardness and poor flexibility, which is insufficient to meet the needs of most conductive fields. Therefore, establishing a way to effectively improve the conductive properties of organic aerogels is a very valuable and challenging issue in this field.
[0004] The present invention prepares a PI nanofiber / carbon nanotube composite conductive aerogel by synthesizing a polyamic acid (PAA) solution, blending carbon nanotubes, combining electrostatic spinning, and freeze drying. The skeleton material is PI nanofibers, and carbon nanotubes are wound around the PI nanofibers to provide sufficient conductive paths for the aerogel, which can greatly improve the conductive properties of the aerogel; compared with traditional inorganic carbon-based aerogels, the aerogel prepared above improves the general brittleness of inorganic carbon-based aerogels. At the same time, the PI nanofibers in the present invention include a PI system that can be heat-melted under high-temperature thermal imidization treatment, and the water-soluble PAA tightly coats the PI nanofibers, so that cross-linking occurs between the PI nanofibers after imidization, thereby ensuring the good flexibility and resilience of the PI composite aerogel of the present invention, which can have a wide range of application prospects in the fields of flexible wearable devices and the like. Summary of the invention
[0005] The purpose of the present invention is to solve the deficiencies of the prior art and provide a polyimide nanofiber / carbon nanotube composite conductive aerogel and a preparation method thereof. The composite conductive aerogel provided by the present invention has good flexibility, can be repeatedly compressed and bent, has good conductivity, has low thermal conductivity, and the use density of the aerogel can be controlled. At the same time, the preparation method of the composite conductive aerogel provided by the present invention requires mild process conditions, is easy to replicate on a large scale, and has good application prospects.
[0006] Specifically include:
[0007] 1. A polyimide nanofiber / carbon nanotube composite conductive aerogel, comprising a skeleton material, a conductive filler and a bonding component; the skeleton material comprises at least one polyimide nanofiber, the conductive filler comprises carbon nanotubes, and the bonding component comprises at least one polyimide; in parts by weight, the skeleton material is 50 to 100 parts by weight, the conductive filler is 1 to 50 parts by weight, and the bonding component is 1 to 40 parts by weight.
[0008] Furthermore, the apparent density of the polyimide nanofiber / carbon nanotube composite conductive aerogel is 5 to 50 mg / cm 3 , preferably 6 to 45 mg / cm 3 , particularly preferably 7 to 40 mg / cm 3 .
[0009] Furthermore, the diameter of the polyimide nanofiber is 20 to 1000 nm, preferably 50 to 800 nm, and more preferably 100 to 600 nm.
[0010] 2. A method for preparing a polyimide nanofiber / carbon nanotube composite conductive aerogel, comprising the following steps:
[0011] A: using dibasic acid anhydride and diamine to condense into a polyamic acid solution, preparing the obtained polyamic acid solution into polyamic acid nanofibers, and then subjecting the obtained polyamic acid nanofibers to thermal imidization treatment to obtain polyimide nanofibers;
[0012] B: using dibasic acid anhydride and diamine to condense into a thermosetting polyamic acid solution, pouring the solution into a coagulation liquid, filtering, and drying to obtain an anhydrous polyamic acid solid;
[0013] C: dissolving anhydrous polyamic acid solid in an aqueous mixed solvent to obtain a water-soluble polyamic acid solution, and then dispersing carbon nanotubes in the water-soluble polyamic acid solution to obtain a carbon nanotube dispersion;
[0014] D: crushing one or more polyimide nanofibers and dispersing them in the above carbon nanotube dispersion to obtain a polyimide nanofiber / carbon nanotube composite dispersion; wherein at least one polyimide nanofiber is a hot-melt polyimide nanofiber; when multiple composite nanofibers are selected, the remaining nanofibers are thermosetting polyimide nanofibers;
[0015] E: The polyimide nanofiber / carbon nanotube composite dispersion in step D is rapidly frozen to prepare a crystalline phase of the composite dispersion; freeze-dried and then thermally imidized to obtain a polyimide nanofiber / carbon nanotube composite conductive aerogel.
[0016] 3. Furthermore, the solid content of the polyamic acid solution in step A is 5-30wt%, preferably 6-25wt%; the method for preparing polyamic acid nanofibers is one or more of electrospinning, air blowing spinning, and air blowing assisted electrospinning; the thermal imidization temperature is 250-400°C, preferably 280-350°C.
[0017] 4. Furthermore, the coagulation liquid described in step B is one or more of deionized water, ethanol, acetone, ethyl acetate, and hydrocarbons, preferably deionized water.
[0018] 5. Furthermore, the aqueous mixed solvent in step C is a mixed solution of an organic amine, deionized water and a low-carbon alcohol, wherein the organic amine is a fatty amine, including at least one of ethylenediamine, triethylamine and isopropylamine, preferably triethylamine; the alcohol is a low-carbon alcohol, including at least one of ethanol, methanol, tert-butanol and propanol, preferably tert-butanol; the mass ratio of the anhydrous polyamic acid solid to the organic amine is 1:1 to 1:6, preferably 1:2 to 1:4, the mass ratio of the deionized water to the low-carbon alcohol is 10:0.1 to 5:5, preferably 9:1 to 8:2, and the mass ratio of the anhydrous polyamic acid solid to the deionized water is 0.01 to 0.5%, preferably 0.05 to 0.2%.
[0019] 6. Furthermore, the hot-melt polyimide nanofibers in step D are selected from one or more of the polyimide nanofibers of hexafluorodianhydride / 4,4'-diaminodiphenyl ether system, the polyimide nanofibers of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride / 4,4'-diaminodiphenyl ether system, the polyimide nanofibers of bisphenol A dianhydride / 4,4'-diaminodiphenyl ether system, the polyimide nanofibers containing 4,4'-diaminodiphenylmethane system in the structure, P84 type polyimide nanofibers, and polyetherimide nanofibers.
[0020] 7. Furthermore, the dibasic acid anhydride used in the precursor polyamic acid fiber of the thermosetting polyimide nanofiber in step D is one or a mixture of two or more of biphenyltetracarboxylic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic anhydride, and 3,4,9,10-tetracarboxylic anhydride, and the diamine is one or a mixture of two or more of diaminodiphenyl ether, p-phenylenediamine, 4,4'-diaminodiphenyl sulfone, 9,9-bis(4-aminophenyl)fluorene, and 2,2'-bis(trifluoromethyl)diaminobiphenyl.
[0021] 8. Furthermore, in step D, the mass ratio of polyimide nanofibers to carbon nanotubes is (90-50):(10-50), preferably (80-60):(20-40); the mass concentration of the polyimide nanofiber / carbon nanotube composite dispersion is 0.5-5wt%, preferably 1-3wt%.
[0022] 9. Furthermore, the thermal imidization treatment in step E is performed by heating the temperature from room temperature to 250-400°C and keeping the temperature for 1-60 min, with a heating rate of 1-20°C / min, preferably 2-5°C / min.
[0023] 10. A polyimide nanofiber / carbon nanotube composite conductive aerogel and its products containing any one of the above.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] (1) The process conditions required for the preparation method of the composite conductive aerogel provided by the present invention are mild, easy to operate, convenient for large-scale replication, and have better prospects for mass production and promotion;
[0026] (2) The composite conductive aerogel prepared by the present invention can effectively solve the defects of the current PI aerogel that is insufficient in conductivity and cannot be applied in the fields of piezoresistive sensing, and has good application prospects in the fields of flexible wearables and supercapacitors.
[0027] (3) The hot-melt polyimide nanofibers used in the present invention have the property of self-crosslinking when heated. Under high temperature treatment, a dense cross-linked network structure will be formed inside the aerogel, which strengthens the skeleton structure of the aerogel and adds elastic support points to the aerogel, thereby making the aerogel have excellent compression rebound properties;
[0028] (4) The water-soluble PAA solution used in the present invention can be used as a dispersant for carbon nanotubes, solving the problem of poor dispersion of carbon nanotubes due to agglomeration, and can also act as an adhesive between carbon nanotubes and PI nanofibers, playing a role of secondary synergistic cross-linking, giving the composite conductive aerogel better compression resilience, ensuring that the composite aerogel can quickly feedback changes in electrical signals under external pressure, thereby making the PI nanofiber / carbon nanotube composite aerogel have a relatively high sensitivity.
[0029] (5) The PI nanofiber / carbon nanotube composite conductive aerogel provided by the present invention has a skeleton material of PI nanofibers and a conductive filler of carbon nanotubes, both of which have excellent high temperature resistance, giving the composite aerogel excellent temperature resistance, and can be used in piezoresistive sensors in high temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a morphological picture of the polyimide nanofiber / carbon nanotube composite aerogel floating on a flower in Example 2;
[0031] Figure 2 is a SEM microscopic morphology of the polyimide / nanofiber / carbon nanotube composite aerogel in Examples 1 to 4;
[0032] Figure 3 is a compressive stress curve at 80% strain in the polyimide nanofiber / carbon nanotube composite aerogel in Examples 1 to 4 and Comparative Example 1;
[0033] Figure 4 is a compression stress-strain curve of the polyimide nanofiber / carbon nanotube composite aerogel in Example 1 after 100 compression cycles;
[0034] Figure 5 is a thermogravimetric analysis (TGA) curve of the polyimide nanofiber composite aerogel in Examples 1 to 4 and Comparative Example 1;
[0035] Figure 6 The time-current curve of the polyimide nanofiber / carbon nanotube composite aerogel under different compressive stresses in Example 4 DETAILED DESCRIPTION
[0036] The invention is further described below in conjunction with specific examples. It should be noted that the following examples are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. Therefore, although the present invention has been described in detail in this specification with reference to the following examples, it should be understood by those skilled in the art that the present invention can still be modified or replaced by equivalents; and all technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.
[0037] Example 1
[0038] Polyamic acid (PAA) fibers of the PMDA-ODA (thermosetting) / ODPA-ODA (hot melt) system are prepared, and polyimide (PI) nanofibers of the PMDA-ODA / ODPA-ODA system are obtained after high-temperature imidization. Then, carbon nanotubes are dispersed in a water-soluble PAA solution and the above-mentioned PI nanofibers are dispersed therein by a homogenizer, and then poured into a mold for freeze-drying, and then subjected to high-temperature thermal imidization to obtain a PI nanofiber / carbon nanotube composite aerogel with a certain cross-linked structure.
[0039] (1) Weigh 2.016 g of pyromellitic dianhydride (PMDA) and 1.850 g of 4,4'-diaminodiphenyl ether (ODA) in a molar ratio of 1:1, dissolve all of the ODA in 30 mL of N,N'-dimethylformamide (DMF) solvent, and stir mechanically. After all of the ODA is dissolved in the DMF, add PMDA in an ice-water bath, stir evenly, and react for 4 h to obtain a PAA solution with a solid content of 12 wt%. Then, the PAA solution is loaded into a 20 mL syringe, and a PAA nanofiber membrane is prepared by electrospinning technology. The membrane is imidized at 300 °C to obtain PI nanofibers of the PMDA-ODA system, and the PI nanofibers of the ODPA-ODA system are prepared by the same method.
[0040] (2) The PAA solution of the PMDA-ODA system was slowly poured into magnetically stirred deionized water, allowed to stand for 24 h for solvent exchange, and then placed in a freeze dryer for vacuum freeze drying to obtain anhydrous PAA solid.
[0041] (3) The above-mentioned anhydrous PAA solid, triethylamine, deionized water and tert-butanol are mixed and dissolved in a ratio of 0.1g:0.3g:90g:10g to obtain a water-soluble PAA solution, and then 0.1g of carbon nanotubes are slowly added to the above-mentioned anhydrous PAA solution and dispersed evenly under ultrasound to obtain a carbon nanotube dispersion; then 0.8g of PI nanofibers of the PMDA-ODA system and 0.1g of PI nanofibers of the ODPA-ODA system are added to the above-mentioned carbon nanotube dispersion, and dispersed evenly with a homogenizer to obtain a PI nanofiber / carbon nanotube composite dispersion.
[0042] (4) Pour the above PI nanofiber / carbon nanotube composite dispersion into a mold and place it in a vacuum freeze dryer to prepare uncrosslinked PI nanofiber / carbon nanotube composite aerogel by vacuum freeze drying (vacuum degree of 0-10Pa, drying time of 72h); finally, place the above aerogel in a hot furnace, heat it from room temperature to 300℃ at a heating rate of 2℃ / min and keep it warm for 0.5h, so as to prepare a PI nanofiber / carbon nanotube composite conductive aerogel with a crosslinked morphology. The density of the aerogel is 12.241mg / cm 3 , the porosity is 99.261%, the shrinkage is 3.243%, and the stress under the compressive strain of 80% is 20.359 kPa.
[0043] Comparative Example 1
[0044] According to Example 1, no carbon nanotubes were added, and the remaining steps were the same as in Example 1 to obtain PI nanofiber aerogel, the density of which was 10.417 mg / cm 3 , the porosity is 99.83%, the shrinkage is 18.55%, and the stress under the compressive strain of 80% is 18.450 kPa.
[0045] Example 2
[0046] PAA fibers of PMDA-ODA (thermosetting) / ODPA-ODA (hot melt) system are prepared, and PI nanofibers of PMDA-ODA / ODPA-ODA system are obtained after high-temperature imidization. Then, carbon nanotubes are dispersed in a water-soluble PAA solution and the above-mentioned polyimide nanofibers are dispersed therein by a homogenizer, poured into a mold for freeze-drying, and then subjected to high-temperature thermal imidization to obtain a polyimide nanofiber / carbon nanotube composite aerogel with a certain cross-linked structure.
[0047] (1) Weigh 2.016 g of pyromellitic anhydride (PMDA) and 1.850 g of 4,4'-diaminodiphenyl ether (ODA) in a molar ratio of 1:1, dissolve all of the ODA in 30 mL of N,N'-dimethylformamide (DMF) solvent, stir mechanically, and after all of the ODA is dissolved in the DMF, add PMDA under ice-water bath conditions to obtain a PAA solution with a solid content of 12 wt%, which is then loaded into a 20 mL syringe, and the PAA nanofibers are prepared using electrospinning technology. The specific parameters of the electrospinning machine are spinning voltage: 20 kV; spinning temperature: room temperature; spinning humidity: 40%; syringe needle diameter: No. 18; receiving roller speed: 80.0 m / min; receiving distance: 20 cm. The prepared PAA nanofiber membrane is imidized at 300 °C to obtain a PMDA-ODA system PI nanofiber membrane, and the ODPA-ODA system PI nanofiber is prepared using the same method.
[0048] (2) The PAA solution of the PMDA-ODA system was slowly poured into magnetically stirred deionized water, allowed to stand for 24 h for solvent exchange, and then placed in a freeze dryer for vacuum freeze drying to obtain anhydrous PAA solid.
[0049] (3) The above-mentioned anhydrous PAA solid, triethylamine, deionized water and tert-butanol are mixed and dissolved in a ratio of 0.1g:0.3g:90g:10g to obtain a water-soluble PAA solution, and then 0.2g of carbon nanotubes are slowly added to the above-mentioned anhydrous PAA solution and dispersed evenly under ultrasound to obtain a carbon nanotube dispersion; then 0.8g of PMDA-ODA and 0.1g of PI nanofiber membrane of the ODPA-ODA system are added to the above-mentioned carbon nanotube dispersion and dispersed evenly under a homogenizer to obtain a PI nanofiber / carbon nanotube composite dispersion.
[0050] (4) Pour the above PI nanofiber / carbon nanotube composite dispersion into a mold and place it in a vacuum freeze dryer to prepare uncrosslinked PI nanofiber / carbon nanotube composite aerogel by vacuum freeze drying (vacuum degree 0-10Pa, drying time 72h); finally, place the above aerogel in a hot furnace, heat it from room temperature to 300℃ at a heating rate of 2℃ / min and keep it warm for 0.5h, so as to prepare a PI nanofiber / carbon nanotube composite conductive aerogel with a crosslinked morphology. The density of the aerogel is 13.535mg / cm 3 , the porosity is 99.04%, the shrinkage is 7.026%, and the stress under the compressive strain of 80% is 29.770 kPa.
[0051] Example 3
[0052] PAA fibers of the PMDA-ODA / ODPA-ODA system were prepared, and PI nanofibers of the PMDA-ODA / ODPA-ODA system were obtained after high-temperature imidization. Then, carbon nanotubes were dispersed in a water-soluble PAA solution and the PI nanofibers were dispersed therein by a homogenizer. The solution was poured into a mold for freeze-drying, and then subjected to high-temperature thermal imidization to obtain a PI nanofiber / carbon nanotube composite aerogel with a certain cross-linked structure.
[0053] (1) Weigh 2.016 g of pyromellitic dianhydride (PMDA) and 1.850 g of 4,4'-diaminodiphenyl ether (ODA) in a molar ratio of 1:1, dissolve all of the ODA in 30 mL of N,N'-dimethylformamide (DMF) solvent, stir mechanically, and after all of the ODA is dissolved in the DMF, add PMDA under ice-water bath conditions to obtain a PAA solution with a solid content of 12 wt%, and then load the PAA solution into a 20 mL syringe, and use electrospinning technology to prepare PAA nanofiber membranes. The specific parameters of the electrospinning machine are spinning voltage: 20 kV; spinning temperature: room temperature; spinning humidity: 40%; syringe needle diameter: 18; receiving roller speed: 80.0 m / min; receiving distance: 20 cm. The prepared PAA nanofiber membrane is imidized at 300 ° C to obtain a PMDA-ODA system PI nanofiber membrane, and the same method is used to prepare ODPA-ODA system PI nanofibers.
[0054] (2) The PAA solution of the PMDA-ODA system was slowly poured into magnetically stirred deionized water, allowed to stand for 24 h for solvent exchange, and then placed in a freeze dryer for vacuum freeze drying to obtain anhydrous PAA solid.
[0055] (3) The anhydrous PAA solid, triethylamine, deionized water and tert-butanol are mixed and dissolved in a ratio of 0.1 g: 0.3 g: 90 g: 10 g to obtain a water-soluble PAA solution, and then 0.3 g of carbon nanotubes are slowly added to the anhydrous PAA solution and dispersed evenly under ultrasound to obtain a carbon nanotube dispersion; then 0.8 g of PI nanofibers of the PMDA-ODA system and 0.1 g of PI nanofibers of the ODPA-ODA system are added to the carbon nanotube dispersion and dispersed evenly using a homogenizer to obtain a PI nanofiber / carbon nanotube composite dispersion.
[0056] (4) Pour the above PI nanofiber / carbon nanotube composite dispersion into a mold and place it in a vacuum freeze dryer to prepare uncrosslinked PI nanofiber / carbon nanotube composite aerogel by vacuum freeze drying (vacuum degree 0-10Pa, drying time 72h); finally, place the above aerogel in a hot furnace, heat it from room temperature to 300℃ at a heating rate of 2℃ / min and keep it warm for 0.5h, so as to prepare a PI nanofiber / carbon nanotube composite conductive aerogel with a crosslinked morphology. The density of the aerogel is 14.496mg / cm 3 , the porosity is 98.972%, the shrinkage is 7.505%, and the stress under the compressive strain of 80% is 44.2298 kPa.
[0057] Example 4
[0058] A PAA nanofiber membrane of a PMDA-ODA / ODPA-ODA system is prepared, and a PI nanofiber membrane of a PMDA-ODA / ODPA-ODA system is obtained after high-temperature imidization. Then, carbon nanotubes are dispersed in a water-soluble PAA solution and the polyimide nanofibers are dispersed therein by a homogenizer. The solution is poured into a mold for freeze-drying, and then subjected to high-temperature thermal imidization to obtain a polyimide nanofiber / carbon nanotube composite aerogel with a certain cross-linked structure.
[0059] (1) Weigh 2.016 g of pyromellitic anhydride (PMDA) and 1.850 g of 4,4'-diaminodiphenyl ether (ODA) in a molar ratio of 1:1, dissolve all of the ODA in 30 mL of N,N'-dimethylformamide (DMF) solvent, stir mechanically, and after all of the ODA is dissolved in the DMF, add PMDA under ice-water bath conditions to obtain a PAA solution with a solid content of 12 wt%, and then load the PAA solution into a 20 mL syringe, and use electrospinning technology to prepare PAA nanofiber membranes. The specific parameters of the electrospinning machine are spinning voltage: 20 kV; spinning temperature: room temperature; spinning humidity: 40%; syringe needle diameter: 18; receiving roller speed: 80.0 m / min; receiving distance: 20 cm. The prepared PAA nanofiber membrane is imidized at 300 ° C to obtain a PI nanofiber membrane of the PMDA-ODA system, and the PI nanofiber membrane of the ODPA-ODA system is prepared by the same method.
[0060] (2) The PAA solution of the PMDA-ODA system was slowly poured into magnetically stirred deionized water, allowed to stand for 24 h for solvent exchange, and then placed in a freeze dryer for vacuum freeze drying to obtain anhydrous PAA solid.
[0061] (3) The above-mentioned anhydrous PAA solid, triethylamine, deionized water and tert-butanol are mixed and dissolved in a ratio of 0.1g:0.3g:90g:10g to obtain a water-soluble PAA solution, and then 0.4g of carbon nanotubes are slowly added to the above-mentioned anhydrous PAA solution and dispersed evenly under ultrasound to obtain a carbon nanotube dispersion; then 0.8g of PI nanofibers of the PMDA-ODA system and 0.1g of PI nanofibers of the ODPA-ODA system are added to the above-mentioned carbon nanotube dispersion and dispersed evenly in a homogenizer to obtain a PI nanofiber / carbon nanotube composite dispersion.
[0062] (4) Pour the above PI nanofiber / carbon nanotube composite dispersion into a mold and place it in a vacuum freeze dryer to prepare uncrosslinked PI nanofiber / carbon nanotube composite aerogel by vacuum freeze drying (vacuum degree of 0-10Pa, drying time of 72h); finally, place the above aerogel in a hot furnace, heat it from room temperature to 300℃ at a heating rate of 2℃ / min and keep it warm for 0.5h, so as to prepare a PI nanofiber / carbon nanotube composite conductive aerogel with a crosslinked morphology. The density of the aerogel is 15.529mg / cm 3 , the porosity is 98.899%, the shrinkage is 3.524%, and the stress under the compressive strain of 80% is 26.002 kPa.
[0063] Example 5
[0064] PAA fibers of the BPDA-ODA / ODPA-ODA system were prepared, and PI nanofibers of the PMDA-ODA / ODPA-ODA system were obtained after high-temperature imidization. Then, carbon nanotubes were dispersed in a water-soluble PAA solution and the PI nanofibers were dispersed therein by a homogenizer. The solution was poured into a mold for freeze-drying, and then subjected to high-temperature thermal imidization to obtain a polyimide nanofiber / carbon nanotube composite aerogel with a certain cross-linked structure.
[0065] (1) Weigh 2.30 g of biphenyltetracarboxylic acid dianhydride (BPDA) and 1.565 g of 4,4'-diaminodiphenyl ether (ODA) in a molar ratio of 1:1, dissolve all of the ODA in 30 mL of N,N'-dimethylformamide (DMF) solvent, stir mechanically, and after all of the ODA is dissolved in the DMF, add BPDA under ice-water bath conditions to obtain a PAA solution with a solid content of 12 wt%, and then load the PAA solution into a 20 mL syringe, and use electrospinning technology to prepare PAA nanofiber membranes. The specific parameters of the electrospinning machine are spinning voltage: 20 kV; spinning temperature: room temperature; spinning humidity: 40%; syringe needle diameter: No. 18; receiving roller speed: 80.0 m / min; receiving distance: 20 cm. The prepared PAA nanofiber membrane is imidized at 300 ° C to obtain a PI nanofiber membrane of the BPDA-ODA system, and the PI nanofiber of the ODPA-ODA system is prepared by the same method.
[0066] (2) The PAA solution of the BPDA-ODA system was slowly poured into magnetically stirred deionized water, allowed to stand for 24 h for solvent exchange, and then placed in a freeze dryer for vacuum freeze drying to obtain anhydrous PAA solid.
[0067] (3) The above-mentioned anhydrous PAA solid, triethylamine, deionized water and tert-butanol are mixed and dissolved in a ratio of 0.1g:0.3g:90g:10g to obtain a water-soluble PAA solution, and then 0.4g of carbon nanotubes are slowly added to the above-mentioned anhydrous PAA solution and dispersed evenly under ultrasound to obtain a carbon nanotube dispersion; then 0.8g of PI nanofibers of the BPDA-ODA system and 0.1g of PI nanofibers of the ODPA-ODA system are added to the above-mentioned carbon nanotube dispersion and dispersed evenly in a homogenizer to obtain a PI nanofiber / carbon nanotube composite dispersion.
[0068] (4) Pour the above PI nanofiber / carbon nanotube composite dispersion into a mold and place it in a vacuum freeze dryer to prepare uncrosslinked PI nanofiber / carbon nanotube composite aerogel by vacuum freeze drying (vacuum degree 0-10Pa, drying time 72h); finally, place the above aerogel in a hot furnace, heat it from room temperature to 280℃ at a heating rate of 2℃ / min and keep it warm for 0.5h, so as to prepare a PI nanofiber / carbon nanotube composite conductive aerogel with a crosslinked morphology. The density of the aerogel is 16.252mg / cm 3 , the porosity is 99.025%, the shrinkage is 5.295%, and the stress under the compressive strain of 80% is 24.325 kPa.
[0069] Example 6
[0070] PAA fibers of the ODPA-ODA system are prepared, and PI nanofibers of the ODPA-ODA system are obtained after high-temperature imidization. Then, carbon nanotubes are dispersed in a water-soluble PAA solution and the above-mentioned PI nanofibers are dispersed therein by a homogenizer. The solution is then poured into a mold for freeze-drying, and then subjected to high-temperature thermal imidization to obtain a PI nanofiber / carbon nanotube composite aerogel with a certain cross-linked structure.
[0071] (1) Weigh 3.04 g of 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride (ODPA) and 1.96 g of 4,4'-diaminodiphenyl ether (ODA) in a molar ratio of 1:1, dissolve all of the ODA in 30 mL of N,N'-dimethylformamide (DMF) solvent, stir mechanically, and after all of the ODA is dissolved in the DMF, add ODPA under ice-water bath conditions to obtain a PAA solution with a solid content of 15 wt%, then load the PAA solution into a 20 mL syringe, and use electrospinning technology to prepare PAA nanofibers. The specific parameters of the electrospinning machine are spinning voltage: 20 kV; spinning temperature: room temperature; spinning humidity: 40%; syringe needle diameter: 18; receiving roller speed: 80.0 m / min; receiving distance: 20 cm. The prepared PAA nanofiber membrane is imidized at 300 ° C to obtain a PI nanofiber membrane of the ODPA-ODA system.
[0072] (2) The PAA solution of the ODPA-ODA system was slowly poured into magnetically stirred deionized water, allowed to stand for 24 h for solvent exchange, and then placed in a freeze dryer for vacuum freeze drying to obtain anhydrous PAA solid.
[0073] (3) The above-mentioned anhydrous PAA solid, triethylamine, deionized water and tert-butanol are mixed and dissolved in a ratio of 0.1g:0.3g:90g:10g to obtain a water-soluble PAA solution, and then 0.4g of carbon nanotubes are slowly added to the above-mentioned anhydrous PAA solution and dispersed evenly under ultrasound to obtain a carbon nanotube dispersion; then 0.9g of the PI nanofiber membrane of the ODPA-ODA system is added to the above-mentioned carbon nanotube dispersion and dispersed evenly in a homogenizer to obtain a PI nanofiber / carbon nanotube composite dispersion.
[0074] (4) Pour the above PI nanofiber / carbon nanotube composite dispersion into a mold and place it in a vacuum freeze dryer to prepare uncrosslinked PI nanofiber / carbon nanotube composite aerogel by vacuum freeze drying (vacuum degree of 0-10Pa, drying time of 72h); finally, place the above aerogel in a hot furnace, heat it from room temperature to 150℃ at a heating rate of 2℃ / min and keep it warm for 0.5h, and then heat it to 320℃ at a heating rate of 2℃ / min and keep it warm for 0.5h, so as to prepare PI nanofiber / carbon nanotube composite conductive aerogel with crosslinked morphology. The density of the aerogel is 21.042mg / cm 3 , the porosity is 99.315%, the shrinkage is 12.217%, and the stress under the compressive strain of 80% is 55.256 kPa.
Claims
1. A polyimide nanofiber / carbon nanotube composite conductive aerogel, characterized in that: The polyimide nanofiber / carbon nanotube composite conductive aerogel comprises a skeleton material, a conductive filler and a bonding component; The skeleton material includes at least one polyimide nanofiber; The conductive filler includes carbon nanotubes; The bonding component includes at least one polyimide; In parts by weight, the skeleton material is 90 parts by weight, the conductive filler is 20 to 40 parts by weight, and the bonding component is 1 to 40 parts by weight; The apparent density of the polyimide nanofiber / carbon nanotube composite conductive aerogel is 5 to 50 mg / cm 3 , The diameter of the polyimide nanofiber is 20 to 1000 nm. The method for preparing the polyimide nanofiber / carbon nanotube composite conductive aerogel comprises the following steps: A: using dibasic acid anhydride and diamine to condense into a polyamic acid solution, preparing the obtained polyamic acid solution into polyamic acid nanofibers, and then subjecting the obtained polyamic acid nanofibers to thermal imidization treatment to obtain polyimide nanofibers; B: using dibasic acid anhydride and diamine to condense into a thermosetting polyamic acid solution, pouring the solution into a coagulation liquid, filtering, and drying to obtain an anhydrous polyamic acid solid; C: dissolving anhydrous polyamic acid solid in an aqueous mixed solvent to obtain a water-soluble polyamic acid solution, and then dispersing carbon nanotubes in the water-soluble polyamic acid solution to obtain a carbon nanotube dispersion; D: crushing one or more polyimide nanofibers and dispersing them in the above carbon nanotube dispersion to obtain a polyimide nanofiber / carbon nanotube composite dispersion; The polyimide nanofibers are hot-melt polyimide nanofibers or a mixture of hot-melt polyimide nanofibers and thermosetting polyimide nanofibers; E: The polyimide nanofiber / carbon nanotube composite dispersion in step D is rapidly frozen to prepare a crystalline phase of the composite dispersion; freeze-dried and then thermally imidized to obtain a polyimide nanofiber / carbon nanotube composite conductive aerogel.
2. The polyimide nanofiber / carbon nanotube composite conductive aerogel according to claim 1, wherein: The solid content of the polyamic acid solution in step A is 5-30wt%; The method for preparing the polyamic acid nanofibers is one or more of electrospinning, air blowing spinning, and air blowing assisted electrospinning; The thermal imidization temperature is 250-400°C.
3. The polyimide nanofiber / carbon nanotube composite conductive aerogel according to claim 1, wherein: The coagulation liquid in step B is at least one of deionized water, ethanol, acetone, ethyl acetate, and hydrocarbons.
4. The polyimide nanofiber / carbon nanotube composite conductive aerogel according to claim 1, wherein: The aqueous mixed solvent in step C is a mixed solution of organic amine, deionized water and low-carbon alcohol; The organic amine is a fatty amine, including at least one of ethylenediamine, triethylamine and isopropylamine; The low-carbon alcohol is at least one of ethanol, methanol, tert-butanol and propanol; The mass ratio of anhydrous polyamic acid solid to organic amine is 1:1 to 1:
6. The mass ratio of deionized water to low-carbon alcohol is 10:0.1 to 5:
5. The mass ratio of the anhydrous polyamic acid solid to deionized water is 0.01-0.5%.
5. The polyimide nanofiber / carbon nanotube composite conductive aerogel according to claim 1, wherein: The hot-melt polyimide nanofibers described in step D are selected from one or more of hexafluorodianhydride / 4,4'-diaminodiphenyl ether system polyimide nanofibers, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride / 4,4'-diaminodiphenyl ether system polyimide nanofibers, bisphenol A dianhydride / 4,4'-diaminodiphenyl ether system polyimide nanofibers, polyimide nanofibers containing 4,4'-diaminodiphenylmethane system in the structure, and P84 type polyimide nanofibers.
6. The polyimide nanofiber / carbon nanotube composite conductive aerogel according to claim 1, wherein: The thermosetting polyimide nanofiber is prepared by dibasic acid anhydride and diamine. The dibasic acid anhydride is one or a mixture of two or more of biphenyltetracarboxylic acid anhydride, pyromellitic acid anhydride, benzophenonetetracarboxylic acid anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic acid anhydride, and 3,4,9,10-tetracarboxylic acid anhydride. The diamine is one or a mixture of two or more of diaminodiphenyl ether, p-phenylenediamine, 4,4'-diaminodiphenyl sulfone, 9,9-bis(4-aminophenyl)fluorene and 2,2'-bis(trifluoromethyl)diaminobiphenyl.
7. The polyimide nanofiber / carbon nanotube composite conductive aerogel according to claim 1, wherein: The mass concentration of the composite dispersion of polyimide nanofibers / carbon nanotubes in step D is 0.5-5 wt %.
8. The polyimide nanofiber / carbon nanotube composite conductive aerogel according to claim 1, wherein: The thermal imidization treatment in step E is to increase the temperature from room temperature to 250-400° C. and keep the temperature for 1-60 minutes, with a heating rate of 1-20° C. / min.
9. The method for preparing the polyimide nanofiber / carbon nanotube composite conductive aerogel according to any one of claims 1 to 8, comprising the following steps: A: using dibasic acid anhydride and diamine to condense into a polyamic acid solution, preparing the obtained polyamic acid solution into polyamic acid nanofibers, and then subjecting the obtained polyamic acid nanofibers to thermal imidization treatment to obtain polyimide nanofibers; B: using dibasic acid anhydride and diamine to condense into a thermosetting polyamic acid solution, pouring the solution into a coagulation liquid, filtering, and drying to obtain an anhydrous polyamic acid solid; C: dissolving anhydrous polyamic acid solid in an aqueous mixed solvent to obtain a water-soluble polyamic acid solution, and then dispersing carbon nanotubes in the water-soluble polyamic acid solution to obtain a carbon nanotube dispersion; D: crushing one or more polyimide nanofibers and dispersing them in the above carbon nanotube dispersion to obtain a polyimide nanofiber / carbon nanotube composite dispersion; The polyimide nanofibers are hot-melt polyimide nanofibers or a mixture of hot-melt polyimide nanofibers and thermosetting polyimide nanofibers; E: The polyimide nanofiber / carbon nanotube composite dispersion in step D is rapidly frozen to prepare a crystalline phase of the composite dispersion; freeze-dried and then thermally imidized to obtain a polyimide nanofiber / carbon nanotube composite conductive aerogel.
10. The preparation method according to claim 9, wherein: The solid content of the polyamic acid solution in step A is 5-30wt%; the method for preparing polyamic acid nanofibers is one or more of electrospinning, air blowing spinning, and air blowing assisted electrospinning; The thermal imidization temperature is 250-400°C.
11. The preparation method according to claim 9, wherein: The coagulation liquid in step B is at least one of deionized water, ethanol, acetone, ethyl acetate, and hydrocarbons.
12. The preparation method according to claim 9, wherein: The aqueous mixed solvent in step C is a mixed solution of organic amine, deionized water and low-carbon alcohol; The organic amine is a fatty amine, including at least one of ethylenediamine, triethylamine and isopropylamine; The low-carbon alcohol is at least one of ethanol, methanol, tert-butanol and propanol; The mass ratio of anhydrous polyamic acid solid to organic amine is 1:1 to 1:
6. The mass ratio of deionized water to low-carbon alcohol is 10:0.1 to 5:
5. The mass ratio of the anhydrous polyamic acid solid to deionized water is 0.01-0.5%.
13. The preparation method according to claim 9, wherein: The hot-melt polyimide nanofibers described in step D are selected from one or more of hexafluorodianhydride / 4,4'-diaminodiphenyl ether system polyimide nanofibers, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride / 4,4'-diaminodiphenyl ether system polyimide nanofibers, bisphenol A dianhydride / 4,4'-diaminodiphenyl ether system polyimide nanofibers, polyimide nanofibers containing 4,4'-diaminodiphenylmethane system in the structure, and P84 type polyimide nanofibers.
14. The preparation method according to claim 9, wherein: The thermosetting polyimide nanofiber is prepared by dibasic acid anhydride and diamine. The dibasic acid anhydride is one or a mixture of two or more of biphenyltetracarboxylic acid anhydride, pyromellitic acid anhydride, benzophenonetetracarboxylic acid anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic acid anhydride, and 3,4,9,10-tetracarboxylic acid anhydride. The diamine is one or a mixture of two or more of diaminodiphenyl ether, p-phenylenediamine, 4,4'-diaminodiphenyl sulfone, 9,9-bis(4-aminophenyl)fluorene and 2,2'-bis(trifluoromethyl)diaminobiphenyl.
15. The preparation method according to claim 9, wherein: The mass concentration of the composite dispersion of polyimide nanofibers / carbon nanotubes in step D is 0.5-5 wt %.
16. The preparation method according to claim 9, wherein: The thermal imidization treatment in step E is to increase the temperature from room temperature to 250-400° C. and keep the temperature for 1-60 minutes, with a heating rate of 1-20° C. / min.
17. A product comprising the polyimide nanofiber / carbon nanotube composite conductive aerogel according to any one of claims 1 to 8 or the polyimide nanofiber / carbon nanotube composite conductive aerogel prepared by the preparation method according to any one of claims 9 to 16.
Citation Information
Patent Citations
RGO / polyimide composite aerogel, preparation method and application thereof
CN111218112A
Thermal-insulation anisotropic polyimide nanofiber aerogel and preparation method thereof
CN110157035A