A method for resisting impact erosion of a bucket of an ultra-high head impulse turbine
By using semi-elastic contact connected carbide bushings and supersonic flame thermal spraying technology on the ultra-high head impact turbine water bucket, the problem of water bucket abrasion under strong impact is solved, and the wear resistance and lifespan are significantly improved.
Patent Information
- Application Number
- CN202211572235.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-08
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-12-08
AI Technical Summary
The ultra-high head impact turbine bucket is prone to abrasion and coating peeling under the strong impact of sediment flow. It is difficult for the existing coating to effectively protect in this environment.
The cemented carbide bushing with semi-elastic contact connection is fixed on the inner wall of the water bucket, and the supersonic flame thermal spraying technology is used to prepare the cemented carbide protective coating on the surface of the outer wall and fasteners, combined with a specific formula of cemented carbide materials to improve Anti-wear properties.
The service life of the water bucket is significantly extended, and the resistance to sediment abrasion is increased by 3 to 5 times. Compared with traditional methods, the life of the water bucket is extended from half a year to one year to more than 5 years.
Smart Images

Figure CN115837467B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of water conservancy surface technology and engineering, and in particular to a method for resisting impact and abrasion of a bucket of an ultra-high water head impulse turbine. Background Art
[0002] With the continuous advancement of technology, the application of impulse turbines in high-head hydropower stations has become more and more extensive. However, the bucket life of impulse turbines is still short, especially in some hydropower stations with ultra-high head of more than one thousand meters, the bucket is eroded very badly. According to investigations, engineers have improved the erosion and wear of impulse turbines and extended the life of turbines by preparing highly wear-resistant metal ceramic coatings or polyurethane coatings on the surface of the buckets. However, according to actual feedback from use, the effect of the above coatings is limited. Because in the case of ultra-high head, the impact force from the nozzle to the bucket is very huge, and the silt in the water will cause a very large impact and plowing effect on the inner wall of the bucket. The commonly used WC series cemented carbide coating is generally prepared by supersonic flame spraying. The coating thickness prepared by this method is not too thick, usually in the range of 200~400 microns, and it has a good anti-wear and anti-corrosion effect when used in mixed flow turbines, axial flow propeller turbines and some low-head impulse turbines. However, when applied to ultra-high head impulse turbines, especially on the inner wall of the bucket, the thin and brittle metal ceramic coating will be easily broken by the impact and fall off from the substrate. The polyurethane coating has good elasticity and is very good at resisting vertical impact of sand particles, but its ability to resist sand cutting is weak, and because of its low bonding strength with the substrate, it is easy to peel off due to strong force. Therefore, there is an urgent need for an effective solution to the impact and abrasion resistance problem of the bucket of the impulse turbine with ultra-high head of more than one kilometer. Summary of the invention
[0003] The present invention aims to solve the corrosion and wear resistance problem of the bucket of an ultra-high head impulse turbine and provides an impact and abrasion resistance method for the bucket of an ultra-high head impulse turbine. Because the inner wall of the bucket is directly and strongly impacted by the sediment and water flow, the present invention uses a hard alloy bushing fixed to the inner wall of the bucket in a specific way to protect it. In addition, a hard alloy protective coating is prepared on the outer wall of the bucket and the surface of the fastener by using supersonic flame thermal spraying technology.
[0004] The technical solution adopted by the present invention is:
[0005] A method for resisting impact erosion of a bucket of an ultra-high head impulse turbine comprises fixing a set of carbide bushings on the entire surface of the inner wall of the bucket by a semi-elastic contact connection method, wherein the carbide bushings and the bucket are bonded by structural adhesive to absorb and buffer different elastic micro-deformations between the bushings and the bucket, and the edges of the carbide bushings are pressed against the bucket by fasteners to prevent the carbide bushings from moving.
[0006] Furthermore, a hard alloy protective coating is prepared on the outer wall of the water bucket and the surface of the fastener using supersonic flame thermal spraying technology.
[0007] The manufacturing technology of the cemented carbide bushing selects vacuum sintering technology to obtain the characteristics of high density, low impurities and high strength. The cemented carbide mixed powder is first pressed under high pressure to form a blank of suitable size in the shape of the inner wall of the bucket, ensuring that after vacuum sintering, the size of the cemented carbide bushing matches the size of the turbine bucket. Then the vacuum sintering process is carried out, including the following three processes: pre-burning stage, high temperature sintering stage, and cooling stage. In the pre-burning stage, when the vacuum degree is lower than 10Pa, the temperature begins to rise. When the appropriate temperature is reached, it is kept warm for a certain time to ensure that impurities are discharged. The temperature is generally in the range of 250℃~600℃, and the holding time is determined according to the amount of the forming agent. According to the size of the general impulse turbine bucket, the holding time can be in the range of 12h~24h. In the high temperature sintering stage, the temperature is selected in the range of 1300℃~1500℃, and the holding time is selected in the range of 2h~10h, which needs to be selected according to the material and size of the cemented carbide bushing. In the cooling stage, inert gas, such as argon, is introduced to accelerate cooling and also increase the density of the cemented carbide bushing.
[0008] Furthermore, the material of the cemented carbide bushing is a combination of WC-Co-inhibitor-wetting agent-rare earth, and the particle size of each component powder is ultra-fine, less than 1 micron. The composite formula combination is preferably: WC-Co-VC-TaC-La2O3, WC-Co-Cr2C3-TiC-Mo-CeO2, WC-Co-NbC-Cr-La2O3; this material formula makes the cemented carbide bushing have finer grains, higher strength, higher density, and higher toughness, which is very suitable for the working environment of the impulse turbine bucket.
[0009] Furthermore, the thickness of the cemented carbide bushing can be made very thick, much thicker than the cemented carbide coating prepared by supersonic flame thermal spraying, which is generally less than 0.4mm thick. Under strong scouring of mud and sand, the thin cemented carbide coating will easily peel off from the substrate due to the different deformation coefficients of the coating and the substrate, as well as the low bonding strength between the coating and the substrate (generally around 70Mpa). The thick high-strength cemented carbide bushing is more resistant to scouring and wear by mud and sand, and at the same time, because of the semi-elastic contact connection with the water bucket, it will not break due to the different deformation coefficients of the cemented carbide bushing material and the water bucket material. The semi-elastic contact connection method refers to the fact that the cemented carbide bushing and the water bucket are bonded by structural adhesive on the one hand, and the structural adhesive can absorb and buffer the different elastic micro-deformations between the two, preventing the cemented carbide bushing from cracking and breaking. On the other hand, the edge of the cemented carbide bushing is pressed by fasteners to further prevent the cemented carbide bushing from moving.
[0010] The fastener includes two parts, one part is a fixed part, which can be welded and fixed on the water bucket along the upper surface of the water bucket, and a through hole can be drilled in the middle; the other part is a movable part, and a threaded hole (not a through hole) can be drilled inside it. The two parts are fastened by fastening bolts and the carbide bushing is pressed on the water bucket.
[0011] Pelton turbine bucket protection process:
[0012] 1) Weld the fixing part of the fastener to the upper surface of the bucket of the impulse turbine;
[0013] 2) For the inner wall, outer wall and other surfaces of the impulse turbine, use a cleaning agent to clean the surface oil, and then use white corundum to sandblast the above surfaces. The surface roughness of the bucket after sandblasting reaches Ra10 or above.
[0014] 3) Use high-strength structural adhesive to coat the inner wall of the bucket. For example, high-strength acrylic structural adhesive can be used. It is resistant to acid, alkali, water, and oil corrosion, impact resistant, has a wide operating temperature range (-30~150℃), and a bonding strength of up to 70Mpa. It is very suitable for bonding between WC carbide bushings and steel buckets, and is also very suitable for the working environment of impulse turbine buckets.
[0015] 4) Place the carbide bushing close to the inner wall of the impulse turbine bucket, tighten the movable part of the fastener with bolts, and press the carbide bushing, waiting for curing for more than 24 hours.
[0016] 5) For other flow areas of the bucket that need to be subjected to supersonic flame thermal spraying of cemented carbide coating, WC-Co series cemented carbide coating is prepared by supersonic flame thermal spraying technology.
[0017] In addition, the present invention also provides an impulse turbine bucket that can operate under ultra-high water head, including a bucket body, a hard alloy bushing, and a fastener; the fastener includes a fixing part and a movable part; the hard alloy bushing covers the entire inner wall of the bucket body and is connected to the inner wall of the bucket by a structural adhesive, the fixing part is welded to the edge of the bucket body, the movable part presses the hard alloy bushing to the edge of the bucket and fastens it to the fixing part by bolts, and a hard alloy protective coating is prepared on other flow areas of the bucket and the surface of the fastener.
[0018] The beneficial effects of the present invention are:
[0019] The protection of the inner wall of the bucket adopts a hard alloy bushing instead of a coating. The thickness of the hard alloy bushing can be as thick as that of the coating. At the same time, the hard alloy bushing adopts a new formula. The two greatly enhance its impact and wear resistance, thereby greatly improving the service life of the inner wall of the bucket. At the same time, the areas of the bucket that are indirectly impacted by sediment are all prepared by supersonic flame thermal spraying technology. WC-Co series hard alloy coatings are greatly extended. The overall life of the impulse turbine bucket. Compared with the commonly used turbine 0Cr13Ni5Mo stainless steel, the commonly used WC-Co series hard alloy coating has an improved ability to resist sediment abrasion by 3 to 5 times. The hard alloy bushing method provided by the present invention has greatly improved the ability to resist sediment impact and abrasion on the inner wall of the bucket compared with the traditional supersonic flame thermal spraying WC-Co series hard alloy coating. The actual application effect: compared with the traditional method of spraying coatings on buckets, the service life of buckets is half a year to one year. The method provided by the present invention can achieve a service life of high-head impulse turbine buckets of more than 5 years. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the water bucket of the impulse turbine in the present invention.
[0021] In the figure: 1-carbide bushing, 2-buoy base, 3-movable part in the fastener, 4-fixed part in the fastener, 5-welding seam, 6-WC carbide coating. DETAILED DESCRIPTION
[0022] The following is further described with reference to the accompanying drawings and specific implementation cases.
[0023] Reference Figure 1 A schematic diagram showing a method for resisting impact erosion of the bucket of an ultra-high head Pelton turbine is shown.
[0024] Example 1
[0025] The composition of cemented carbide bushing 1: WC-Co-VC-TaC-La2O3, including Co 9%wt, particle size 0.5~1μm, VC 10%wt, particle size 0.5~1μm, TaC 7%wt, particle size 0.5~1μm, La2O31%wt, particle size 0.5~1μm, and the rest is WC with a particle size of 1~2μm.
[0026] The manufacturing technology of cemented carbide bushing 1 selects vacuum sintering technology to obtain the characteristics of high density, low impurities and high strength. The cemented carbide mixed powder is first pressed under high pressure to form a blank of suitable size in the shape of the inner wall of the bucket, ensuring that after vacuum sintering, the size of the cemented carbide bushing 1 matches the inner wall size of the turbine bucket matrix 2. Then the vacuum sintering process is carried out, including the following three processes: pre-burning stage, high-temperature sintering stage, and cooling stage. During the pre-burning stage, when the vacuum degree is lower than 1Pa, the temperature begins to rise. When it reaches 350℃, it is kept warm for 10 hours to ensure that impurities are discharged. During the high-temperature sintering stage, the temperature is kept warm at 1400℃ for 5 hours. During the cooling stage, argon gas is introduced at a pressure of 3MPa to accelerate cooling, and at the same time, the density of the cemented carbide bushing can be increased. The average thickness of the cemented carbide bushing is made into 5mm.
[0027] A through hole is drilled inside the fixing piece 4 in the fastener and welded to the upper surface outlet of the water bucket base 2. The position of the weld 5 can be selected at the welding connection, and multiple fasteners can be arranged around the upper plane of the water bucket.
[0028] A threaded hole which is not a through hole is drilled inside the movable part 3 in the fastener, one end of which is close to the carbide bushing 1, and the other end is fastened to the fixed part 4 in the fastener by a fastening bolt to press the carbide bushing 1.
[0029] The WC cemented carbide coating 6 can be prepared by HVOF (supersonic oxygen flame spraying) technology in the designated area: including the outer wall of the bucket substrate 2, the fixed part 4 in the fastener and the surface of the movable part 3 in the fastener. The spraying material can be selected from the WC-Co series cemented carbide coating powder formula that has been maturely applied in the market, such as WC-10Co-4Cr powder.
[0030] Pelton turbine bucket protection process:
[0031] 1. Weld the fixing member 4 in the fastener to the upper surface of the bucket base 2 of the impulse turbine;
[0032] 2. Use a cleaning agent to clean the oil stains on the inner wall, outer wall and other surfaces of the water bucket base 2, and then use white corundum to sandblast the above surfaces. The surface roughness of the water bucket after sandblasting reaches Ra10 or above.
[0033] 3. High-strength acrylic structural adhesive is used, which is resistant to acid, alkali, water, oil medium corrosion, impact resistance, wide working temperature range (-30~150℃), and bonding strength can reach 70Mpa. It is very suitable for the adhesion between WC carbide bushing 1 and steel bucket substrate 2, and is also very suitable for the working environment of impulse turbine bucket.
[0034] 4. Place the carbide bushing 1 close to the inner wall of the bucket base 2 of the impulse turbine, tighten the movable part 3 in the fastener with bolts, and press the carbide bushing 1, and wait for curing for more than 24 hours.
[0035] 5. For other flow areas of the bucket that need to be subjected to supersonic flame thermal spraying of cemented carbide coating, WC-Co series cemented carbide coating is prepared by supersonic flame thermal spraying technology.
[0036] 6. After spraying, it can be put into use. When the next bucket maintenance time comes, the carbide bushing 1 can be quickly replaced, which greatly saves the maintenance time and cost of the turbine. The carbide coating in the indirect scouring area of the bucket of the impulse turbine is less affected by wear and erosion. Therefore, after the carbide bushing 1 is replaced many times, the indirect impact area of the bucket needs to be re-coated.
[0037] Example 2
[0038] Composition of cemented carbide bushing 1: WC-Co-Cr2C3-TiC-Mo-CeO2, of which Co 10%wt, particle size 0.5~1μm, Cr2C3 12%wt, particle size 0.5~1μm, TiC 4%wt, particle size 0.5~1μm, Mo 5%wt, particle size 0.5~1μm, CeO20.8%wt, particle size 0.5~1μm, and the rest is WC with a particle size of 1~2μm.
[0039] The manufacturing technology of cemented carbide bushing 1 selects vacuum sintering technology to obtain the characteristics of high density, low impurities and high strength. The cemented carbide mixed powder is first pressed under high pressure to form a blank of suitable size in the shape of the inner wall of the bucket, ensuring that after vacuum sintering, the size of the cemented carbide bushing 1 matches the inner wall size of the turbine bucket matrix 2. Then the vacuum sintering process is carried out, including the following three processes: pre-burning stage, high-temperature sintering stage, and cooling stage. During the pre-burning stage, when the vacuum degree is lower than 0.2Pa, the temperature begins to rise. When it reaches 430℃, it is kept warm for 15 hours to ensure that impurities are discharged. During the high-temperature sintering stage, the temperature is kept warm at 1450℃ for 6 hours. During the cooling stage, argon gas is introduced at a pressure of 4MPa to accelerate cooling, and at the same time, it can also increase the density of the cemented carbide bushing. The average thickness of the cemented carbide bushing is made into 8mm.
[0040] A through hole is drilled inside the fixing piece 4 in the fastener, and it is welded to the upper surface outlet of the water bucket base 2. The position of the weld 5 can be selected at the welding connection, and multiple fasteners are distributed around the upper plane of the water bucket.
[0041] A threaded hole which is not a through hole is drilled inside the movable part 3 in the fastener, one end of which is close to the carbide bushing 1, and the other end is fastened to the fixed part 4 in the fastener by a fastening bolt to press the carbide bushing 1.
[0042] The WC cemented carbide coating 6 can be prepared by HVOF (supersonic oxygen flame spraying) technology in the designated area: including the outer wall of the bucket substrate 2, the fixed part 4 in the fastener and the surface of the movable part 3 in the fastener. The spraying material can be a powder formula that has been maturely applied in the market, such as WC-10Co-4Cr powder.
[0043] Pelton turbine bucket protection process:
[0044] 1. Weld the fixing member 4 in the fastener to the upper surface of the bucket base 2 of the impulse turbine;
[0045] 2. Use a cleaning agent to clean the oil stains on the inner wall, outer wall and other surfaces of the water bucket base 2, and then use white corundum to sandblast the above surfaces. The surface roughness of the water bucket after sandblasting reaches Ra10 or above.
[0046] 3. High-strength silicone structural adhesive is used, which has the characteristics of acid, alkali, water, oil medium corrosion, impact resistance, wide working temperature range, and bonding strength up to 60Mpa. It is very suitable for the adhesion between WC carbide bushing 1 and steel bucket substrate 2, and is also very suitable for the working environment of impulse turbine bucket.
[0047] 4. Place the carbide bushing 1 close to the inner wall of the bucket base 2 of the impulse turbine, tighten the movable part 3 in the fastener with bolts, and press the carbide bushing 1, and wait for curing for more than 24 hours.
[0048] 5. For other flow areas of the bucket that need to be subjected to supersonic flame thermal spraying of cemented carbide coating, WC-Co series cemented carbide coating is prepared by supersonic flame thermal spraying technology.
[0049] 6. After spraying, it can be put into use. When the next bucket maintenance time comes, the carbide bushing 1 can be quickly replaced, which greatly saves the maintenance time and cost of the turbine. The carbide coating in the indirect scouring area of the bucket of the impulse turbine is less affected by wear and erosion. Therefore, after the carbide bushing 1 is replaced many times, the indirect impact area of the bucket needs to be re-coated.
[0050] Example 3
[0051] Composition of cemented carbide bushing 1: WC-Co-NbC-Cr-La2O3, of which Co 12%wt, particle size 0.5~1μm, NbC 8%wt, particle size 0.5~1μm, Cr 7%wt, particle size 0.5~1μm, La2O31.2%wt, particle size 0.5~1μm, and the rest is WC with a particle size of 1~2μm.
[0052] The manufacturing technology of cemented carbide bushing 1 selects vacuum sintering technology to obtain the characteristics of high density, low impurities and high strength. The cemented carbide mixed powder is first pressed under high pressure to form a blank of suitable size in the shape of the inner wall of the bucket, ensuring that after vacuum sintering, the size of the cemented carbide bushing 1 matches the inner wall size of the turbine bucket matrix 2. Then the vacuum sintering process is carried out, including the following three processes: pre-burning stage, high-temperature sintering stage, and cooling stage. During the pre-burning stage, when the vacuum degree is lower than 5Pa, the temperature begins to rise. When it reaches 500℃, it is kept warm for 10 hours to ensure that impurities are discharged. During the high-temperature sintering stage, the temperature is kept warm at 1380℃ for 7 hours. During the cooling stage, argon gas is introduced at a pressure of 5MPa to accelerate cooling, and at the same time, the density of the cemented carbide bushing can be increased. The average thickness of the cemented carbide bushing is made into 10mm.
[0053] A through hole is drilled inside the fixing piece 4 in the fastener, and it is welded to the upper surface outlet of the water bucket base 2. The position of the weld 5 can be selected at the welding connection, and multiple fasteners are distributed around the upper plane of the water bucket.
[0054] A threaded hole which is not a through hole is drilled inside the movable part 3 in the fastener, one end of which is close to the carbide bushing 1, and the other end is fastened to the fixed part 4 in the fastener by a fastening bolt to press the carbide bushing 1.
[0055] The WC cemented carbide coating 6 can be prepared by HVOF (supersonic oxygen flame spraying) technology in the designated area: including the outer wall of the bucket substrate 2, the fixed part 4 in the fastener and the surface of the movable part 3 in the fastener. The spraying material can be a powder formula that has been maturely applied in the market, such as WC-10Co-4Cr powder.
[0056] Pelton turbine bucket protection process:
[0057] 1. Weld the fixing member 4 in the fastener to the upper surface of the bucket base 2 of the impulse turbine;
[0058] 2. Use a cleaning agent to clean the oil stains on the inner wall, outer wall and other surfaces of the water bucket base 2, and then use white corundum to sandblast the above surfaces. The surface roughness of the water bucket after sandblasting reaches Ra10 or above.
[0059] 3. High-strength epoxy resin structural adhesive is used, which has the characteristics of acid, alkali, water, oil medium corrosion, impact resistance, wide working temperature range, and bonding strength up to 30Mpa. It is very suitable for the adhesion between WC carbide bushing 1 and steel bucket substrate 2, and is also very suitable for the working environment of impulse turbine bucket.
[0060] 4. Place the carbide bushing 1 close to the inner wall of the bucket base 2 of the impulse turbine, tighten the movable part 3 in the fastener with bolts, and press the carbide bushing 1, and wait for curing for more than 48 hours.
[0061] 5. For other flow areas of the bucket that need to be subjected to supersonic flame thermal spraying of cemented carbide coating, WC-Co series cemented carbide coating is prepared by supersonic flame thermal spraying technology.
[0062] 6. After spraying, it can be put into use. When the next bucket maintenance time comes, the carbide bushing 1 can be quickly replaced, which greatly saves the maintenance time and cost of the turbine. The carbide coating in the indirect scouring area of the bucket of the impulse turbine is less affected by wear and erosion. Therefore, after the carbide bushing 1 is replaced many times, the indirect impact area of the bucket needs to be re-coated.
[0063] The above is only a preferred implementation case of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above implementation case based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for resisting impact erosion of a bucket of an ultra-high head impulse turbine, characterized in that: include: A set of cemented carbide bushings is fixed on the entire surface of the inner wall of the water bucket by a semi-elastic contact connection method. The semi-elastic contact connection method means that the cemented carbide bushing and the water bucket are bonded by structural adhesive to absorb and buffer the different elastic micro-deformations between the bushing and the water bucket, and the edge of the cemented carbide bushing is pressed against the water bucket by fasteners to prevent the cemented carbide bushing from moving; The material of the cemented carbide bushing is any one of WC-Co-VC-TaC-La2O3, WC-Co-Cr2C3-TiC-Mo-CeO2, and WC-Co-NbC-Cr-La2O3; The structural adhesive is an acrylate structural adhesive, a silicone structural adhesive or an epoxy resin structural adhesive; The fastener comprises two parts, one part is a fixed part which is welded and fixed on the edge of the water bucket, and the other part is a movable part which presses the carbide bushing on the water bucket, and the two parts are fastened by fastening bolts.
2. The method for resisting impact erosion of a bucket of an ultra-high head Pelton turbine according to claim 1, characterized in that: The hard alloy protective coating is prepared on the outer wall of the bucket and the surface of the fasteners by using the supersonic flame thermal spraying technology.
3. The method for resisting impact erosion of a bucket of an ultra-high head Pelton turbine according to claim 1, characterized in that: include: 1) Weld the fixing parts of the fasteners to the upper surface of the bucket of the impulse turbine; 2) For the inner wall, outer wall and other surfaces of the impulse turbine, use a cleaning agent to clean the surface oil, and then use white corundum to sandblast the cleaned surface. The surface roughness of the bucket after sandblasting reaches Ra10 or above; 3) Use structural adhesive to coat the inner wall of the water bucket; 4) Place the carbide bushing close to the inner wall of the impulse turbine bucket, press the movable parts of the fasteners against the carbide bushing and the bucket, and fasten the movable parts and the fixed parts with bolts, and wait for curing for more than 24 hours; 5) WC-Co cemented carbide coatings are prepared on other flow areas of the bucket and the surface of fasteners by supersonic flame thermal spraying technology.
4. An ultra-high head impulse turbine bucket, characterized in that: It includes a water bucket body, a hard alloy bushing, and a fastener; the fastener includes a fixed part and a movable part; the hard alloy bushing covers the inner wall of the entire water bucket body and is connected to the inner wall of the water bucket by a structural adhesive; the fixed part is welded to the edge of the water bucket body; the movable part presses the hard alloy bushing to the edge of the water bucket and is fastened to the fixed part by bolts; a hard alloy protective coating is prepared on other flow areas of the water bucket and the surface of the fastener; the material of the hard alloy bushing is any one of WC-Co-VC-TaC-La2O3, WC-Co-Cr2C3-TiC-Mo-CeO2, and WC-Co-NbC-Cr-La2O3; The structural adhesive is an acrylate structural adhesive, a silicone structural adhesive or an epoxy resin structural adhesive.