Diamond / copper composite material and preparation method thereof

By treating the diamond surface with the thermal diffusion method and compounding it with copper using SPS technology, the problem of the interface between diamond and copper is solved, the thermal conductivity and thermal expansion coefficient of the diamond/copper composite material are significantly improved, and the demand for high-end electronic packaging materials is met.

CN115821097BActive Publication Date: 2024-10-11ANHUI SHANGXINJINGGONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211523322.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-01
Publication Date
2024-10-11
Estimated Expiration
2042-12-01

AI Technical Summary

Technical Problem

The poor wettability and inability of direct connection between diamond and copper lead to a reduction in the thermal conductivity of diamond/copper composites, making it difficult to meet the requirements for high thermal conductivity and low thermal expansion coefficient.

Method used

Thermal diffusion method is used to treat the diamond surface to form a metal or non-metal coating layer, and is compounded with copper through SPS technology to improve the interface bonding.

Benefits of technology

The thermal conductivity of the diamond/copper composite material is significantly improved and its thermal expansion coefficient is close to that of the chip, achieving efficient heat dissipation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003974299730000011
    Figure HDA0003974299730000011
  • Figure HDA0003974299730000012
    Figure HDA0003974299730000012
  • Figure HDA0003974299730000013
    Figure HDA0003974299730000013
Patent Text Reader

Abstract

The present invention discloses a method for preparing a diamond / copper composite material, wherein the diamond / copper composite material prepared thereby comprises a chip packaging material of the material. The method comprises the following steps: 1) placing diamond powder and powder of a heat diffusion material into a V-type powder mixer for mechanical mixing; 2) placing the mixed powder obtained in step 1 into a crucible, and performing heat diffusion treatment in a vacuum furnace; 3) separating the mixed material after the heat diffusion treatment in step 2 to obtain diamond coated with the heat diffusion material; 4) mixing the diamond coated with the heat diffusion material with copper powder evenly, and sintering and forming by SPS technology. The method according to the present invention is simple and fast, and the obtained diamond / copper composite material has high thermal conductivity and high density, and the thermal expansion coefficient is similar to that of the chip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a diamond / copper composite material, specifically a method of first treating the surface of diamond by a thermal diffusion method to form a metal or non-metal coating layer on the surface of diamond particles, and then using SPS technology to prepare the coating layer diamond / copper composite material. Background Art

[0002] With the continuous development of information technology, the power of electronic equipment used in many high-tech fields such as military industry, electronics industry, new energy, aerospace, etc. is getting higher and higher, and the heat generation is getting higher and higher. The heat dissipation problem has become a bottleneck restricting the development of these industries. In the design of high-performance electronic packaging materials, higher and higher requirements are put forward for the thermal conductivity, density, thermal expansion coefficient and other properties of core chip heat dissipation materials. The thermal conductivity of high-quality diamond is very high, which can reach 2000W / (m·K), and it is an insulator at room temperature. It also has the characteristics of low dielectric constant and low thermal expansion coefficient. However, single diamond is not easy to make packaging materials, and the cost is very high. It is more ideal to make it into a metal-based composite material. Among them, the thermal conductivity of copper is 390W / (m·K), which is the second highest metal after silver. Therefore, diamond / copper composite materials are the most promising to become the next generation of high-end electronic packaging materials.

[0003] The difficulties in preparing diamond / copper composite materials are: (1) Diamond and copper have poor wettability, with a wetting angle of 138° at 1150°C; (2) Diamond and copper will not undergo phase change at high temperatures, carbon has no solid solubility in copper, and diamond and copper cannot be directly connected. Directly compounding diamond and copper will reduce the thermal conductivity of the composite material to 276W / (m·K). Therefore, it is urgent to develop a diamond / copper composite material with high thermal conductivity and a thermal expansion coefficient similar to that of the chip, so as to promote the replacement of electronic packaging materials. Summary of the invention

[0004] The present invention aims at the preparation of diamond / copper high thermal conductivity composite materials, and proposes a method for treating the surface of diamond by using a thermal diffusion method to improve the interface bonding problem between diamond and copper. The treated diamond and copper are used to prepare a composite material by spark plasma sintering technology. The results show that the thermal conductivity of the composite material is greatly improved, indicating that this method can significantly improve the interface bonding between diamond and copper. In addition, the thermal expansion coefficient of the composite material according to the present invention is similar to the thermal expansion coefficient of the chip (6x10 -6 / K) is very close.

[0005] The method for preparing the diamond / copper high thermal conductivity composite material of the present invention is: firstly, using a vacuum furnace to perform heat diffusion treatment on the surface of diamond with powders of heat diffusion materials (tungsten, chromium, titanium, niobium, vanadium, boron, molybdenum, tantalum), the heat-treated diamond particles are cleaned and dried, and then mixed evenly with copper powder, and then sintered by SPS technology to obtain a diamond / copper composite material with high thermal conductivity and high density.

[0006] Therefore, according to a first aspect of the present invention, there is provided a method for preparing a diamond / copper composite material, comprising the following steps:

[0007] Step 1: Put the diamond powder and the powder of the thermal diffusion material into a V-type powder mixer and mix them mechanically evenly;

[0008] Step 2: The mixed powder obtained in step 1 is placed in a crucible and subjected to thermal diffusion treatment in a vacuum furnace, wherein the thermal diffusion conditions are as follows:

[0009] Vacuum degree: below 20Pa;

[0010] Heating rate: 20~30℃ / min

[0011] Insulation temperature: 800~1050℃;

[0012] Insulation time: 0.5 to 2.5 hours, preferably 1.0 to 2.0 hours;

[0013] Cooling rate: cooling with the furnace;

[0014] Step 3: Separating the mixture after the thermal diffusion treatment obtained in step 2 to obtain diamonds coated with thermal diffusion materials;

[0015] Step 4: After the diamond coated with the heat diffusion material is evenly mixed with the copper powder, the diamond / copper composite material is obtained by sintering using the SPS technology.

[0016] Preferably, the diamond powder has a particle size of 50 to 600 μm.

[0017] Preferably, the heat diffusion material is one or more selected from tungsten, chromium, titanium, niobium, vanadium, boron, molybdenum and tantalum.

[0018] Preferably, the particle size of the thermal diffusion material powder is 2-50 μm.

[0019] Preferably, in step 1, the volume ratio of diamond to thermal diffusion material powder is 1:1, and the mechanical mixing time in the V-type powder mixer is 2 to 24 hours, preferably, the mechanical mixing time is 5 to 12 hours.

[0020] Preferably, in step 3, the method for separating the mixture after the thermal diffusion treatment is to first coarsely screen the powder with a mesh screen, and then wash it multiple times with an ultrasonic cleaning machine until it is clarified.

[0021] Preferably, the conditions for sintering the mixed powder using SPS technology in step 5 are:

[0022] The temperature is 700-950°C, preferably 800-900°C,

[0023] The holding time is 0 to 10 minutes, and the furnace is cooled after the holding is completed.

[0024] During the sintering process, the pressure remains constant at 10 to 30 MPa.

[0025] Preferably, in the diamond / copper composite material, the volume ratio of diamond is 20% to 70%, preferably, the volume ratio of diamond is 40% to 65%, and more preferably 60%.

[0026] According to a second aspect of the present invention, there is provided a diamond / copper high thermal conductivity composite material obtained according to the method for preparing a diamond / copper high thermal conductivity composite material according to the present invention.

[0027] Preferably, the density of the diamond / copper high thermal conductivity composite material is above 99.0%.

[0028] Preferably, the thermal expansion coefficient of the diamond / copper high thermal conductivity composite material is 7.00x10 -6 ~10.00x10 -6 / K, more preferably 8.00x10 -6 ~9.00x10 -6 / K.

[0029] Preferably, the thermal conductivity of the diamond / copper high thermal conductivity composite material is 400-700 W / (m·K), preferably 430-650 W / (m·K).

[0030] Preferably, in the diamond / copper composite material, the volume ratio of diamond is 20% to 70%, preferably, the volume ratio of diamond is 40% to 65%, and more preferably 60%.

[0031] According to a third aspect of the present invention, there is provided a chip packaging material, which comprises the diamond / copper high thermal conductivity composite material according to the present invention.

[0032] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0033] (1) The present invention uses a thermal diffusion method to wet the surface of diamond. Compared with other coating methods including PVD, CVD, vacuum micro-plating, chemical plating, and salt bath plating, the present invention has the characteristics of good diamond surface modification quality, obvious effect, easy control of process parameters, strong operability, and mass production.

[0034] (2) The coated diamond obtained by the present invention has a high-strength, uniform and dense coating layer, which helps to obtain a dense diamond / copper composite material with high thermal conductivity.

[0035] (3) The present invention prepared diamonds coated with different materials including tungsten, chromium, titanium, niobium, vanadium, boron, molybdenum, and tantalum on the surface, and tested the thermal conductivity of diamond / copper composites with different coating layers. Diamond / copper composites with a diamond volume fraction of 20%-70% were successfully prepared. Spark plasma sintering was used for sintering, and the sintering process was simple and fast, and the resulting composite material had excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1a and Figure 1b The following are the actual photos of the untreated diamond powder according to Example 1 and the tungsten-coated diamond obtained through step 3);

[0037] Figure 2 is a SEM image of the tungsten-coated diamond obtained through step 4) of Example 1. DETAILED DESCRIPTION

[0038] The present invention is further described below by way of examples, but the embodiments of the present invention are not limited thereto.

[0039] The spark plasma sintering system used in the following embodiments is from SINTER LAND Co., Ltd. of Japan, and the models are LABOX-350 and LABOX-6020. It should be noted that the sintering of diamond / copper composite block using the method of the present invention and equipment of other manufacturers and models is also within the scope of the present invention. Spark plasma sintering includes pulse power-on pressure sintering, electric field assisted sintering, pulse current rapid sintering, etc.

[0040] The inner diameter of the sintered graphite mold used in the following examples is Φ13 mm, and the thermal conductivity of the composite material is tested using an LFA-467 laser thermal conductivity meter, and the thermal expansion coefficient of the material is measured using a DIL402C thermal expansion meter. The diamond powder used is from Zhengzhou Abrasives and Grinding Research Institute Co., Ltd., with a particle size of 200 μm; the copper powder is purchased from Sinopharm Group, with a particle size of 35 μm; other metal or non-metal powders are purchased from Sinopharm Group, with a particle size of no more than 10 μm.

[0041] Example 1

[0042] The diamond / copper composites were prepared by the following steps:

[0043] Step 1: Mix diamond powder and tungsten powder in a V-type powder mixer at a volume ratio of 1:1 for 6 hours.

[0044] Step 2: put the powder obtained in step 1 into a crucible, heat it to 1000°C in a vacuum furnace and keep it warm for 2 hours, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0045] Step 3: The mixture after the thermal diffusion treatment in step 2 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain tungsten-coated diamond.

[0046] Step 4: Weigh 0.98 g of tungsten-coated diamond and 1.65 g of copper powder with a particle size of 35 μm, mix the tungsten-coated diamond and the copper powder evenly, and then use SPS to rapidly heat and sinter to obtain a diamond / copper composite material.

[0047] The sintering temperature is 850℃, the holding time is 5min, the sintering pressure is 30MPa, and the furnace is cooled after the holding time. The relative density of the obtained sample is >99.0%, the thermal conductivity is 600W / (m·K), and the thermal expansion coefficient is 8.63x10 -6 / K.

[0048] Example 2

[0049] The diamond / copper composite material was prepared as follows:

[0050] Step 1: Mix diamond powder and chromium powder in a V-type mixer at a volume ratio of 1:1 for 12 hours.

[0051] Step 2: put the powder obtained in step 1 into a crucible, heat it to 900°C in a vacuum furnace and keep it warm for 1.5 hours, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0052] Step 3: The mixture after the thermal diffusion treatment in step 2 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain chromium-coated diamond particles.

[0053] Step 4: Weigh 0.98 g of chromium-coated diamond and 1.65 g of copper powder, mix the chromium-coated diamond and copper powder evenly, and then use SPS to rapidly heat and sinter to obtain a diamond / copper composite material.

[0054] The sintering temperature is 900℃, the holding time is 3min, the sintering pressure is 25MPa, and the furnace is cooled after the holding time. The obtained sample has a relative density of >99.0%, a thermal conductivity of 530W / (m·K), and a thermal expansion coefficient of 8.34x10 -6 / K.

[0055] Example 3

[0056] The diamond / copper composite material was prepared as follows:

[0057] Step 1: Mix diamond powder and vanadium powder in a V-type powder mixer at a volume ratio of 1:1 for 12 hours.

[0058] Step 2: put the powder obtained in step 1 into a crucible, heat it to 950°C in a vacuum furnace and keep it warm for 1 hour, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0059] Step 3: The mixture after the thermal diffusion treatment in step 2 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain vanadium-coated diamond.

[0060] Step 4: Weigh 0.98 g of vanadium-coated diamond and 1.65 g of copper powder, mix the vanadium-coated diamond and copper powder evenly, and then use SPS to rapidly heat and sinter to obtain a diamond / copper composite material.

[0061] The sintering temperature is 900℃, the holding time is 3min, the sintering pressure is 25MPa, and the furnace is cooled after the holding time. The relative density of the obtained sample is >99.0%, the thermal conductivity is 650W / (m·K), and the thermal expansion coefficient is 8.29x10 -6 / K.

[0062] Example 4

[0063] The diamond / copper composite material was prepared as follows:

[0064] Step 1: Mix diamond powder and molybdenum powder in a V-type mixer at a volume ratio of 1:1 for 12 hours.

[0065] Step 2: put the powder obtained in step 1 into a crucible, heat it to 1050°C in a vacuum furnace and keep it warm for 1.5 hours, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0066] Step 3: The mixture after the thermal diffusion treatment in step 2 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain molybdenum-coated diamonds.

[0067] Step 4: Weigh 0.98 g of molybdenum-coated diamond and 1.65 g of copper powder, mix the molybdenum-coated diamond and copper powder evenly, and then use SPS to rapidly heat and sinter to obtain a diamond / copper composite material.

[0068] The sintering temperature is 900℃, the holding time is 3min, the sintering pressure is 25MPa, and the furnace is cooled after the holding time is over. The obtained sample has a relative density of >99.0%, a thermal conductivity of 500W / (m·K), and a thermal expansion coefficient of 8.67x10 -6 / K.

[0069] Example 5

[0070] The diamond / copper composite material was prepared as follows:

[0071] Step 1: Mix diamond powder and boron powder in a V-type powder mixer at a volume ratio of 1:1 for 12 hours.

[0072] Step 2: put the powder obtained in step 1 into a crucible, heat it to 1050°C in a vacuum furnace and keep it warm for 2 hours, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0073] Step 3: The mixture after the thermal diffusion treatment in step 2 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain boron-coated diamond.

[0074] Step 4: Weigh 0.98 g of boron-coated diamond and 1.65 g of copper powder, mix the boron-coated diamond and copper powder evenly, and then use SPS to rapidly heat and sinter to obtain a diamond / copper composite material.

[0075] The sintering temperature is 900℃, the holding time is 3min, the sintering pressure is 25MPa, and the furnace is cooled after the holding time. The obtained sample has a relative density of >99.0%, a thermal conductivity of 580W / (m·K), and a thermal expansion coefficient of 8.77x10 -6 / K.

[0076] Example 6

[0077] The diamond / copper composite material was prepared as follows:

[0078] Step 1: Mix diamond powder and niobium powder in a V-type powder mixer at a volume ratio of 1:1 for 12 hours.

[0079] Step 2: put the powder obtained in step 1 into a crucible, heat it to 1000°C in a vacuum furnace and keep it warm for 1 hour, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0080] Step 3: The mixture after the thermal diffusion treatment in step 3 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain niobium-coated diamond.

[0081] Step 4: Weigh 0.98 g of niobium-coated diamond and 1.65 g of copper powder, mix the niobium-coated diamond and copper powder evenly, and then sinter them by rapid heating using SPS to obtain a diamond / copper composite material.

[0082] The sintering temperature is 900℃, the holding time is 3min, the sintering pressure is 25MPa, and the furnace is cooled after the holding time. The obtained sample has a relative density of >99.0%, a thermal conductivity of 550W / (m·K), and a thermal expansion coefficient of 8.49x10 -6 / K.

[0083] Example 7

[0084] The diamond / copper composite material was prepared as follows:

[0085] Step 1: Mix diamond powder and tantalum powder in a V-type powder mixer at a volume ratio of 1:1 for 12 hours.

[0086] Step 2: The powder obtained in step 2 is placed in a crucible, and heated to 1050°C in a vacuum furnace and kept warm for 1.5 hours, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0087] Step 3: The mixture after the thermal diffusion treatment in step 2 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain tantalum-coated diamond.

[0088] Step 4: Weigh 0.98 g of tantalum-coated diamond and 1.65 g of copper powder, mix the tantalum-coated diamond and copper powder evenly, and then use SPS to rapidly heat and sinter to obtain a diamond / copper composite material.

[0089] The sintering temperature is 900℃, the holding time is 3min, the sintering pressure is 25MPa, and the furnace is cooled after the holding time. The obtained sample has a relative density of >99.0%, a thermal conductivity of 480W / (m·K), and a thermal expansion coefficient of 8.56x10 -6 / K.

[0090] Example 8

[0091] The diamond / copper composite material was prepared as follows:

[0092] Step 1: Mix diamond and titanium powder in a V-type mixer at a volume ratio of 1:1 for 12 hours.

[0093] Step 2: put the powder obtained in step 1 into a crucible, heat it to 850°C in a vacuum furnace and keep it warm for 0.5h, wherein the heating rate is 25°C / min, the vacuum degree is below 20Pa, and the cooling rate is cooling with the furnace;

[0094] Step 3: The mixture after the thermal diffusion treatment in step 2 is first coarsely sieved with a mesh screen, and then cleaned with an ultrasonic cleaning machine for multiple times until it is clarified to obtain titanium-coated diamond.

[0095] Step 4: Weigh 0.98 g of titanium-coated diamond and 1.65 g of copper powder, mix the titanium-coated diamond and copper powder evenly, and then use SPS to rapidly heat and sinter to obtain a diamond / copper composite material.

[0096] The sintering temperature is 900℃, the holding time is 3min, the sintering pressure is 25MPa, and the furnace is cooled after the holding time. The obtained sample has a relative density of >99.0%, a thermal conductivity of 430W / (m·K), and a thermal expansion coefficient of 8.87x10 -6 / K.

[0097] Comparative Example 1

[0098] The diamond / copper composite material was prepared in the same manner as in Example 1, except that the vacuum furnace in step 2 was heated to 1100° C., kept at this temperature for 4 hours, and the heating rate was 25° C. / min.

[0099] The relative density of the sample was 98.9%, the thermal conductivity was 527 W / (m·K), and the thermal expansion coefficient was 9.3x10 -6 / K.

[0100] Comparative Example 2

[0101] The diamond / copper composite material was prepared in the same manner as in Example 2, except that the vacuum furnace in step 2 was heated to 1100° C., kept at this temperature for 4 hours, and the heating rate was 25° C. / min.

[0102] The relative density of the sample was 99.2%, the thermal conductivity was 463 W / (m·K), and the thermal expansion coefficient was 8.79x10 -6 / K.

[0103] Comparing Examples 1 to 8 with Comparative Examples 1 and 2, it can be seen that the diamond / copper composite material prepared according to the method of the present invention has significantly improved thermal conductivity and a lower thermal expansion coefficient. One possible reason is that the method according to the present invention inhibits the graphitization of diamond. Diamond will graphitize at 850°C under normal pressure, losing its own advantage of high thermal conductivity. Low vacuum can inhibit the graphitization of diamond, but graphitization will also occur at 1000°C. In the present invention, the thermal diffusion temperature is close to or lower than the graphitization temperature of diamond, and the thermal diffusion insulation time is short, which makes the coating thickness of the diamond coated with the prepared thermal diffusion material thin and the degree of graphitization of the diamond surface is small, which leads to higher thermal conductivity of the prepared diamond / copper composite material.

Claims

1. A method for preparing a diamond / copper composite material, comprising the following steps: Step 1: Put diamond powder and powder of thermal diffusion material into a V-type powder mixer for mechanical mixing, wherein the thermal diffusion material is one or more selected from tungsten, chromium, titanium, niobium, vanadium, boron, molybdenum and tantalum; Step 2: The mixed powder obtained in step 1 is placed in a crucible and subjected to thermal diffusion treatment in a vacuum furnace, wherein: The thermal diffusion conditions are as follows: Vacuum degree: below 20Pa; Heating rate: 20~30℃ / min Insulation temperature: 800~1050℃; Insulation time: 0.5~2.5h; Cooling rate: cooling with the furnace; Step 3: Separating the mixture after the thermal diffusion treatment obtained in step 2 to obtain diamonds coated with the thermal diffusion material, wherein the method for separating the mixture after the thermal diffusion treatment is to first coarsely sieve the powder with a mesh screen, and then wash it with an ultrasonic cleaning machine for multiple times until it is clear; Step 4: After the diamond coated with the thermal diffusion material is evenly mixed with copper powder, the diamond / copper composite material is obtained by sintering using SPS technology; Among them, the conditions for sintering the mixed powder using SPS technology are: The temperature is 700~950℃, The holding time is 0 to 10 minutes, and the furnace is cooled after the holding is completed. During the sintering process, the pressure remains constant at 10 to 30 MPa.

2. The method for preparing a diamond / copper composite material according to claim 1, wherein: The holding time in step 2) is 1.0 to 2.0 h.

3. The method for preparing a diamond / copper composite material according to claim 1, wherein: The sintering temperature in step 4) is 800-900°C.

4. The method for preparing a diamond / copper composite material according to claim 1, wherein: The diamond powder particle size is 50 to 600 μm; The particle size of the thermal diffusion material powder is 2 to 50 μm.

5. The method for preparing a diamond / copper composite material according to claim 1, wherein: In step 1, the volume ratio of diamond to the thermal diffusion material powder is 1:1, and the mechanical mixing time in the V-type powder mixer is 2 to 24 hours.

6. The method for preparing a diamond / copper composite material according to claim 1, wherein: In step 1), the mechanical mixing time is 5 to 12 hours.

7. The method for preparing a diamond / copper composite material according to any one of claims 1 to 6, wherein: In the diamond / copper composite material, the volume ratio of diamond is 20% to 70%.

8. The method for preparing a diamond / copper composite material according to claim 7, wherein: In the diamond / copper composite material, the volume ratio of diamond is 40% to 65%.

9. A diamond / copper high thermal conductivity composite material obtained by the method for preparing a diamond / copper high thermal conductivity composite material according to any one of claims 1 to 8.

10. The diamond / copper high thermal conductivity composite material according to claim 9, wherein: The density of the diamond / copper high thermal conductivity composite material is above 99.0%.

11. The diamond / copper high thermal conductivity composite material according to claim 9, wherein: The thermal expansion coefficient of the diamond / copper high thermal conductivity composite material is 7.00x10 -6 ~10.00x10 -6 / K.

12. The diamond / copper high thermal conductivity composite material according to claim 9, wherein: The thermal expansion coefficient of the diamond / copper high thermal conductivity composite material is 8.00x10 -6 ~9.00x10 -6 / K.

13. The diamond / copper high thermal conductivity composite material according to any one of claims 9 to 12, wherein: The thermal conductivity of the diamond / copper high thermal conductivity composite material is 400-700 W / (m·K).

14. The diamond / copper high thermal conductivity composite material according to claim 13, wherein: The thermal conductivity of the diamond / copper high thermal conductivity composite material is 430-650 W / (m·K). 15 . A chip packaging material comprising the diamond / copper high thermal conductivity composite material according to any one of claims 9 to 14.