A method for smelting pure titanium ingot with low oxygen content

By controlling the environmental humidity and process parameters during the smelting process of titanium sponge, the problem of difficult oxygen content in VAR smelting technology is solved, and the preparation of low-oxygen content pure titanium ingots is realized, which improves the quality and oxygen content of the ingot. Uniformity.

CN115852170BActive Publication Date: 2024-11-26西部超导材料科技股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211489918.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-25
Publication Date
2024-11-26
Estimated Expiration
2042-11-25

AI Technical Summary

Technical Problem

The existing VAR smelting technology is difficult to effectively control pure titanium ingots with an oxygen content of ≤0.05%, which cannot meet the strict requirements for oxygen content in the high-tech industry, and the impurity element removal effect is limited.

Method used

By selecting low oxygen and low chlorine titanium sponge, controlling the ambient humidity, adjusting the melting speed and self-consuming electrode feeding speed during the first and final product smelting process, controlling the arc distance range, combining the stable arc magnetic field and crucible gap, improving the melting The exhaust effect of the pool achieves stable control of oxygen content.

Benefits of technology

The preparation of pure titanium ingots with an oxygen content of ≤0.05% was successfully achieved, which improved the quality of the ingot and the uniformity of the oxygen content, and avoided the problem of increased oxygen content caused by impurities volatilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852170B_ABST
    Figure CN115852170B_ABST
Patent Text Reader

Abstract

The present invention relates to a smelting method of a low-oxygen content pure titanium ingot, comprising the following steps: S1, using a hydraulic press to press sponge titanium into an electrode block, and using a welding box to weld multiple electrode blocks into consumable electrodes; S2, smelting the consumable electrode once to obtain a primary ingot, and adjusting the melting speed and the feeding speed of the consumable electrode to control the arc distance in the smelting process within a certain range; S3, after the primary ingot is cooled and taken out of the furnace, the end face of the primary ingot is flattened, and the surface of the primary ingot is peeled; S4, drying the primary ingot; S5, turning the primary ingot around to smelt the finished product, and adjusting the melting speed and the feeding speed of the consumable electrode to control the arc distance in the finished product smelting process within a certain range, and combining the arc stabilizing magnetic field to control the stirring of the molten pool and the edge of the molten pool; S6, cooling the finished product after smelting. The method can stably control the oxygen content of the pure titanium ingot in the VAR smelting process within 0.05%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metal processing and relates to a smelting method for a pure titanium ingot with low oxygen content. Background Art

[0002] Titanium and titanium alloys have been widely used in aerospace, electric power, shipbuilding, marine engineering, chemical industry, biomedicine, metallurgy, sports equipment and other fields due to their low density, high strength, good corrosion resistance and excellent biocompatibility. Among them, the domestic grades of industrial pure titanium mainly include TA1, TA2, TA3, etc., which are widely used in chemical industry, petroleum, electric power, metallurgy, environmental protection, biomedicine and other fields.

[0003] Among them, TA1 requires the oxygen content to be ≤0.1%. In recent years, with the development of high-tech industries such as aerospace and electronic information, the demand for high-purity titanium is increasing, and the requirements for oxygen content are becoming more stringent. The oxygen content standard of ≤0.1% is already difficult to meet the use requirements. Many application requirements for the oxygen content in pure titanium have required the oxygen content in the ingot to be ≤0.05%. For the VAR smelting process, the effect of removing impurity elements such as N, O, and H is very limited. Due to the above technical difficulties, VAR smelting still has no good solution to the method of controlling ultra-low oxygen content. How to stably prepare pure titanium ingots with an oxygen content of ≤0.05% through VAR smelting has become a technical bottleneck in the materials field. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and propose a smelting method for pure titanium ingots with low oxygen content, which controls the selection of raw materials, environment and other process factors combined with the control of melting rate, consumable electrode feed speed and arc distance during the primary smelting and finished product smelting process, so that the oxygen content of the final pure titanium ingot is ≤0.05%.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for smelting a low-oxygen-content pure titanium ingot comprises the following steps:

[0007] S1. Using a hydraulic press to press titanium sponge into electrode blocks, and using a welding box to weld multiple electrode blocks into consumable electrodes;

[0008] S2. When the pre-vacuum is ≤1.0Pa and the leakage rate is ≤0.5Pa / min, the consumable electrode is melted once to obtain an ingot. During the melting process, the arc stabilizing current is controlled to be 10-25A DC. The arc distance range is controlled by adjusting the melting speed and the consumable electrode feed speed.

[0009] S3. After the primary ingot is cooled and taken out of the furnace, the end surface of the primary ingot is flattened and the surface of the primary ingot is peeled, with the peeling depth ≥3mm;

[0010] S4, drying the primary ingot at a temperature of 50-150°C for a drying time of ≥2h;

[0011] S5. When the pre-vacuum is ≤1.0Pa and the leakage rate is ≤0.5Pa / min, the primary ingot is turned around for finished product smelting. The arc stabilizing current is 10-30A. During the smelting process, the arc distance range is controlled by adjusting the melting speed and the consumable electrode feed speed.

[0012] S6. After the finished product is smelted, it is cooled and taken out of the furnace.

[0013] Furthermore, the titanium sponge in S1 is 0 A Grade or grade 0, the oxygen content in the sponge titanium is ≤0.06%, and the Cl element content is ≤0.05%.

[0014] Furthermore, in S1, the humidity in the environment before the titanium sponge is pressed by the hydraulic press is ≤60%.

[0015] Furthermore, the time period from the completion of pressing the titanium sponge into the electrode block to the start of the first smelting of the consumable electrode is ≤24 hours.

[0016] Furthermore, in S2, before the first smelting, the diameter ratio of the consumable electrode to the crucible is ≤4 / 5; in S6, before the finished product smelting, the diameter ratio of the consumable electrode to the crucible is ≤7 / 8.

[0017] Furthermore, during the primary smelting process of S2, the molten pool is controlled to reach the edge, and the flash width is ≤20mm; during the finished product smelting process of S5, the molten pool is controlled to reach the edge, and the flash width is ≤5mm.

[0018] Furthermore, during the primary smelting process of S2, the melting rate is 10-20 kg / min, and the consumable electrode feed speed is 10-30 mm / min; during the finished product smelting process of S5, the melting rate is 15-30 kg / min, and the consumable electrode feed speed is 2-20 mm / min.

[0019] Furthermore, during the primary smelting process of S2, the arc distance ranges from 30 to 80 mm; during the finished product smelting process of S5, the arc distance ranges from 30 to 100 mm.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The technicians of the present invention have found through a large number of creative experimental explorations that to obtain a pure titanium ingot with a low oxygen content, it is necessary not only to control the oxygen content in the titanium sponge, but also to control the Cl content in the titanium sponge. When the Cl content is greater than 0.05%, the volatilization of Cl compounds during a single smelting process will cause the vacuum in the smelting process to become extremely poor. In the worst case, the vacuum in the molten pool will even exceed 20Pa. This vacuum will inhibit the discharge of water vapor and its decomposition products H and O in the molten pool, which will directly lead to an increase in the O content in the ingot, and it is difficult to further reduce the O content in the ingot by multiple smelting methods. Based on this, the present invention selects low O and low Cl titanium sponge, controls the ambient humidity during the consumable electrode pressing process, and adjusts the melting speed and the consumable electrode feed speed during the single and finished product smelting process to control the arc distance in the smelting process within a certain range, combines the arc stabilizing magnetic field to control the stirring of the molten pool and the molten pool to the edge, and cooperates with a certain crucible gap to effectively promote the exhaust effect of the molten pool, and finally achieves the control capability of the oxygen content of the pure titanium ingot ≤0.05% during the VAR smelting process. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0024] Figure 1 This is a diagram showing the situation of the primary ingot molten pool reaching the edge in Example 1 of the present invention;

[0025] Figure 2 This is a diagram of a finished pure titanium ingot obtained in Example 1 of the present invention;

[0026] Figure 3 This is a diagram showing the edge of the first ingot melt pool in Comparative Example 1 of the present invention;

[0027] Figure 4 It is a diagram showing the situation of the first ingot molten pool reaching the edge in comparative example 2 of the present invention. DETAILED DESCRIPTION

[0028] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples of devices consistent with some aspects of the present invention as detailed in the appended claims.

[0029] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0030] A method for smelting a low-oxygen-content pure titanium ingot comprises the following steps:

[0031] Step 1: Use GB / T 2524-2019 A Grade 0 or grade 1 titanium sponge, the oxygen content in the titanium sponge is controlled below 0.06%, and the Cl element is controlled below 0.05%;

[0032] Step 2: Use a hydraulic press to press the titanium sponge into an electrode block, and use a welding box to weld multiple electrode blocks into consumable electrodes. The humidity in the environment before pressing the titanium sponge with the hydraulic press is ≤60%;

[0033] Step 3: When the pre-vacuum is ≤1.0Pa and the leakage rate is ≤0.5Pa / min, the consumable electrode is melted once to obtain an ingot. During the melting process, the arc stabilization current is controlled to be 10-25A DC. By adjusting the melting speed and the feeding speed of the consumable electrode, the arc distance range is controlled to be 30-80mm, the melting speed is 10-20kg / min, and the feeding speed of the consumable electrode is 10-30mm / min; the time period from the completion of pressing the sponge titanium into the electrode block to the start of the first melting of the consumable electrode is ≤24h; the diameter ratio of the consumable electrode to the crucible is ≤4 / 5; during the first melting process, the molten pool is controlled to the edge, and the flash width is ≤20mm;

[0034] Step 4: After the primary smelting is cooled and taken out of the furnace, the end face of the primary ingot is flattened and the surface of the primary ingot is peeled, with the peeling depth ≥3mm;

[0035] Step 5: Dry the primary ingot at a temperature of 50-150°C for a drying time of ≥2h;

[0036] Step 6: When the pre-vacuum is ≤1.0Pa and the leakage rate is ≤0.5Pa / min, the primary ingot is turned around for finished product smelting, the arc stabilizing current is 10-30A, the melting rate is 15-30kg / min, the consumable electrode feed speed is 2-20mm / min; the diameter ratio of the consumable electrode to the crucible is ≤7 / 8; during the finished product smelting process, the molten pool is controlled to the edge, the flash width is ≤5mm, and the arc distance is controlled to be in the range of 30-100mm.

[0037] Step 7: After the finished product is smelted, it is cooled and taken out of the furnace.

[0038] In the above preparation method, on the basis of controlling the oxygen content in the titanium sponge to be less than 0.06% and the Cl element to be less than 0.05%, before pressing the electrode, the humidity in the environment is controlled to be ≤60%, which can effectively avoid the absorption of moisture by the titanium sponge due to the high humidity in the production environment, thereby causing the water vapor or decomposition products H and O to be unable to be fully discharged during the smelting process; after the first smelting is completed, the surface of the ingot is peeled ≥3mm, because after the first ingot is smelted, there are more low-melting point volatiles on the surface of the ingot. These volatiles are very easy to absorb water vapor in the air during the process of slow cooling of the ingot in contact with the air. Once the ingot absorbs water vapor, the removal effect is not good in the finished product smelting stage, which will directly lead to an increase in the oxygen content of the ingot. After the first ingot is peeled, the ingot is dried at 50-150°C for more than 2h to further control the dryness of the ingot surface. The purpose of the above process control measures is to reduce the moisture absorption or water absorption of the consumable electrode or the first ingot.

[0039] In the case where the consumable electrode or the primary ingot does not absorb moisture, if the smelting process parameters are not properly controlled, the oxygen content of the pure titanium finished ingot will also be high. For example, if the molten pool does not reach the edge well during the smelting process, the flash edge of the ingot is too thick, and the water vapor or H, O in the molten pool is difficult to be effectively discharged, which will directly affect the oxygen content of the final finished ingot. When the molten pool reaches the edge well, the exhaust effect of the molten pool is significantly improved. In the prior art, the molten pool is usually achieved by increasing the smelting power. However, due to the poor fluidity of pure titanium in the liquid molten pool, increasing the power will cause the stability of the molten pool to deteriorate during the smelting process, and the molten pool will shake violently, which will aggravate the molten pool's poor edge, thereby affecting the exhaust of the molten pool.

[0040] The preparation method of the present invention controls the theoretical arc distance within the range of 30 to 80 mm by adjusting the melting speed and the consumable electrode feed speed during the first smelting process. The arc distance range also avoids the shaking or short circuit of the molten pool caused by the excessive pressure of the consumable electrode on the molten pool due to the short arc distance, and the large loss of smelting input power caused by the long arc distance, the poor molten pool edge caused by insufficient molten pool heat, and the occurrence of excessively thick flash. Combined with the arc-stabilizing magnetic field stirring control and the crucible gap control, the flash width during the smelting process is constrained to less than 20 mm, which effectively improves the exhaust effect of the molten pool. In the finished product smelting, the theoretical arc distance is controlled to 30 to 100 mm. When the finished product smelting has a better molten pool edge than the first smelting, the arc-stabilizing current control and the crucible gap control are combined to lengthen the arc distance to increase the stirring effect and further increase the exhaust effect, so that the oxygen content of the final pure titanium ingot is ≤0.05%, thereby improving the quality of the ingot.

[0041] Example 1

[0042] Step 1: Use GB / T 2524-2019 AGrade 0 or grade 1 titanium sponge, the oxygen content in the titanium sponge is ≤0.05%, and the Cl element is ≤0.04%;

[0043] Step 2: Use a hydraulic press to press the titanium sponge into an electrode block with a specification of Φ415 mm, and use a welding box to weld the electrode block into a consumable electrode under the condition that the ambient humidity is ≤60%;

[0044] Step 3: Within 12 hours after the consumable electrode is pressed, when the pre-vacuum reaches below 1.0Pa and the leakage rate is below 0.5Pa / min, a Φ560mm crucible is used for primary smelting. The melting speed of the primary smelting is set to 10kg / min, and the feeding speed of the consumable electrode is set to 10mm / min. The melting speed and the feeding speed of the consumable electrode are adjusted to make the target value of the theoretical arc distance in the melting process 70-80mm. The arc stabilization current is 15A DC, and the flash width is controlled to ≤15mm during the smelting process;

[0045] Step 4: After the primary smelting is cooled and taken out of the furnace, the end face of the primary ingot is flattened and the surface of the primary ingot is peeled, with a peeling depth of 4 mm;

[0046] Step 5: drying the primary ingot at a temperature of 100°C for 4 hours;

[0047] Step 6: Turn the primary ingot around for finished product smelting. When the pre-vacuum reaches below 1.0Pa and the leakage rate is below 0.05Pa / min, a Φ640mm crucible is used for finished product smelting. The arc stabilizing current for finished product smelting is 25A, the melting speed is set to 26-30kg / min, and the consumable electrode feed speed is set to 2-7mm / min. Through the control of the melting speed and the consumable electrode feed speed, the theoretical calculated arc distance during the smelting process is controlled at 80-100mm, and the flash width during the smelting process is controlled at ≤5mm.

[0048] Step 7: After the finished product is smelted, it is cooled and taken out of the furnace.

[0049] The vacuum degree during the first ingot melting process in this embodiment is ≤0.7pa, and the first ingot molten pool reaches the edge as shown in the following figure. Figure 1 As shown, the actual burr width is ≤10mm through measurement.

[0050] The actual vacuum degree during the melting process of the finished ingot corresponding to this embodiment is less than or equal to 0.5Pa. The photo of the finished ingot is shown in Figure 2 shown.

[0051] Block samples were taken from the head, middle and tail of the Φ640 mm ingot melted in this embodiment for analysis. The gas element sampling test results of different parts of the Φ640 mm ingot are shown in Table 1:

[0052] Table 1.

[0053] Location O% N% H% head 0.035 0.004 0.001 Central 0.037 0.003 0.001 Tail 0.037 0.004 0.001

[0054] It can be seen from Table 1 that the oxygen content of the head, middle and tail of the Φ640 mm ingot can be stably controlled at a level of ≤ 0.04%, and the oxygen content of different positions of the ingot is evenly distributed without any increase in O.

[0055] Example 2

[0056] Step 1: Use 0A grade or 0 grade titanium sponge in GB / T 2524-2019, the oxygen content in the titanium sponge is 0.05% and the Cl content is 0.04%;

[0057] Step 2: Use a hydraulic press to press the titanium sponge into an electrode block of Φ500mm, and use a welding box to weld the electrode block into a consumable electrode under an ambient humidity of 60%;

[0058] Step 3: Within 24 hours after the consumable electrode is pressed, when the pre-vacuum reaches below 1.0Pa and the leakage rate is below 0.5Pa / min, a Φ640mm crucible is used for primary smelting. The melting rate of the primary smelting is set to 15kg / min, and the feeding speed of the consumable electrode is set to 12-15mm / min. The melting rate and the feeding speed of the consumable electrode are adjusted to make the theoretical calculated arc distance target value 70-80mm. The arc stabilizing current is 25A DC, and the flash width is controlled to ≤12mm during the smelting process;

[0059] Step 4: After the primary smelting cooling furnace temperature is controlled at 300°C, the end face of the primary ingot is flattened and the surface of the primary ingot is peeled, with a peeling depth of 3mm;

[0060] Step 5: Dry the primary ingot at a temperature of 150°C for 4 hours;

[0061] Step 6: Turn the primary ingot around for finished product smelting. When the pre-vacuum reaches below 1.0Pa and the leakage rate is below 0.5Pa / min, a Φ720mm crucible is used for finished product smelting. The arc stabilization current for finished product smelting is 28A, the melting speed is set to 30kg / min, and the consumable electrode feed speed is set to 15mm / min. The theoretical calculated arc distance target value is 100mm through the adjustment of the melting speed and the consumable electrode feed speed, and the flash width is controlled to be ≤5mm during the smelting process.

[0062] Step 7: After the finished product is smelted, it is cooled and taken out of the furnace.

[0063] Block samples were taken from the head, middle and tail of the Φ720 mm ingot melted in this embodiment for analysis. The results of gas element sampling and detection at different parts of the Φ720 mm ingot are shown in Table 2:

[0064] Table 2.

[0065] Location O% N% H% head 0.041 0.003 0.001 Central 0.039 0.002 0.001 Tail 0.038 0.003 0.001

[0066] It can be seen from Table 2 that the oxygen content of the head, middle and tail of the Φ720 mm ingot can be stably controlled at a level of ≤ 0.05%, and the oxygen content of different positions of the ingot is evenly distributed without any increase in O.

[0067] Example 3

[0068] Step 1: Use GB / T 2524-2019 A Grade 0 or grade 0 titanium sponge, the oxygen content in the titanium sponge is 0.03% and the Cl content is 0.03%;

[0069] Step 2: Use a hydraulic press to press the titanium sponge into an electrode block of Φ400 mm, and use a welding box to weld the electrode block into a consumable electrode under an ambient humidity of 40%;

[0070] Step 3: Within 20 hours after the consumable electrode is pressed, when the pre-vacuum reaches below 1.0Pa and the leakage rate is below 0.05Pa / min, a Φ560mm crucible is used for primary smelting. The melting rate of the primary smelting is set to 20kg / min, and the feeding speed of the consumable electrode is set to 25-30mm / min. The theoretical calculated arc distance target value is 30-40mm through the adjustment of the melting speed and the feeding speed of the consumable electrode. The arc stabilization current adopts 15A DC, and the flash width is controlled to be ≤10mm during the smelting process;

[0071] Step 4: After the primary smelting is cooled and taken out of the furnace, the end face of the primary ingot is flattened and the surface of the primary ingot is peeled, with a peeling depth of 5 mm;

[0072] Step 5: Dry the primary ingot at a temperature of 150°C for 8 hours;

[0073] Step 6: Turn the primary ingot around for finished product smelting. When the pre-vacuum reaches below 1.0Pa and the leakage rate is below 0.5Pa / min, a Φ640mm crucible is used for finished product smelting. The arc stabilizing current for finished product smelting is 30A, the melting speed is set to 15-18kg / min, and the consumable electrode feed speed is set to 20mm / min. By adjusting the melting speed and the consumable electrode feed speed, the theoretical calculated arc distance target value is 30-40mm, and the flash width is controlled at ≤3mm during the smelting process.

[0074] Step 7: After the finished product is smelted, it is cooled and taken out of the furnace.

[0075] Block samples were taken from the head, middle and tail of the Φ640 mm ingot melted in this embodiment for analysis. The gas element sampling test results of different parts of the Φ640 mm ingot are shown in Table 3:

[0076] Table 3.

[0077] Location O% N% H% head 0.037 0.003 0.001 Central 0.039 0.002 0.001 Tail 0.040 0.003 0.001

[0078] It can be seen from Table 1 that the oxygen content in the head, middle and tail of the Φ640 mm ingot can be stably controlled at a level of ≤ 0.05%, without any increase in O.

[0079] Comparative Example 1:

[0080] The difference between Comparative Example 1 and Example 1 is that: in step 1, the Cl element content in the titanium sponge is 0.06%; in step 3, the melting rate is 16 kg / min, the consumable electrode feed speed is set to 25 mm / min, the theoretically calculated arc distance is 25 mm, and the flash width is not controlled; in step 4, the primary ingot is not subjected to skinning treatment.

[0081] The remaining steps are the same as those in Example 1.

[0082] It was found in the first smelting process that the vacuum was poor due to the selection of Cl element content of 0.06%, with an average value of about 5Pa, which was much higher than ≤0.7Pa in the embodiment. In addition, due to the short theoretical arc distance, the consumable electrode exerted too strong pressure on the molten pool, causing the molten pool to shake violently. The first ingot to the edge was very poor. Figure 3 As shown in the figure, the measurement shows that the molten pool is about 40mm wide and is in a serious state of not reaching the edge. Due to the moisture absorption caused by the failure to peel the ingot, the average vacuum degree during the smelting process of the finished product is about 2Pa.

[0083] After the finished ingot is smelted out of the furnace, block samples are taken from the head, middle and tail of the Φ640 mm ingot in Comparative Example 1 for analysis. The results of sampling and testing of gas elements at different parts of the ingot are shown in Table 4:

[0084] Table 4.

[0085] Location O% N% H% head 0.067 0.005 0.001 Central 0.073 0.003 0.001 Tail 0.075 0.004 0.002

[0086] It can be seen from Table 4 that the oxygen content of different parts of the pure titanium ingot produced by the conventional method exceeds 0.065%.

[0087] Comparative Example 2:

[0088] The difference between Comparative Example 2 and Example 3 is that: in step 2, the electrode pressing environment humidity is 65%; in step 3, the self-consumable power stage feeding speed is not set, the theoretically calculated arc distance is 120 mm, and the burr width is not controlled; in step 5, the primary ingot is not dried; in step 6, the self-consumable power stage feeding speed is not set, the theoretically calculated arc distance is 20 mm, and the burr width is not controlled.

[0089] During the first melting process, it was found that due to the pressing environment humidity of 65%, although the content of O and Cl elements in sponge titanium was very low, the vacuum degree during the first melting process was still relatively poor, with an average value of about 2.3Pa. Since the consumable electrode feed speed was not set during the first melting process, the arc distance during the actual melting process was 120mm, and the actual flash width was measured to be about 50mm. Figure 4 As shown, the arc distance during the secondary smelting process is 20 mm, and the actual flash width is measured to be approximately 20 mm.

[0090] After the finished ingot is smelted out of the furnace, block samples are taken from the head, middle and tail of the Φ640 mm ingot in Comparative Example 2 for analysis. The results of sampling and testing of gas elements at different parts of the ingot are shown in Table 5:

[0091] Table 5.

[0092] Location O% N% H% head 0.063 0.004 0.001 Central 0.070 0.005 0.001 Tail 0.067 0.003 0.002

[0093] It can be seen from Table 5 that the average oxygen content of different parts of the pure titanium ingot produced by the conventional method exceeds 0.065%.

[0094] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0095] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for smelting a low-oxygen content pure titanium ingot, characterized in that: The steps include: S1, using a hydraulic press to press the titanium sponge into an electrode block, and using a welding box to weld multiple electrode blocks into consumable electrodes; before using the hydraulic press to press the titanium sponge, the humidity in the environment is ≤ 60%; the titanium sponge in S1 is 0 A Grade 0 or grade 1, the oxygen content in the titanium sponge is ≤0.06%, and the Cl element content is ≤0.05%; S2. When the pre-vacuum is ≤1.0Pa and the leakage rate is ≤0.5Pa / min, the consumable electrode is melted once to obtain a primary ingot. During the melting process, the arc stabilizing current is controlled to be 10-25A DC. The arc distance range is controlled by adjusting the melting speed and the consumable electrode feed speed. During the primary melting process, the molten pool is controlled to reach the edge, the flash width is ≤20mm, and the arc distance range is 30-80mm. S3. After the primary ingot is cooled and taken out of the furnace, the end face of the primary ingot is flattened, and the surface of the primary ingot is peeled, and the peeling depth is ≥3mm; S4, drying the primary ingot at a temperature of 50-150°C for a drying time of ≥2h; S5. When the pre-vacuum is ≤1.0Pa and the leakage rate is ≤0.5Pa / min, the primary ingot is turned around for finished product smelting, and the arc stabilizing current is 10-30A. During the smelting process, the arc distance range is controlled by adjusting the melting speed and the consumable electrode feed speed; during the finished product smelting process, the molten pool is controlled to the edge, and the flash width is ≤5mm; the arc distance range is 30-100mm; S6. After the finished product is smelted, it is cooled and taken out of the furnace.

2. The method for smelting a low-oxygen-content pure titanium ingot according to claim 1, characterized in that: The time period from the completion of pressing the titanium sponge into the electrode block to the start of the first smelting of the consumable electrode is ≤ 24 hours.

3. The smelting method of a low-oxygen content pure titanium ingot according to claim 1, characterized in that: In S2, before the first smelting, the diameter ratio of the consumable electrode to the crucible is ≤4 / 5; in S6, before the finished product smelting, the diameter ratio of the consumable electrode to the crucible is ≤7 / 8.

4. The method for smelting a low-oxygen content pure titanium ingot according to claim 1, characterized in that: During the primary smelting process of S2, the melting rate is 10-20 kg / min, and the feeding speed of the consumable electrode is 10-30 mm / min; during the finished product smelting process of S5, the melting rate is 15-30 kg / min, and the feeding speed of the consumable electrode is 2-20 mm / min.