A method for reducing scrap steel blowing loss in converter steelmaking process
By sorting and storing the steel outgoing parts after the converter furnace and precisely controlling the scrap steel structure model, adjusting the timing and amount of scrap steel added, the problem of scrap steel oxidation reaction during the converter steelmaking process is solved, and efficient resource utilization and production cost are achieved.
Patent Information
- Application Number
- CN202211464829.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-11-22
AI Technical Summary
During the converter steelmaking process, the oxidation reaction of iron and manganese and other elements in scrap steel leads to resource loss and increase solid waste, increasing production costs and environmental impact.
Install scrap steel into the bucket at the steel outlet after the converter furnace, store and add scrap steel according to type and block size. By accurately controlling the scrap steel structure model and argon blowing mode, the oxidation amount of scrap steel during the smelting process and the steel discharge process is reduced, and the steel discharge process is also reduced. Adjust the timing and amount of scrap steel to control the end point temperature of the converter.
It effectively reduces the blow loss of scrap steel, reduces the cost of steel materials and alloys, reduces the external discharge of solid waste and oxygen consumption, and improves resource utilization and production efficiency.
Smart Images

Figure CN115820972B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for reducing scrap steel blowing loss and lowering production costs in a converter steelmaking process. Background Art
[0002] Scrap steel is the main raw material for converter steelmaking production, accounting for about 10-30% of steel materials. In 2021, the scrap steel consumption of key steel enterprises across the country was about 130kg / t. Based on the national steel output of 1.03 billion tons in 2021, the national scrap steel consumption is more than 130 million tons. At present, most of the converter scrap steel of domestic and foreign steel mills is added to the converter furnace before converter smelting. The scrap steel structure is added according to the fixed structure of scrap steel resources, resulting in partial oxidation reaction of iron, manganese and other elements in the scrap steel with oxygen during the smelting process, producing oxides that enter the slag, resulting in the loss of beneficial elements such as iron and manganese in the scrap steel, reducing resource utilization.
[0003] In addition, after the iron, manganese and other elements in scrap steel are oxidized and enter the slag, the amount of solid waste such as slag and oxygen consumption will increase, which has a great impact on the company's energy conservation and emission reduction work. Summary of the invention
[0004] The purpose of the present invention is to provide a method for reducing scrap steel blowing loss in the converter steelmaking process. This method can effectively reduce the oxidation amount of elements such as iron and manganese in the scrap steel during the converter smelting process, thereby reducing the amount of solid waste discharged by the enterprise while reducing the cost of steel materials and alloys.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] The present invention provides a method for reducing scrap steel blowing loss in a converter steelmaking process, the method comprising the following steps:
[0007] 1) Install a scrap steel loading bucket above the steel tapping area behind the converter, open a chute connected to the top of the ladle, and install a gate valve between the chute and the loading bucket;
[0008] 2) Scrap steel is classified and stored and added according to its type and size. Scrap steel includes socially recycled crushed scrap steel and / or surface non-oxidized scrap steel with a size of ≤300mm;
[0009] 3) When loading the converter scrap steel, load the same scrap steel of the same type of steel smelted in the converter into the scrap steel loading bucket installed above the steel tapping area;
[0010] 4) The crushed scrap steel recycled from the society in the scrap steel added to the converter furnace is dynamically added according to the scrap steel structure model based on the precise control of the total amount of FeO raw materials entering the converter, and the total amount of scrap steel added to the converter furnace remains unchanged;
[0011] 5) After the alloy is added during the steel-making process, the ladle bottom blowing mode is selected with a large flow rate, and the lower gate valve of the scrap steel hopper is opened to add the same scrap steel as the smelting steel into the ladle;
[0012] 6) After steel is tapped, open the ladle to the argon blowing position for argon blowing or refining.
[0013] As a further improvement of the above method, in step 2), the crushed scrap steel recycled from the society is stored separately, and the surface non-oxidized scrap steel with a size of ≤300 mm is stored according to the major types of steel;
[0014] As a further improvement of the above method, the crushed scrap steel recycled by the society is bulk material or bulk material briquette with a maximum side length of ≤200mm, and the scrap steel has severe surface oxidation and an oxide ratio of 12±2%.
[0015] As a further improvement of the above method, the surface non-oxidized scrap steel with a block size of ≤300mm is classified into major steel types, and the major steel types are the common alloy element content of the steel type ±0.10%, and the trace element content ±0.010%.
[0016] As a further improvement of the above method, in step 3), the amount of similar scrap steel is controlled according to the steel output of 10±2kg / t, and the amount of scrap steel added to the converter furnace is reduced by 10±2kg / t accordingly.
[0017] As a further improvement of the above method, in step 4), the scrap steel structure model based on the precise control of the total amount of FeO in the converter raw material is a scrap steel structure model in which the amount of scrap steel containing a higher proportion of FeO is determined according to the total charge of the furnace, the molten iron charge and the amount of FeO coolant added.
[0018] As a further improvement of the above method, the scrap steel structure model calculates the demand for socially recycled scrap steel based on the FeO demand in the converter during smelting under different molten iron consumption and the amount of FeO brought in by the FeO-containing coolant added during the smelting process, and adds it as required to achieve a balance in FeO demand during the smelting process.
[0019] As a further improvement of the above method, the formula for calculating the demand for socially recycled scrap steel is: the demand for socially recycled scrap steel = (FeO content requirement in slag during smelting process - amount of FeO-containing coolant added * FeO content in coolant) / FeO content in socially recycled scrap steel * slag amount * steel output / proportion of FeO in the scrap steel participating in the reaction.
[0020] As a further improvement of the above method, the method also includes: the final temperature of the converter is controlled to be 10±2°C higher than the normal temperature.
[0021] As a further improvement of the above method, the bottom blowing flow rate in step 5) is 5.5 to 6.5 L / t.min.
[0022] Specifically, the method of the present invention comprises the following steps: installing a scrap steel loading bucket above the steel tapping position after the converter furnace, opening a chute connected to the top of the ladle, and installing a gate valve at the chute and the loading bucket; the scrap steel is classified and stored and added according to the type and size, wherein the crushed scrap steel recycled from the society is stored separately, and the surface non-oxidized scrap steel with a size of ≤300mm is classified and stored according to the major types of steel; when loading the converter scrap steel, the same type of scrap steel of the smelting steel type of the furnace is loaded into the scrap steel loading bucket installed above the steel tapping position, and the amount of the same type of scrap steel is controlled according to the steel tapping amount of 10±2kg / t, and the amount of scrap steel added to the converter furnace is reduced accordingly 10±2kg / t; the crushed scrap steel recycled from the society in the scrap steel in the converter is dynamically added according to the scrap steel structure model based on the precise control of the total amount of FeO raw materials entering the converter, and the total amount of scrap steel added to the converter remains unchanged; the final temperature of the converter is controlled at 10±2℃ higher than the normal temperature; after the alloy is added in the steelmaking process, the ladle bottom blowing mode selects the large flow model (flow rate 5.5~6.5L / t.min), and then the lower gate valve of the scrap steel hopper is opened to add the scrap steel of the same type as the smelting steel into the ladle; after the steelmaking is completed, the ladle is opened to the argon blowing position for argon blowing or refining.
[0023] Compared with the prior art, the advantages of the present invention are:
[0024] The present invention installs a scrap steel loading bucket above the steel tapping position after the converter, and the scrap steel is stored and added dynamically according to the major types of steel, appropriately increases the converter terminal temperature, adjusts the ladle bottom blowing model during the steel tapping process, and adds the same type of scrap steel as the smelting steel to the ladle, effectively reducing the scrap steel blowing loss during the converter smelting process, reducing the amount of alloy added, and reducing the amount of solid waste discharged by the enterprise while reducing the cost of steel materials and alloys. In addition, the method can reduce the amount of oxidation reaction during the converter smelting process, reduce oxygen consumption, and play a positive role in reducing process energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the scrap steel loading bucket above the steel tapping position after the converter furnace of the present invention;
[0026] Reference numerals:
[0027] 1. Scrap steel is loaded into bucket, 2. Gate valve, 3. Chute, 4. Ladle. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with specific embodiments.
[0029] In order to enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application are clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.
[0030] The present invention provides a method for reducing scrap steel blowing loss in a converter steelmaking process, the method comprising the following steps:
[0031] 1) Install a scrap steel loading bucket 1 above the steel tapping position after the converter furnace, open a chute 3 connected to the top of the ladle 4, and install a gate valve 2 between the chute and the loading bucket;
[0032] 2) Scrap steel is classified and stored according to type and size. Recycled scrap steel is stored separately, and surface-free scrap steel with a size of ≤300mm is stored according to the major types of steel.
[0033] Among them, the recycled crushed scrap steel is stored separately, and the surface non-oxidized scrap steel with a size of ≤300mm is stored by steel type. The recycled crushed scrap steel is bulk material or bulk material briquette with a maximum side length of ≤200mm, and the surface is severely oxidized. The oxide ratio is 12±2% (due to the severe oxidation of the crushed material surface, the price is about 300 yuan / t lower than other scrap steel); the surface non-oxidized scrap steel with a size of ≤300mm is stored by steel type, and the steel type category is the common alloy element content of the steel type ±0.10%, and the trace element content ±0.010%. In actual production, the main steel types smelted by the enterprise are mainly classified. Steel types that are not smelted or smelted in small quantities are not classified, and the post-furnace scrap steel process is not adopted;
[0034] 3) When loading the converter scrap steel, load the same type of scrap steel of the same type of steel being smelted in this furnace into the scrap steel loading bucket installed above the steel tapping position. The amount of the same type of scrap steel is controlled according to the steel tapping amount of 10±2kg / t, and the amount of scrap steel added to the converter furnace is reduced by 10±2kg / t accordingly;
[0035] 4) The crushed scrap steel recycled from the society in the scrap steel added to the converter furnace is dynamically added according to the scrap steel structure model based on the precise control of the total amount of FeO raw materials entering the converter, and the total amount of scrap steel added to the converter furnace remains unchanged;
[0036] The scrap steel structure model based on the precise control of the total amount of FeO in the raw materials fed into the converter is a scrap steel structure model that determines the amount of scrap steel with a high FeO ratio according to the total charge of this furnace, the charge of molten iron and the amount of FeO-containing coolant added, as shown in the following table; it is mainly based on the FeO demand in the converter furnace during smelting under different molten iron consumption and the amount of FeO brought by the FeO-containing coolant added during the smelting process, to calculate the demand for recycled crushed scrap steel in society, and add it as required to achieve the balance of FeO demand in the converter smelting process, to prevent the situation where the Fe element in the scrap steel is oxidized in large quantities due to insufficient FeO in the furnace during the smelting process, and to alleviate the problems of increased oxygen content in molten steel and alloy recovery rate due to excess FeO in the furnace during the smelting process and increased FeO in the slag. The calculation formula is as follows:
[0037] The demand for recycled crushed steel scrap = (FeO content requirement in slag during smelting process - FeO-containing coolant added * FeO content in coolant) / FeO content in recycled crushed steel scrap * slag volume * steel output / FeO participation ratio in the crushed steel scrap;
[0038] 5) The final temperature of the converter is controlled to be 10±2℃ higher than the normal temperature;
[0039] 6) After the alloy is added during the steel-making process, the ladle bottom blowing mode is selected with a large flow rate model (flow rate 5.5-6.5L / t.min), and the lower gate valve of the scrap steel hopper is opened to add the same scrap steel as the smelting steel into the ladle;
[0040] 7) After steel is tapped, the ladle is opened to the argon blowing position for argon blowing or refining, which can reduce the blowing loss of iron, manganese, vanadium and other elements in the scrap steel during the converter smelting process and maximize resource benefits.
[0041] The scrap steel structure model of the present invention, which is based on the precise control of the total amount of FeO in the raw material entering the converter, is based on determining the amount of FeO-containing coolant added according to the parameters of the molten iron entering the furnace, calculating the amount of FeO required to be supplemented according to the FeO brought by the coolant and the FeO demand value of the converter smelting, and then calculating the amount of crushed scrap steel added under different molten iron conditions according to the FeO content in the crushed scrap steel. When adding scrap steel according to this model, the FeO demand in the converter smelting process is balanced, and there will be no situation where the scrap steel is oxidized in large quantities due to insufficient FeO in the furnace during the smelting process. It can also effectively avoid the problems of strong oxidation of the terminal slag produced by excessive FeO in the furnace due to excessive addition of crushed scrap steel, low alloy recovery rate, etc. (as shown in the following table).
[0042] Scrap steel structure model based on precise control of the total amount of FeO in the converter (150-ton converter)
[0043]
[0044]
[0045] The details are as follows:
[0046] Example 1 Control of reducing scrap steel blowing loss in steelmaking process of 150t converter (steel output 150t)
[0047] A method for reducing scrap steel blowing loss in a converter steelmaking process, the method comprising the following steps:
[0048] 1) Install a scrap steel loading bucket above the steel tapping area behind the converter, open a chute connected to the top of the ladle, and install a gate valve between the chute and the loading bucket;
[0049] 2) Scrap steel is classified and stored according to type and size. Recycled scrap steel is stored separately, and surface-free scrap steel with a size of ≤300mm is stored according to the major types of steel.
[0050] 3) This furnace smelts HRB400E-1, with a total loading of 159t, 129t of molten iron, and 30t of scrap steel. When loading the converter scrap steel, 1.5t of HRE400E series scrap steel with a block size of ≤300mm is loaded into the scrap steel loading bucket installed above the steel tapping position, and the remaining 28.5t of scrap steel is loaded into the scrap steel bucket and added to the converter furnace, of which the amount of crushed scrap steel is 20t;
[0051] 4) The final temperature of the converter is 1659℃ (normal tapping temperature is 1650℃), the composition meets the standard, and the steel is tapped directly;
[0052] 5) After the alloy is added during the steel-making process, the ladle bottom blowing mode is selected to the large flow model (flow rate 5.5-6.5L / t.min), and the lower gate valve of the scrap steel hopper is opened to add 1.5t of scrap steel into the ladle;
[0053] 6) After steel is tapped, open the ladle to the argon blowing position for argon blowing or refining.
[0054] 7) The casting of this furnace is normal, and the amount of ingot cast is 150.15t.
[0055] Example 2 Control of reducing scrap steel blowing loss in steelmaking process of 150t converter (steel output 150t)
[0056] A method for reducing scrap steel blowing loss in a converter steelmaking process, the method comprising the following steps:
[0057] 1) Install a scrap steel loading bucket above the steel tapping area behind the converter, open a chute connected to the top of the ladle, and install a gate valve between the chute and the loading bucket;
[0058] 2) Scrap steel is classified and stored according to type and size. Recycled scrap steel is stored separately, and surface-free scrap steel with a size of ≤300mm is stored according to the major types of steel.
[0059] 3) This furnace smelts HRB400E-1, with a total loading of 159t, 141t of molten iron, and 18t of scrap steel. When loading the converter scrap steel, 1.5t of HRE400E series scrap steel with a block size of ≤300mm is loaded into the scrap steel loading bucket installed above the steel tapping position, and the remaining 16.5t of scrap steel is loaded into the scrap steel bucket and added to the converter furnace, of which the amount of crushed scrap steel is 8t;
[0060] 4) The final temperature of the converter is 1660℃ (normal tapping temperature is 1650℃), the composition meets the standard, and the steel is tapped directly;
[0061] 5) After the alloy is added during the steel-making process, the ladle bottom blowing mode is selected to the large flow model (flow rate 5.5-6.5L / t.min), and the lower gate valve of the scrap steel hopper is opened to add 1.5t of scrap steel into the ladle;
[0062] 6) After steel is tapped, open the ladle to the argon blowing position for argon blowing or refining.
[0063] 7) The casting of this furnace is normal, and the amount of ingot cast is 150.75t.
[0064] Comparative Example 1 Scrap Blowing Loss Control in Steelmaking Process of 150t Converter (Steel Output 150t)
[0065] 1) The steel grade of this converter is HRB400E-1, with a total loading of 159t, 129t of molten iron, 30t of scrap steel, of which 15t is crushed scrap steel;
[0066] 2) The final temperature of the converter is 1650℃, the composition meets the standard, and the steel is tapped directly;
[0067] 3) After steel is tapped, open the ladle to the argon blowing position for argon blowing or refining.
[0068] 4) The casting of this furnace is normal, and the amount of ingot cast is 150.25t.
[0069] Comparative Example 2 Scrap Blowing Loss Control in Steelmaking Process of 150t Converter (Steel Output 150t)
[0070] 1) The steel grade of this converter is HRB400E-1, with a total loading of 159t, 141t of molten iron, 18t of scrap steel, of which 9t is crushed scrap steel;
[0071] 2) The final temperature of the converter is 1650℃, the composition meets the standard, and the steel is tapped directly;
[0072] 3) After steel is tapped, open the ladle to the argon blowing position for argon blowing or refining.
[0073] 4) The casting of this furnace is normal, and the amount of ingot cast is 150.55t.
[0074] The casting amount, alloy amount, oxygen consumption and output efficiency of the embodiment and the comparative example are compared, and the results are shown in Table 1.
[0075] Table 1 Comparison of ingot amount, alloy amount, oxygen consumption and output efficiency
[0076]
[0077] By comparing the implementation cases with the comparative cases, the implementation cases can achieve a balance between the supply and demand of FeO in the converter smelting process by dynamically allocating the amount of crushed scrap steel in the scrap steel according to the situation of the molten iron entering the furnace, thereby preventing the occurrence of a large amount of scrap steel being oxidized due to insufficient FeO content in the furnace, and effectively preventing problems such as excessive FeO in the furnace, strong oxidizing property of the final slag, and low alloy recovery rate caused by excessive addition of crushed scrap steel. By installing a scrap steel charging bucket above the steel tapping site, the timing of adding scrap steel of the same type as the smelting steel is adjusted from adding it in the furnace to adding it into the ladle during the steel tapping process. While reducing the scrap steel blowing loss, the amount of alloy added is reduced. The implementation cases can reduce the oxidation amount of elements such as iron, manganese and vanadium in the scrap steel during the smelting process, effectively reducing production costs.
[0078] Any contents not described in detail in the present invention can be based on the conventional technical knowledge in the art.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the embodiments, it should be understood by those skilled in the art that any modification or equivalent replacement of the technical solutions of the present invention does not depart from the spirit and scope of the technical solutions of the present invention and should be included in the scope of the claims of the present invention.
Claims
1. A method for reducing scrap steel blowing loss in a converter steelmaking process, the method comprising the following steps: 1) Install a scrap steel loading bucket above the steel tapping area behind the converter, open a chute connected to the top of the ladle, and install a gate valve between the chute and the loading bucket; 2) Scrap steel is stored and added according to its type and size, where scrap steel includes recycled crushed scrap steel and / or surface non-oxidized scrap steel with a size of ≤300mm; 3) When loading the converter scrap steel, load the same scrap steel of the same type of steel smelted in the converter into the scrap steel loading bucket installed above the steel tapping area; 4) The scrap steel recycled from the society in the scrap steel added to the converter is dynamically added according to the scrap steel structure model based on the precise control of the total amount of FeO raw materials entering the converter, and the total amount of scrap steel added to the converter remains unchanged; The scrap steel structure model based on the precise control of the total amount of FeO in the converter raw material is a scrap steel structure model that determines the amount of scrap steel with a high FeO ratio according to the total charge of the furnace, the molten iron charge and the amount of FeO coolant added; the scrap steel structure model is based on the FeO demand in the converter furnace during smelting under different molten iron consumption and the amount of FeO added by the FeO-containing coolant during the smelting process, and calculates the demand for crushed scrap steel recycled by the society. The formula for calculating the demand for crushed scrap steel recycled by the society is: 5) After the alloy is added during the steel-making process, the ladle bottom blowing mode is selected with a large flow rate, and the lower gate valve of the scrap steel hopper is opened to add the same scrap steel as the smelting steel into the ladle; 6) After steel is tapped, open the ladle to the argon blowing position for argon blowing or refining.
2. The method for reducing scrap steel blowing loss in converter steelmaking process according to claim 1, characterized in that: In the step 2), the crushed scrap steel recovered from the society is stored separately, and the surface non-oxidized scrap steel with a size of ≤300 mm is stored according to the major types of steel.
3. The method for reducing scrap steel blowing loss in converter steelmaking process according to claim 2, characterized in that: The crushed scrap steel recycled by the society is bulk material or bulk material briquettes with a maximum side length of ≤200mm, and the scrap steel has severe surface oxidation, with an oxide ratio of 12±2%.
4. The method for reducing scrap steel blowing loss in converter steelmaking process according to claim 2, characterized in that: Surface non-oxidized scrap steel with a size of ≤300mm is classified into major steel types, which are the common alloy element content of steel type ±0.10% and the trace element content ±0.010%.
5. The method for reducing scrap steel blowing loss in converter steelmaking process according to claim 1, characterized in that: In the step 3), the amount of similar scrap steel is controlled according to the steel output of 10±2kg / t, and the amount of scrap steel added to the converter furnace is reduced by 10±2kg / t accordingly.
6. The method for reducing scrap steel blowing in converter steelmaking process according to claim 1, characterized in that: The method further comprises: controlling the converter end temperature to be 10±2° C. higher than the normal temperature.
7. The method for reducing scrap steel blowing in converter steelmaking process according to claim 1, characterized in that: The bottom blowing flow rate in step 5) is 5.5 to 6.5 L / t·min.