Method for manufacturing super-flat polycrystalline diamond film on large scale
By growing polycrystalline diamond film on diamond seed growth substrate and transferring it to transfer substrate, and removing the growth substrate by grinding and etching technology, the problem of high surface roughness of polycrystalline diamond film is solved, achieving large The preparation of an area ultra-flat film improves the crystallization quality and optical properties of the film, and supports nano/micrometer-level patterning.
Patent Information
- Application Number
- CN202310540694.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to manufacture high-quality single crystal diamond films under large scale and cost-acceptable conditions. The polycrystalline diamond films limit their application on the nano/micrometer scale due to their high surface roughness.
The polycrystalline diamond film was grown on the diamond seed growth substrate by chemical vapor deposition method, and the growth surface was bonded to the transfer substrate by adhesive, followed by removal of the growth substrate by grinding, dry etching and wet etching. , expose the buried surface and significantly reduce its roughness.
Achieved the preparation of large-area, ultra-flat and transferable polycrystalline diamond films, improved the crystalline quality and optical parameters of the film, approaching the performance of single-crystalline diamond films, and provided a feasible platform for nano/micrometer-level patterns change.
Smart Images

Figure CN118957751A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation technology of polycrystalline diamond films, and in particular relates to a method for large-scale manufacturing of polycrystalline diamond films with ultra-flat surfaces. Background Art
[0002] Diamond materials have excellent intrinsic properties, such as extremely high thermal conductivity, wide optical transparency, wide band gap and ultra-high mechanical hardness, and are considered to be ideal candidates for applications in mechanical, electronic and optical fields. With the significant progress in high pressure and high temperature (HPHT) or chemical vapor deposition (CVD) technology in recent years, large-scale laboratory-grown diamond materials, i.e. synthetic diamonds, can be obtained. In particular, the CVD process is able to produce extremely pure diamonds for optical and mechanical applications. For example, diamond ultrathin films are promising platforms for the development of various photonic structures, such as optical waveguides, resonators, metasurfaces and metalenses.
[0003] Doping diamond can further expand its applications in electronic devices, such as boron-doped p-type semiconductors and superconductors, as well as quantum photonics materials based on atomic defects such as doped nitrogen and silicon, especially those materials called next-generation diamond substrates, such as membranes, which are expected to play an important role in the efficient heat dissipation of circuits and high-power electronic devices, especially for emerging soft / flexible electronic devices.
[0004] Realizing the above-mentioned diamond-based functional elements necessarily involves standard nanofabrication and seamless integration, all of which place higher demands on the surface roughness of diamond materials. In addition, the flat surface of the device is also a prerequisite for many testing / characterization methods that are widely used in the corresponding fields, such as thermal conductivity measurement and bonding in the semiconductor industry.
[0005] However, unlike other materials such as silicon, planarization of diamond is very difficult and requires a lot of time and energy through traditional methods such as polishing.
[0006] Diamond films are mainly produced by homogeneous and heterogeneous growth using chemical vapor deposition (CVD) technology. Single crystal diamond (SCD) films are mainly obtained by homogeneous growth on bulk diamond substrates, and they represent the highest quality required for many applications. For example, it has high mobility for electrons and holes and excellent resistance to radiation, and is also highly valuable for detectors in nuclear and high-energy physics experiments. However, the expensive growth process, limited manufacturing scale, and complex processing of CVD-grown SCD have hindered its widespread application.
[0007] Although heterogeneous growth of SCD on iridium has been demonstrated in a limited number of laboratories around the world, it is still difficult to control the quality of the obtained diamond, which tends to form polycrystalline diamond (PCD) films due to lattice mismatch. Therefore, it is still very challenging to build large-area SCD films on arbitrary substrates.
[0008] In contrast, scalable, inexpensive, and easy-to-grow polycrystalline diamond (PCD) films can be readily obtained on a variety of common substrates, such as Si, SiC, TiC, Co, Pt, Al2O3, Ni, and Re. In particular, based on a sufficiently high nucleus density, it can form a continuous film, and the quality of the film is closely related to the directionality of the nuclei. In order to optimize PCD films, researchers have proposed the concept of nanocrystalline and ultra-nanocrystalline diamond films, which form continuous nuclei by depositing diamond seeds. However, the surface smoothness of PCD films is less than satisfactory, which is one of the biggest bottlenecks in promoting such an excellent platform.
[0009] In summary, the extremely strict growth conditions of single crystal diamond (SCD) have greatly hindered the use of diamond materials in large-scale, cost-acceptable fields; and polycrystalline diamond (PCD) has poor surface morphology and high roughness due to its uneven profile, which seriously limits its further construction of high-precision photonic structures at the nano / micrometer scale. Summary of the invention
[0010] Therefore, the purpose of the present invention is to overcome the problems of poor surface morphology and high roughness of polycrystalline diamond (PCD) films and to provide a simple method for preparing large-area, ultra-flat and transferable PCD films in a scalable and controllable manner.
[0011] A first aspect of the present invention provides a method for large-scale manufacturing of ultra-flat polycrystalline diamond films, the method comprising:
[0012] (1) performing chemical vapor deposition on a growth substrate having a diamond seed crystal on its surface to grow a polycrystalline diamond film, wherein an exposed surface of the polycrystalline diamond film is a growth surface having a first roughness; and a surface of the polycrystalline diamond film bonded to the growth substrate is a buried surface;
[0013] (2) bonding the growth surface of the polycrystalline diamond film to a transfer substrate using an adhesive;
[0014] (3) removing the growth substrate by one or more methods selected from the group consisting of grinding, dry etching, and wet etching to expose the buried surface of the polycrystalline diamond film, wherein the exposed buried surface has a second roughness that is smaller than the first roughness.
[0015] According to the method provided by the present invention, the first roughness may be 10 to 200 nm. In a preferred embodiment of the present invention, the second roughness may be 1 to 10 nm, preferably 1 to 5 nm.
[0016] According to the method provided by the present invention, the buried surface has a higher refractive index than the growth surface. Preferably, the buried surface has a lower extinction coefficient than the growth surface.
[0017] The optical parameters of the polycrystalline diamond film produced by the method of the present invention are at levels comparable to those of SCD grown by the CVD method.
[0018] According to the method provided by the present invention, the position of the XRD diffraction peak of the (111) crystal plane of the buried surface is closer to the standard (111) crystal plane XRD diffraction peak of single crystal diamond than the position of the (111) crystal plane XRD diffraction peak of the growth surface; and the full width at half maximum (FWHM) of the Raman spectrum of the (111) crystal plane of the buried surface is less than the full width at half maximum (FWHM) of the (111) crystal plane of the growth surface. The movement of the XRD diffraction peak indicates the improvement of the crystallization quality, and the narrowing of the full width at half maximum of the Raman spectrum means that the internal crystallization of the film has been improved.
[0019] In some embodiments of the present invention, the thickness of the polycrystalline diamond film may be 200 nm to 800 μm, preferably 200 nm to 1 μm.
[0020] According to the method provided by the present invention, the growth substrate and the transfer substrate may be the same or different, preferably different. In some embodiments of the present invention, the growth substrate may be selected from one or more of Si, SiC, TiC, Co, Pt, Al2O3, Ni, Re, Ir, SiO2 and Mo. In some embodiments of the present invention, the surface roughness of the growth substrate is less than 2nm, preferably less than 1nm, and more preferably less than 0.5nm.
[0021] The transfer substrate can be any material, and the present invention has no particular limitation on this. In order to provide temporary physical support for the polycrystalline diamond film when etching the growth substrate, the transfer substrate is preferably a rigid material, such as one or more of ITO glass, ordinary glass, silicon wafer, sapphire and gallium nitride.
[0022] According to the method provided by the present invention, the diamond seed crystal in step (1) may have a particle size of 2 to 10 nm. Preferably, in step (1), a microwave plasma assisted chemical vapor deposition (MPCVD) device is used to grow the polycrystalline diamond film.
[0023] According to the method provided by the present invention, in step (2), various adhesives can be used to bond the growth surface of the polycrystalline diamond film to the transfer substrate, such as one or more of polymethyl methacrylate (PMMA) electronic resist, water-soluble polyvinyl alcohol, and acetone-soluble photoresist.
[0024] According to the method provided by the present invention, the dry etching in step (3) can be inductively coupled plasma (ICP) etching and / or reactive ion etching; the wet etching includes dissolving the growth substrate with a solution.
[0025] In a preferred embodiment of the present invention, in order to improve production efficiency and avoid curling of the diamond film due to too fast release of internal stress, step (3) may include removing the growth substrate by grinding, dry etching and wet etching in sequence.
[0026] According to the method provided by the present invention, the method may further include dissolving the electronic resist with a solvent to release the polycrystalline diamond film.
[0027] The present invention proposes for the first time a novel and simple method to fabricate large-area, ultra-flat and transferable polycrystalline diamond films in a scalable and controllable manner. The PCD film was successfully transferred from the growth substrate to an arbitrary substrate by grinding, dry etching and wet etching processes. The effectiveness of the method of the present invention was verified by detailed characterization of the surface morphology and material properties of the buried surface. In addition, the present invention also performed nano / micrometer-scale patterning in a bottom-up and top-down manner, verifying the feasibility of the prepared film as a nano / micrometer processing platform. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The embodiments of the present invention are described in detail below with reference to the accompanying drawings, wherein:
[0029] Figure 1 The following are actual photographs of the polycrystalline diamond film prepared in Example 1 of the present invention being placed on a polydimethylsiloxane (PDMS) film (left picture) and an ITO glass (right picture).
[0030] Figure 2 Figures (a), (b), (c) and (d) are respectively physical photographs of the polycrystalline diamond film (growth surface) grown on the silicon wafer in Example 1, as well as the corresponding (b) SEM image and (c) AFM image, and a height variation diagram (d) along the dotted line marked in (c).
[0031] Figure 3Figures (a), (b), (c) and (d) are respectively the actual photographs of the polycrystalline diamond film (buried surface) transferred on the ITO glass, and the corresponding (b) SEM image and (c) AFM image, as well as the height variation diagram (d) along the dotted line marked in (c).
[0032] Figure 4 (a) AFM image of the polished SCD sample and (b) the amplitude variation of the measured cross section.
[0033] Figure 5 Comparison of the refractive indices of the growth surface of the polycrystalline diamond film grown on the silicon wafer in Example 1 (a) and the buried surface of the polycrystalline diamond film transferred on the ITO glass (b).
[0034] Figure 6 1 and 2 are the XRD results of the growth surface of the polycrystalline diamond film grown on the silicon wafer and the buried surface of the polycrystalline diamond film transferred on the ITO glass in Example 1.
[0035] Figure 7 These are Raman spectra of the growth surface of the polycrystalline diamond film grown on the silicon wafer and the buried surface of the polycrystalline diamond film transferred on the ITO glass in Example 1.
[0036] Figure 8 3 is a SEM image of the grating structure formed on the growth surface and buried surface of the patterned polycrystalline diamond film obtained in Example 2.
[0037] Fig. 9 1 and 1 are SEM images of diamond pillar structures formed on the growth surface and buried surface of the patterned polycrystalline diamond film obtained in Example 3.
[0038] Fig.10 1 and 2 are SEM images of the growth surfaces of the polycrystalline diamond films with thicknesses of 400 nm and 1 μm prepared in Example 4. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0040] Example 1
[0041] Fabrication of polycrystalline diamond films
[0042] (1) Heteroepitaxial growth of diamond films
[0043] Diamond heteroepitaxial growth on silicon substrates includes three steps: substrate pretreatment, deposition of diamond seeds and CVD growth of diamond films.
[0044] Substrate pretreatment: The silicon surface was pretreated with hydrogen plasma at 1300 W power, 35 Torr chamber pressure and 300 sccm H 2 A 2-inch silicon wafer was placed in a microwave plasma assisted chemical vapor deposition (MPCVD) apparatus under air flow conditions for 10 minutes.
[0045] Deposition of diamond seed crystals: Diamond seed crystals with a size of less than 10 nm (purchased from Tokyo Chemical Industry Co., Ltd.) were mixed with dimethyl sulfoxide (DMSO), anhydrous ethanol and acetone in a mass ratio of 1:5000:250:250. The mixture was ultrasonically dispersed for 12 hours and then centrifuged at 1000 r / min for 20 minutes to separate impurities. The suspension was spin-coated on a silicon wafer with deposition parameters: 500 r / min, 3 drops were added within 15 s, then the speed was increased to 4500 r / min for 110 s, and repeated three times.
[0046] CVD growth of diamond film: A silicon wafer with diamond seed crystals deposited thereon was placed in an MPCVD device (Seki 6350) to grow a diamond film. The main growth parameters included: 3400 W microwave power, 900 °C temperature, 15 sccm methane flow rate and 40 minutes growth time. A PCD film about 450 nm thick was grown on the silicon substrate.
[0047] (2) Diamond film substrate transfer
[0048] The diamond film on the silicon wafer was cut into small pieces, then cleaned in acetone, isopropanol and deionized water for 10 minutes, and then dried with nitrogen. After the silicon substrate was turned over, another rigid substrate was used to support the diamond film. In this embodiment, 2cm×2cm indium tin oxide (ITO) glass was selected. A drop of 10μl polymethyl methacrylate (PMMA) electron beam resist was dropped on the surface of the ITO glass, and the diamond film was bonded to the ITO substrate. The sample was placed in a vacuum chamber to degas the PMMA for 1 hour, and the pressure of the vacuum chamber was maintained at -1kg / cm 2 After degassing, the samples were heated at 100 °C for 30 min to cure the PMMA.
[0049] The bonded samples were subjected to grinding, dry etching and wet etching in sequence to remove the silicon substrate. Specifically, the process includes: using a crystal phase grinder with a 2000C sandpaper mask to thin the silicon substrate, the rotation speed of the grinder was initially set to 600 rpm, and when the thickness of the silicon substrate was less than 100 μm, it was reduced to 100 rpm (the rotation speed was reduced to prevent curling between the diamond film and the PMMA layer, which is conducive to the rapid release of internal stress); when the thickness of the silicon substrate was reduced to about 20 μm, the sample was transferred to an inductively coupled plasma (ICP) etcher for precise etching, the etching gas was SF6 with a flow rate of 92 sccm, O2 was used as a protective gas with a flow rate of 38 sccm, the RF voltage was set to 600 W, the bias voltage was set to 150 W, the pressure in the chamber was fixed to 35 mTorr, the etching time was 15 minutes, and the etching rate of silicon was about 1.3 μm / min; after ICP etching most of the silicon, the sample was immersed in 20% NaOH for 1 hour to remove silicon residues, and then rinsed with deionized water.
[0050] (3) Immerse the etched sample in acetone solvent to dissolve the PMMA layer. Use any substrate to support the floating polycrystalline diamond film, and then dry it with nitrogen. In this example, the prepared polycrystalline diamond film is placed on a polydimethylsiloxane (PDMS) film or ITO glass for characterization.
[0051] Example 2
[0052] Electron beam lithography patterning
[0053] The growth surface and the buried surface of the polycrystalline diamond film prepared in Example 1 were patterned respectively using an electron beam lithography (EBL) apparatus.
[0054] PMMA 950 resist (3%) was spin-coated on the growth surface and the buried surface at a speed of 3000 r / min, and the thickness of the PMMA coating was about 150 nm. 2 The coated PMMA resist was irradiated with an electron beam in an array of grating structures at a dose of 1.5 Å, and then developed in a mixed solution of isopropyl alcohol (IPA) and water (1:3) at 0°C.
[0055] Example 3
[0056] Construction of diamond pillars
[0057] Preparation of silica sphere etching mask: Commercially available 200nm silica spheres were suspended in 2.5% ethanol solvent, and 20μl of silica sphere suspension and 400μl of ethanol solvent were taken with a pipette and mixed at a ratio of 1:20. The diluted mixture was treated with an ultrasonic machine for 10 minutes to ensure the dispersion of the silica spheres. After the silica spheres were diluted and dispersed, 10μl droplets were extracted with a pipette and placed on the growth surface and buried surface of the diamond film prepared in Example 1, respectively. After the solvent evaporated, a monolayer of silica spheres was formed on the growth surface and the buried surface.
[0058] Dry etching of diamond film: Diamond material was etched with oxygen gas at a flow rate of 30 sccm. The ICP RF voltage, bias voltage and chamber pressure were set to 420 W, 60 W and 10 mTorr respectively. The etching time was 4 minutes and the etching rate was about 1.7 nm / s.
[0059] After etching was completed, the silica spheres were removed by ultrasonic treatment.
[0060] Surface morphology characterization
[0061] 1. Figure 1 The following are actual photographs of the polycrystalline diamond film prepared in Example 1 of the present invention being placed on a polydimethylsiloxane (PDMS) film (left picture) and an ITO glass (right picture).
[0062] 2. Figure 2 Figures (a), (b), (c) and (d) are respectively physical photographs of the polycrystalline diamond film (growth surface) grown on the silicon wafer in Example 1, as well as the corresponding (b) SEM image and (c) AFM image, and a height variation diagram (d) along the dotted line marked in (c). Figure 3 Figures (a), (b), (c) and (d) are respectively the actual photographs of the polycrystalline diamond film (buried surface) transferred on the ITO glass, and the corresponding (b) SEM image and (c) AFM image, as well as the height variation diagram (d) along the dotted line marked in (c).
[0063] Scanning electron microscopy (SEM) was used to characterize the 450 nm thick diamond film ( Figure 2 Figure a) and diamond film transferred onto ITO glass ( Figure 3 The result is as follows Figure 2As shown in Figure 3b and Figure 3b. According to the SEM images, there are some obvious grains on the growth surface, and their sizes are mainly between 100-300 nm. In contrast, the buried surface has a smooth surface profile with some negligible pores, which are caused by the corrosion of silicon residues by NaOH. In order to quantify the smoothness of the diamond film, an area of 10μm×10μm was scanned by atomic force microscopy (AFM) to determine the average roughness. Figure 2 The c graph and Figure 3 The results of Figure c show that the roughness dropped significantly from 32.34 nm to 1.49 nm, close to the level of the polished SCD surface. Figure 2 The d graph and Figure 3 As shown in Figure d, Figure 2 The c graph and Figure 3 The corresponding height change of the cross section marked in panel c further confirms that the surface morphology of the buried surface is significantly improved compared with that of the growth surface.
[0064] 3. In order to compare the buried surface of the flipped diamond film with the standard polished single crystal diamond (SCD), the roughness of the SCD sample was characterized. The standard sample was purchased from Element Six. From the results of AFM measurement ( Figure 4 (a)), the surface roughness of SCD is about 0.37 nm. Figure 4 (b) shows the magnification change of the defined cross section. It can be seen that although the roughness of the buried surface of the flipped polycrystalline diamond film is still greater than that of the SCD sample, the roughness has dropped significantly from 32.34 nanometers (growth surface) to 1.49 nanometers (buried surface), successfully providing conditions for precision manufacturing on the film.
[0065] Optical and material properties characterization of polycrystalline diamond films
[0066] 1. The refractive index of the polycrystalline diamond film grown on the silicon wafer (growth surface) and the polycrystalline diamond film transferred on the ITO glass (buried surface) in Example 1 was measured using an optical ellipsometer.
[0067] Figure 5 The refractive index comparison of the growth surface of the polycrystalline diamond film grown on the silicon wafer (a) and the buried surface of the polycrystalline diamond film transferred on the ITO glass (b) in Example 1, where n represents the refractive index and k represents the extinction coefficient. Figure 5 From the measurement results, the buried surface has a higher refractive index and a lower extinction coefficient than the growth surface, and it is found that the levels of these optical parameters of the buried surface are comparable to those of SCD grown by the CVD method.
[0068] 2. X-ray diffraction (XRD) technology was used to characterize the crystallization characteristics of the polycrystalline diamond film obtained in Example 1. Figure 6 As shown in the figure, obvious diffraction peaks were obtained at 43.96°, 75.14° and 91.52°, corresponding to the (111), (220) and (311) crystal planes, respectively, confirming that the buried surface has diamond properties. The strong diffraction peak of the (111) crystal plane indicates its dominance, which is consistent with other reports. In addition, the full width at half maximum (FWHM) of the (111) crystal plane diffraction peak of the buried surface is 0.64° narrower than that of the growth surface. In addition to the change in FWHM, the position of the diffraction peak of the (111) crystal plane shows a significant shift ( Figure 6 , inset), from 44.36° (growth surface) to 43.96° (buried surface), which is close to the position of the SCD (43.95°) of the standard (111) orientation. The shift of the diffraction peak indicates an improvement in crystal quality, which may be related to the release of internal stress. Normally, due to the lattice mismatch between diamond and the foreign substrate, residual stress will be introduced into the film, which will further induce lattice distortion and lead to abnormal movement of the diffraction peak. By adopting the manufacturing method of the present invention, the residual stress has the opportunity to be released after removing the growth substrate.
[0069] 3. Raman spectroscopy is used to further characterize the crystallization characteristics of the polycrystalline diamond film obtained in Example 1. Figure 7 From the Raman spectrum, at 1332.8cm -1 An obvious diamond scattering peak was observed at , which further proved the state of the film. Figure 7 From the illustration, the FWHM of the buried surface (7.43cm -1 ) than the FWHM of the growth surface (7.67cm -1 ) is narrower than that of the buried surface, indicating that the internal crystallization of the film measured from the buried surface is improved.
[0070] The improved optical properties and crystalline quality of diamond films indicate their potential for developing photonic structures.
[0071] Characterization of nano / micro patterns on polycrystalline diamond films
[0072] 1. The grating structures formed on the growth surface and buried surface of the patterned polycrystalline diamond film obtained in Example 2 were characterized by SEM. The results are as follows: Figure 8As shown, (a) and (b) are SEM images of the growth surface, and (c) and (d) are SEM images of the buried surface. In (a), it can be seen that there are a large number of particles on the growth surface, which are mainly formed during the spin coating process of the PMMA resist. When the PMMA resist encounters large particles distributed on the growth surface, it aggregates, reducing the uniformity of the resist coating. In contrast, the buried surface is very flat and smooth, which is conducive to the uniform coating of the PMMA resist ( Figure 8 (c) Figure), and can form a uniform grating pattern. Figure 8 From the (b) image, in the high magnification SEM image, the grating structure obtained on the growth surface has obvious irregularities along the line shape. With the optimization of the surface morphology, the grating structure made on the buried surface ( Figure 8 (d) shows significantly better uniformity than the growth surface.
[0073] 2. The diamond pillar structures formed on the growth surface and buried surface of the patterned polycrystalline diamond film obtained in Example 3 were characterized by SEM. The results are as follows: Fig. 9 As shown, (a) and (b) are SEM images of the growth surface, (c) and (d) are SEM images of the buried surface, and the scale bars in the figures are 500nm. Since the large grains on the growth surface show different directions, the difference in crystal planes leads to non-uniform etching rate. In addition, since the grain size on the growth surface is comparable to the diameter of the diamond pillar, the non-uniform morphology of the diamond pillar is inevitable ( Fig. 9 In addition, the grains on the top surface of the diamond pillars introduce irregular boundaries and interact strongly with adjacent grains. In contrast, using the buried surface as the etching surface yields diamond pillars with clear boundaries and no surface residues ( Fig. 9 (c)). A smooth, flat buried surface is conducive to obtaining a flat top and clear boundaries of individual pillars ( Fig. 9 (d)). The negligible residue, flat top profile, and smooth boundaries of the diamond pillars fabricated on the buried surface indicate that the buried surface can provide an excellent platform for diamond-based photonic structures.
[0074] Example 4
[0075] Fabrication of polycrystalline diamond films with different thicknesses
[0076] According to the method in Example 1, polycrystalline diamond films with thicknesses of 400 nm and 1 μm were manufactured, respectively, and their surface morphology characteristics were characterized.
[0077] Fig.10These are SEM images of the growth surfaces of polycrystalline diamond films with thicknesses of 400 nm and 1 μm, where (a)-(c) are SEM images of the 400 nm thick diamond film at different magnifications, and (d)-(f) are SEM images of the 1 μm thick diamond film at different magnifications, and the scale bars are all 500 nm.
[0078] according to Fig.10 The morphological features of the growth surface of polycrystalline diamond films of different thicknesses are shown. As the thickness of the film increases from 400nm in (ac) to 1μm in (df), the grain size increases significantly, resulting in a rougher surface of the film. Therefore, the difference in roughness between the growth surface and the buried surface will be further expanded. It will also be more difficult to fabricate structures on thicker diamond films. The strategy of flipping the diamond film proposed in the present invention is crucial to obtaining ultra-flat diamond films, especially for thicker diamond films.
[0079] It can be seen from the above embodiments that the manufacturing method of the present invention obtains a large-area ultra-flat diamond film by transferring the polycrystalline diamond film from the growth substrate to an arbitrary substrate. Compared with the 32.34nm roughness of the growth surface, the buried diamond layer shows a smooth surface with an average roughness of 1.49nm. XRD and Raman measurements show that the crystalline properties of the buried surface are significantly improved compared with the growth surface, which is attributed to the release of stress in the diamond film. In addition, bottom-up and top micro-nano patterning were performed on the film through Examples 2 and 3, and the observation of high-precision good structures obtained on the buried surface confirmed the feasibility of the film platform. The method of the present invention opens up new prospects for the practical development of polycrystalline diamond films and lays an important foundation for accelerating the research and application of diamond materials in various fields.
Claims
1. A method for large-scale production of ultra-flat polycrystalline diamond films, the method comprising: (1) performing chemical vapor deposition on a growth substrate having a diamond seed crystal on its surface to grow a polycrystalline diamond film, wherein an exposed surface of the polycrystalline diamond film is a growth surface having a first roughness; and a surface of the polycrystalline diamond film bonded to the growth substrate is a buried surface; (2) bonding the growth surface of the polycrystalline diamond film to a transfer substrate using an adhesive; (3) removing the growth substrate by one or more methods selected from the group consisting of grinding, dry etching, and wet etching to expose the buried surface of the polycrystalline diamond film, wherein the exposed buried surface has a second roughness that is smaller than the first roughness.
2. The method according to claim 1, wherein: The first roughness is 10-200 nm; preferably, the second roughness is 1-10 nm, more preferably 1-5 nm.
3. The method according to claim 1 or 2, wherein: The buried surface has a higher refractive index than the growing surface; preferably, the buried surface has a lower extinction coefficient than the growing surface.
4. The method according to any one of claims 1 to 3, wherein: Compared with the position of the (111) crystal plane XRD diffraction peak of the growth surface, the position of the (111) crystal plane XRD diffraction peak of the buried surface is closer to the standard (111) crystal plane XRD diffraction peak of single crystal diamond; and the half-maximum full width of the (111) crystal plane XRD diffraction peak of the buried surface is smaller than the half-maximum full width of the (111) crystal plane XRD diffraction peak of the growth surface.
5. The method according to any one of claims 1 to 4, wherein: The thickness of the polycrystalline diamond film is 200 nm to 800 μm, preferably 200 nm to 1 μm.
6. The method according to any one of claims 1 to 5, wherein: The growth substrate is selected from one or more of Si, SiC, TiC, Co, Pt, Al2O3, Ni, Re, Ir, SiO2 and Mo.
7. The method according to any one of claims 1 to 6, wherein: The surface roughness of the growth substrate is lower than 2 nm, preferably lower than 1 nm, and more preferably lower than 0.5 nm.
8. The method according to any one of claims 1 to 7, wherein: The adhesive is an anti-corrosion agent, such as one or more of polymethyl methacrylate electronic anti-corrosion agent, water-soluble polyvinyl alcohol, and photoresist soluble in acetone.
9. The method according to any one of claims 1 to 8, wherein: The particle size of the diamond seed crystal described in step (1) is 2 to 10 nm; Preferably, in step (1), a microwave plasma assisted chemical vapor deposition device is used to grow the polycrystalline diamond film.
10. The method according to any one of claims 1 to 9, wherein: The dry etching in step (3) is inductively coupled plasma (ICP) etching and / or reactive ion etching; the wet etching includes dissolving the growth substrate with a solution; Preferably, step (3) comprises removing the growth substrate by sequentially using grinding, dry etching and wet etching methods.
Citation Information
Cited By
Method for manufacturing super-flat polycrystalline diamond film on large scale
CN119465395A
Composite wafer and integration method and application thereof
CN120221490A
Composite wafer, integration method and applications thereof
CN120221490B
A method for mass production of ultraflat polycrystalline diamond films
CN120677268B
Machining method for inner surface and outer surface of polycrystalline diamond
CN120680386A