A catalyst for preparing symmetrical octahydroanthracene, preparation method and application thereof
Through the preparation method of supported metal catalysts, the problems of harsh conditions and low conversion of the hydrogenation process of fused ring aromatic hydrocarbons are solved, and the method of efficient preparation of symmetric octahydroanthracene is realized. It has high selectivity and mild process conditions and is suitable for industrial production.
Patent Information
- Application Number
- CN202310186847.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-01
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-03-01
AI Technical Summary
In the prior art, the hydrogenation process conditions of the condensed ring aromatic hydrocarbons are harsh and the conversion rate is low. The conversion rate and selectivity of the benzene ring selected hydrogenation catalyst in the condensed ring aromatic hydrocarbons are low, making it difficult to efficiently prepare symmetric octahydroanthracene.
Using the catalyst preparation method of metal-supported metal, the precursor metal salt is uniformly dispersed on the support and reduced treatment in a sodium hydroxide solution, followed by secondary reduction in a tube furnace to form a catalyst and in an autoclave. Carry out hydrogenation reaction.
It achieves 100% conversion of anthracene and more than 80% selectivity of symmetric octahydroanthracene. The process conditions are mild, green and environmentally friendly, and easy to produce in industrialization.
Smart Images

Figure CN116159558B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coal chemical industry and fine chemical industry, and particularly relates to a catalyst for preparing symmetrical octahydroanthracene, a preparation method and an application thereof. Background Art
[0002] Anthracene, as a typical polycyclic aromatic hydrocarbon, exists in large quantities in heavy crude oil and coal tar. It is a type of carcinogen itself, which seriously threatens human health. With the development of fine chemicals, people's demand for fine chemicals is increasing. Among them, the hydrogenation product of anthracene, symmetrical octahydroanthracene, is an important industrial intermediate that can effectively replace tetramethylbenzene and is widely used in the production of tetracarboxylic anhydride, polyimide resin, dyes, plasticizers, and surfactants.
[0003] Traditional anthracene hydrogenation catalysts mainly use metal sulfide catalysts, such as patent CN105772034A using microemulsion method to prepare molybdenum disulfide catalysts can achieve different hydrogenation performance, isomerization performance and hydrocracking performance by regulating process conditions, but it needs to be carried out under high temperature and high pressure harsh conditions with a maximum temperature of 300 ° C and a maximum pressure of 7MPa, and the reaction is easily restricted by thermodynamic equilibrium, so the ability to hydrogenate anthracene is greatly limited. Patent CN108586182A uses a loaded precious metal catalyst prepared by strong electrostatic adsorption theory for anthracene hydrogenation to prepare symmetrical octahydroanthracene, but its catalyst preparation process is cumbersome and the process flow is complicated, making it difficult to mass produce the catalyst. Patent CN115108877A uses low-toxicity manganese compounds to catalyze anthracene hydrogenation. After a long high-pressure reaction of 12-24h, the depth of hydrogenation is limited to dihydroanthracene, which is affected by the saturated market environment and limits its further application. Patent CN111718232A discloses a method for producing high-energy hydrocarbon fuel by hydrogenating anthracene oil with a noble metal supported catalyst, which mainly involves hydrofining anthracene oil, and does not involve selective hydrogenation of anthracene to prepare fine chemical intermediates. In addition, other patents involve reports on selective hydrogenation to high-end target products (symmetrical octahydroanthracene). Therefore, seeking a catalyst that can both efficiently convert condensed aromatics and selectively hydrogenate the benzene rings in condensed aromatics, and providing an effective way to efficiently utilize coal tar to prepare fine chemicals (symmetrical octahydroanthracene) has become a hot topic in current research. Summary of the invention
[0004] Aiming at the problems of harsh process conditions and low conversion rate of hydrogenation of polycyclic aromatic hydrocarbons, and low conversion rate and selectivity of catalysts for selective hydrogenation of benzene rings in polycyclic aromatic hydrocarbons, the present invention provides a catalyst, preparation method and application of symmetrical octahydroanthracene. The current situation urgently needs to realize the transformation of products from primary resource type to high-end material type and high added value type.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a catalyst for preparing symmetrical octahydroanthracene, comprising the following steps:
[0007] Step 1, loading the metal on the carrier: placing the carrier in water and ultrasonicating it to make it uniformly dispersed in the water, then pouring the precursor metal salt into the above uniform dispersion, stirring continuously during the process so that the active component is uniformly loaded on the carrier;
[0008] Step 2, chemical reagent reduction: adding sodium hydroxide solution to the above-mentioned dispersion after loading to adjust the pH value to 8-10, adding reducing agent while stirring for reduction; after the reduction is completed, suction filtration, washing and vacuum drying;
[0009] Step 3, secondary reduction in a tubular furnace: Place the dried catalyst in a tubular furnace and reduce it in a hydrogen atmosphere. Secondary reduction ensures the reduction of the active components of the catalyst on the one hand, and on the other hand, it can promote a stronger interaction between some carriers and active components to construct the SMSI effect. (If the catalyst to be protected is not secondary reduced or the reduction temperature is not right, the hydrogenation effect will be very poor).
[0010] Furthermore, the carrier is a mixture of one or more of magnesium oxide, calcium oxide, calcium carbonate, zinc oxide, aluminum oxide, silicon oxide, or silicon carbide.
[0011] Furthermore, the precursor metal salt is PdCl2, Pd(OAc)2, H2PtCl6, RuCl3, H 12 C l6 One of the noble metal salts such as N3Rh, and the metal loading amount is 0.5 to 5 wt%.
[0012] Furthermore, the reducing agent is one of sodium borohydride, hydrazine hydrate and methanol.
[0013] Furthermore, in step 3, the secondary reduction temperature of the tubular furnace is 100-500°C.
[0014] In the application of the catalyst obtained by the above preparation method in the preparation of symmetrical octahydroanthracene by hydrogenation of anthracene, anthracene is dissolved in an organic solvent to prepare a solution of a certain concentration, and then the obtained solution and the catalyst are placed in a high-pressure reactor for hydrogenation reaction.
[0015] Furthermore, the organic solvent is one of cyclohexane, tetrahydrofuran and decahydronaphthalene, and the concentration of anthracene in the solution is 0.01 to 5 mol / L.
[0016] Furthermore, the mass ratio of the catalyst to anthracene is 0.5 to 3:1.
[0017] Furthermore, the reaction pressure in the high-pressure reactor is 0.5-8 MPa, the reaction temperature is 100-500° C., and the reaction time is 2-15 h.
[0018] A catalyst prepared according to the above preparation method.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] The present invention provides a method for preparing the catalyst for preparing symmetrical octahydroanthracene by highly selective hydrogenation of anthracene: (1) the conversion rate of anthracene reaches 100%, and the selectivity of symmetrical octahydroanthracene reaches more than 80%; (2) the raw materials for the synthesis of the catalyst are cheap, the operation steps are conventional, and the preparation scheme is highly adjustable; (3) the process conditions are mild, green and environmentally friendly, and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 TEM characterization image of the catalyst. DETAILED DESCRIPTION
[0022] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the following embodiments will provide a more comprehensive description of the present invention, but they should not be construed as limiting the practicable scope of the present invention.
[0023] The conversion and selectivity of the examples were calculated by gas chromatography area normalization method.
[0024] The gas chromatogram was obtained by a Japanese KYOWAGLAS-XAH-12 gas chromatograph.
[0025] Example 1
[0026] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 400℃ for 3h to obtain a 1wt% Pd / SiO2 catalyst.
[0027] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0028] Example 2
[0029] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 400℃ for 3h to obtain a 1wt% Pd / SiO2 catalyst.
[0030] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 1 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0031] Example 3
[0032] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 400℃ for 3h to obtain a 1wt% Pd / SiO2 catalyst.
[0033] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 5 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0034] Example 4
[0035] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add appropriate amount of PdCl2 solution dropwise during stirring and continue stirring for 3h. After complete impregnation, add 2mol / L NaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry and place it in a tubular furnace. After hydrogen reduction at 400℃ for 3h, a 1wt% Pd / SiO2 catalyst is obtained.
[0036] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 180°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the resulting solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0037] Example 5
[0038] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add appropriate amount of PdCl2 solution dropwise during stirring and continue stirring for 3h. After complete impregnation, add 2mol / L NaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry and place it in a tubular furnace. After hydrogen reduction at 400℃ for 3h, a 1wt% Pd / SiO2 catalyst is obtained.
[0039] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 220°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the resulting solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0040] Example 6
[0041] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 400℃ for 3h to obtain a 1wt% Pd / SiO2 catalyst.
[0042] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 200°C. The reaction was continued for 10 h with continuous stirring. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0043] Example 7
[0044] Weigh 0.2 g of ZnO carrier and disperse it in 50 mL of deionized water by ultrasonic dispersion, then stir it. During the stirring process, add an appropriate amount of PdCl2 solution dropwise and continue stirring for 3 hours. After complete impregnation, add 2 mol / L NaOH solution to adjust the pH of the turbid solution to 9. Then add 10 mL of 6 mol / L fresh sodium borohydride aqueous solution and continue stirring for 3 hours. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 400°C for 3 hours to obtain a 1 wt% Pd / ZnO catalyst.
[0045] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / ZnO catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 1 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0046] Example 8
[0047] Weigh 0.2g SiC carrier and disperse it in 50mL deionized water by ultrasonic dispersion and stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry and place it in a tubular furnace. After hydrogen reduction at 400℃ for 3h, a 1wt% Pd / Al2O3 catalyst is obtained.
[0048] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / Al2O3 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 1 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0049] Example 9
[0050] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion and stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After the impregnation is complete, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9, then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then filter, wash, dry and place in a tube furnace. Reduce with hydrogen at 400℃ for 3h to obtain 1wt% Pd / SiO2 catalyst. The same method is used to prepare 1wt% Pd / SiC catalyst.
[0051] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.025 g of 1 wt% Pd / SiO2 and 0.025 g of 1 wt% Pd / SiC catalyst were mixed evenly and added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen, and then the hydrogen pressure in the reactor was slowly controlled to 3 MPa. The temperature was set to 200°C and the reaction was continued for 8 h under continuous stirring. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0052] Example 10
[0053] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir. Add appropriate amount of H2PtCl6 solution dropwise during stirring and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry and place in a tubular furnace. After hydrogen reduction at 400℃ for 3h, a 1wt% Pt / SiO2 catalyst is obtained.
[0054] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pt / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0055] Embodiment 11
[0056] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 400℃ for 3h to obtain a 1wt% Pd / SiO2 catalyst.
[0057] Anthracene was dissolved in decahydronaphthalene to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0058] Example 12
[0059] Weigh 0.2g SiO2 carrier and disperse it in 50mL deionized water by ultrasonic dispersion, then stir it. Add an appropriate amount of PdCl2 solution dropwise during the stirring process and continue stirring for 3h. After complete impregnation, add 2mol / LNaOH solution to adjust the pH of the turbid solution to 9. Then add 10mL 6mol / L fresh sodium borohydride aqueous solution and continue stirring for 3h. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 500℃ for 3h to obtain a 1wt% Pd / SiO2 catalyst.
[0060] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / SiO2 catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 200°C. The reaction was continued with stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0061] Comparative Example
[0062] Weigh 0.2 g of activated carbon carrier and disperse it in 50 mL of deionized water by ultrasonic dispersion, then stir it. During the stirring process, add an appropriate amount of PdCl2 solution dropwise and continue stirring for 3 hours. After complete impregnation, add 2 mol / L NaOH solution to adjust the pH of the turbid solution to 9, then add 10 mL of 6 mol / L fresh sodium borohydride aqueous solution and continue stirring for 3 hours. Then, filter, wash, dry, place in a tubular furnace, and reduce with hydrogen at 400°C for 3 hours to obtain a 1 wt% Pd / AC catalyst.
[0063] Anthracene was dissolved in cyclohexane to prepare 10 mL of a 0.02 mol / L solution. 0.05 g of a 1 wt% Pd / AC catalyst was added to the solution. A hydrogenation reaction was carried out in a high-pressure reactor. The air in the reactor was first replaced with hydrogen. The hydrogen pressure in the reactor was then slowly controlled to 3 MPa. The temperature was set to 200°C. The reaction was continued under stirring for 8 h. After the reaction was completed, the obtained solution was characterized and calculated. The conversion rate and selectivity are listed in Table 1.
[0064] Table 1 Example reaction product conversion rate and octahydroanthracene selectivity
[0065]
[0066]
[0067] By comparing several groups of examples, it is not difficult to find that the catalyst and process conditions provided by the present invention have a very good implementation effect on the preparation of octahydroanthracene by hydrogenation of anthracene, and the total conversion rate can be guaranteed to be 100%, and the selectivity for symmetrical octahydroanthracene is extremely high, which is higher than 80%. Figure 1 As shown in the figure, by measuring the lattice fringes, it is consistent with the lattice size of a certain alloy catalyst. It is the SMSI effect constructed by this special preparation method that makes it show excellent activity and selectivity in the reaction of anthracene hydrogenation to prepare symmetrical octahydroanthracene.
[0068] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.
Claims
1. A method for preparing a catalyst for preparing symmetrical octahydroanthracene, characterized in that: The following steps are involved: Step 1, loading the metal on the carrier: placing the carrier in water and ultrasonicating it to make it uniformly dispersed in the water, then pouring the precursor metal salt into the above uniform dispersion, stirring continuously during the process so that the active component is uniformly loaded on the carrier; Step 2, chemical reagent reduction: adding sodium hydroxide solution to the above-mentioned dispersion after loading to adjust the pH value to 8-10, and adding reducing reagent while stirring for reduction; After the reduction is completed, the mixture is filtered, washed and vacuum dried; Step 3, secondary reduction in a tubular furnace: placing the dried catalyst in a tubular furnace and reducing it under a hydrogen atmosphere; The carrier is a mixture of one or more of zinc oxide, aluminum oxide, silicon oxide or silicon carbide; The precursor metal salt is PdCl2, Pd(OAc)2, H2PtCl6, RuCl3, H 12 C l6 One of N3Rh, and the metal loading is 0.5~5 wt%; In step 3, the secondary reduction temperature of the tubular furnace is 400-500° C.; The reducing agent is one of sodium borohydride and hydrazine hydrate.
2. An application of the catalyst obtained by the preparation method according to claim 1 in the preparation of symmetrical octahydroanthracene by hydrogenation of anthracene, characterized in that: Anthracene is dissolved in an organic solvent to prepare a solution, and then the obtained solution and a catalyst are placed in a high-pressure reactor for hydrogenation reaction.
3. The use according to claim 2, characterized in that: The organic solvent is one of cyclohexane, tetrahydrofuran and decahydronaphthalene, and the concentration of anthracene in the solution is 0.01-5 mol / L.
4. The use according to claim 2, characterized in that: The mass ratio of the catalyst to anthracene is 0.5-3:
1.
5. The use according to claim 2, characterized in that: The reaction pressure in the high-pressure reactor is 0.5-8 MPa, the reaction temperature is 100-500° C., and the reaction time is 2-15 h.
6. The catalyst prepared according to the preparation method of claim 1.
Citation Information
Patent Citations
Preparation method for hydrogenation catalyst for polycyclic aromatic hydrocarbons, catalyst and application thereof
CN105772034A
Method for preparing symmetrical octahydroanthracene by selective hydrogenating of anthracene
CN108586182A
Method for preparing anthracene and phenanthrene through co-carbonization of hydrogenated anthracene oil and refined asphalt
CN111718232A
Preparation method of 9, 10-dihydroanthracene
CN115108877A
Palladium catalyst for production of H2O2 by using fixed bed anthraquinone method and preparation method thereof
CN102389799A