A rapid medium-temperature carbonitriding process for alloy carburizing steel gears
Through the rapid medium-temperature carbonitriding process, the problems of high temperature, long time and surface defects of traditional carbonitriding treatment are solved, and the high hardness and wear resistance of alloy carburized steel gears are achieved, which is suitable for a variety of gear materials.
Patent Information
- Application Number
- CN202211477457.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-11-23
AI Technical Summary
Traditional carbonitriding treatment has problems such as high temperature, long time, and difficult to control surface defects such as oxidation and non-martensitic structure in the surface layer, resulting in a decrease in the mechanical properties of the gear.
The rapid medium-temperature carbonitriding process of alloy carburized steel gears is used to form Dispersed nano-sized carbonitride compounds control the level and transfer speed of carbonitride compounds and reduce surface defects.
Significantly improve the surface hardness and wear resistance of the gear, reduce the processing temperature and time, control the level of carbonitride and surface defects, and achieve a high hardness and high wear resistance gear surface, suitable for 20CrMnTi, 8620 and other materials Gear parts.
Smart Images

Figure CN115852300B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of heat treatment of metal materials and relates to a rapid medium-temperature carbonitriding process for alloy carburizing steel gears. Background Art
[0002] Automobile transmission gears are core components that connect the engine to drive the wheels, and they are responsible for transmitting stress. Gears transmit power through the contact of tooth surfaces, so the tooth surfaces are often in a complex working environment with high contact stress, friction, alternating stress, and impact stress, which leads to tooth surface contact fatigue, bending fatigue, pitting and fracturing as the main failure forms of gear parts, significantly reducing the service life of gear parts. Therefore, how to obtain high hardness and high wear resistance on the gear surface is the key to ensuring the working reliability and long service life of the gear. Surface chemical heat treatments such as surface carburizing and carbonitriding have become the main means to improve the surface structure and service performance of gears.
[0003] At present, conventional gear carburizing processes are carried out at 920-940°C. On the one hand, the treatment temperature is high, which is not conducive to controlling the heat treatment deformation of the gear. On the other hand, it requires a long treatment time. For example, if a 1mm thick carburized layer is required, it generally takes about 12-15 hours to process. It can be seen that the carburizing treatment temperature is high, and it is difficult to control the heat treatment deformation and the cost is high. The carbonitriding process can significantly reduce the chemical heat treatment temperature and time of the gear. At the same time, due to the infiltration of nitrogen atoms, it can effectively improve the hardenability and hardness of the alloy and retain sufficient toughness.
[0004] However, the traditional carbonitriding treatment has a slow penetration rate of carbon and nitrogen atoms, and is often prone to surface defects such as surface oxidation and non-martensitic structure. At present, it is still difficult to control the thickness of non-martensitic structure on the surface of carburized steel gears, and it is easy to cause agglomeration and abnormal coarsening of carbon and nitrogen compounds, reducing the mechanical properties of steel gears. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention proposes a rapid medium-temperature carbonitriding process for alloy carburizing steel gears, which not only reduces the temperature and shortens the time of the carbonitriding treatment, but also realizes the rapid penetration of carbon and nitrogen atoms on the gear surface and forms dispersed nano-sized carbonitriding compounds on the surface of the carburizing steel gear, thereby significantly improving the surface hardness of the carburizing steel gear (the hardness is as high as 65-67HRC after quenching in oil, and the hardness can be maintained at 62-64HRC after tempering at 170°C for 3 hours), wear resistance and fatigue resistance.
[0006] The present invention is achieved through the following technical solutions:
[0007] A rapid medium-temperature carbonitriding process for alloy carburizing steel gears comprises the following steps:
[0008] S1, heat treating the alloy carburizing steel gear in a carbon-nitrogen atmosphere for 0.5-1.5 h under a condition below the critical temperature of austenitization to obtain a pretreated alloy carburizing steel gear;
[0009] S2, subjecting the pretreated alloy carburizing steel gear to the following carbonitriding process at 840-880° C. in a carbonitriding atmosphere to complete rapid medium-temperature carbonitriding of the alloy carburizing steel gear;
[0010] When the thickness of the infiltrated layer d1 is less than 0.7 mm, the carbonitriding process is a strong infiltration process, and the strong infiltration time t1 satisfies the following relationship: 2≤t1<4h;
[0011] When the thickness of the infiltration layer d2 satisfies the following relationship: 0.7≤d2<1.2mm, the carbonitriding process is first strong infiltration and then diffusion, and the total time t2 satisfies the following relationship: 4≤t2<10h, and the strong infiltration time is the same as the diffusion time;
[0012] When the thickness of the carburized layer d3 satisfies the following relationship: 1.2≤d3<1.5mm, the carbonitriding process is to perform strong carburization first and then diffuse to obtain an alloy carburized steel gear after one strong carburization-diffusion, and then the alloy carburized steel gear after the one strong carburization-diffusion is subjected to strong carburization again and then diffused to obtain an alloy carburized steel gear after the second strong carburization-diffusion, and the total time t3 of the two strong carburization-diffusions satisfies the following relationship: 10≤t3<14h, and finally the alloy carburized steel gear after the two strong carburization-diffusions is subjected to strong carburization for 10-30min.
[0013] Furthermore, the alloy carburizing steel gear described in S1 is pretreated at 680-720°C.
[0014] Furthermore, the carbon-nitrogen atmosphere described in S1 and S2 is a mixed atmosphere formed by ammonia and gas obtained by cracking liquid ethanol or gas obtained by cracking liquid methanol.
[0015] Furthermore, during the heat treatment of the alloy carburizing steel gear described in S1, the volume of ammonia when the mixed atmosphere is input accounts for 50%-75% of the total volume of the mixed atmosphere, and the volume of residual ammonia in the mixed atmosphere during the heat treatment process accounts for 6%-10%.
[0016] Furthermore, in S2, when the thickness of the diffusion layer d1 is less than 0.7 mm, the carbon potential in the carbonitriding process is 0.9%-1.2%, and the nitrogen potential is 0.1%-0.3%.
[0017] Furthermore, in S2, when the thickness d2 of the diffusion layer satisfies the following relationship: 0.7≤d2<1.2mm, the carbon potential of the strong diffusion in the carbonitriding process is 0.9%-1.1%, the nitrogen potential is 0.2%-0.3%, the diffused carbon potential is 0.7%-0.9%, and the nitrogen potential is 0.15%-0.25%.
[0018] Furthermore, in S2, when the thickness of the diffusion layer d3 satisfies the following relationship: 1.2≤d3<1.5mm, the carbon potential and nitrogen potential of the strong diffusion in the first strong diffusion-diffusion, and the carbon potential and nitrogen potential of the diffusion are the same as the carbon potential and nitrogen potential corresponding to the diffusion layer thickness d2.
[0019] Furthermore, in S2, when the thickness d3 of the diffusion layer satisfies the following relationship: 1.2≤d3<1.5mm, the carbon potential of the second strong diffusion is 0.9%-1.0%, and the nitrogen potential is 0.05%-0.15%, and the carbon potential and nitrogen potential of the diffusion are the same as those of the first diffusion.
[0020] Furthermore, in S2, when the thickness of the diffusion layer d3 satisfies the following relationship: 1.2≤d3<1.5mm, the first strong diffusion time t b1 , diffusion time t d1 , and the second strong penetration-diffusion time t b2 , diffusion time t d2 Satisfies the following relationship: b2 =0.5t b1 ; 0.5t d1 ≤t d2 ≤1.5t d1 .
[0021] Furthermore, the carbon potential of the alloy carburized steel gear after the double carburization-diffusion described in S2 is 0.85%-1.0% and the nitrogen potential is 0.1%-0.2% after 10-30 minutes of carburization.
[0022] Compared with the prior art, the present invention has the following beneficial technical effects:
[0023] The invention discloses a rapid medium-temperature carbonitriding process for alloy carburizing steel gears. The process comprises: performing strong carburizing on a carburizing layer (d1 < 0.7 mm), and forming dispersed carbonitride compounds on the surface of the alloy carburizing steel gears. The process comprises performing strong carburizing on a medium carburizing layer (0.7 ≤ d2 < 1.2 mm) and then diffusing the same, and forming dispersed granular carbonitride compounds on the surface of the alloy carburizing steel gears. The process comprises performing two strong carburizing-diffusion cycle treatment processes and a final short-time strong carburizing on a thicker carburizing layer (1.2 ≤ d3 < 1.5 mm). The first cycle of strong infiltration and diffusion treatment can control the carbonitrides to not be abnormally coarsened, and its metallographic level is ≤ level 5. After the second cycle of strong infiltration and diffusion treatment, the level of carbonitrides can be controlled to ≤ level 4. At the same time, the transfer speed of active carbon and nitrogen atoms in alloy carburizing steel gears is improved, and a high infiltration rate is maintained. It also effectively reduces surface oxidation and surface non-martensitic structure thickness, and inhibits the formation and abnormal coarsening of continuous coarse carbonitrides at grain boundaries, thereby obtaining dispersed carbonitrides on the workpiece surface and obtaining a gear workpiece with high surface hardness and high wear resistance. The present invention can obtain a thicker penetration layer depth in a relatively short time. For example, after treatment at 880°C for 6 hours, an effective hardened layer (550HV1) with a thickness of 1.03mm and 0.84mm can be obtained at the pitch circle and tooth root of a 20CrMnTi gear respectively; after treatment at 880°C for 9.6 hours, a penetration layer with a thickness of 1.18mm can be obtained on the surface of an 8620RH gear. The treated sample can obtain high surface hardness and high wear resistance, and its surface hardness is as high as 793HV 0.5 (measured at 0.1mm), subsurface hardness up to 821HV 0.5 (Measured value at 0.2mm). Compared with conventional carburizing treatment, the present invention reduces the treatment temperature from 930℃ to 840-880℃, significantly reduces the treatment temperature (reduced by 50-90℃), and reduces deformation. The present invention is also suitable for alloy steel gear parts made of materials such as 20CrMo, 8620, 20Cr and 20MnCr5. The limit thickness of the carburized layer obtained by the traditional carbonitriding treatment process is about 0.7-0.8mm. The present invention adopts two strong carburizing-diffusion cycle treatment processes and short-time strong carburizing for thicker carburized layers, and realizes a fast medium-temperature (840-880℃) carbonitriding process for obtaining a thicker carburized layer (1.2-1.5mm) on the surface of a large-module gear. The carburizing rate is equivalent to that of an ordinary carburizing process at 920℃, and is easy to operate and easy to implement. It significantly reduces the treatment temperature and shortens the treatment time. It has a carburizing rate equivalent to that of a 920℃ carburizing treatment, and therefore has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1a This is a surface microstructure diagram of a tooth block made of 20CrMnTi material corresponding to Example 1 of the present invention after carbonitriding + tempering at 860°C / 9h at a metallographic magnification of 100 times.
[0025] Figure 1b This is a surface microstructure diagram of a tooth block made of 20CrMnTi material corresponding to Example 1 of the present invention after carbonitriding + tempering at 860°C / 9h at a metallographic magnification of 1000 times.
[0026] Figure 2 This is a surface microstructure diagram of the tooth block made of 8620RH material corresponding to Example 2 of the present invention after carbonitriding + tempering at 880°C / 9.6h at a metallographic magnification of 500 times.
[0027] Figure 3a This is a microstructure diagram of the tooth root position of the tooth block made of 20CrMnTi material corresponding to Example 4 of the present invention after 880°C / 6h carbonitriding + tempering at 1000 times the metallographic magnification.
[0028] Figure 3b This is a microstructure diagram of the pitch circle position of the tooth block made of 20CrMnTi material corresponding to Example 4 of the present invention after 880°C / 6h carbonitriding + tempering at a metallographic magnification of 1000 times.
[0029] Figure 4 This is a surface microstructure diagram of a tooth block made of 20CrMnTi material corresponding to Example 5 of the present invention after carbonitriding + tempering at 880°C / 13.5h at a metallographic magnification of 500 times. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0031] Compared with ordinary carburizing, medium-temperature carbonitriding has the advantages of low treatment temperature, good hardenability, good wear resistance and tempering stability, and small gear distortion after treatment. However, it is easy to have three black structural defects, which are actually non-martensitic structures of different forms in the surface layer, resulting in a significant reduction in gear fatigue strength and service life.
[0032] The present invention proposes a rapid medium-temperature carbonitriding process for alloy carburizing steel gears, comprising the following steps:
[0033] Step 1: Pretreatment below the critical temperature of austenitization (abbreviated as AC1);
[0034] When the carburizing furnace is heated to 680-720°C, a mixed atmosphere formed by the gas after cracking of ammonia and liquid ethanol or the gas after cracking of liquid methanol is introduced into the carburizing furnace, and the alloy carburizing steel gear is placed in the carburizing furnace. 1 mol of liquid ethanol or liquid methanol is cracked in the carburizing furnace, each producing 1 mol of CO. The alloy carburizing steel gear is treated in the mixed atmosphere for 0.5-1.5h. The volume of ammonia in the mixed atmosphere when it is input accounts for 50%-75% of the total volume. During the heat treatment process, the residual ammonia in the atmosphere in the carburizing furnace accounts for 6%-10% of the total volume.
[0035] Methanol cracking reaction formula: CH3OH→CO+2H2;
[0036] Ethanol decomposition reaction formula: C2H5OH→CO+3H2+[C].
[0037] Step 2: Medium temperature carbonitriding treatment;
[0038] The pre-treated alloy carburizing steel gear is placed in a carburizing furnace at 840-880°C, and continues to be subjected to medium-temperature carbonitriding treatment in the above-mentioned mixed atmosphere.
[0039] For gears with shallow infiltration layer (d1<0.7mm), after intensive infiltration for 2≤t<4h, subsequent quenching in oil can be carried out after coming out of the furnace; for gears with medium infiltration layer (0.7≤d2<1.2mm), they need to undergo diffusion treatment after intensive infiltration and then subsequent quenching in oil can be carried out after coming out of the furnace; for gears with thicker infiltration layer (1.2≤d3<1.5mm), a cyclic intensive infiltration-diffusion process is required, and then subsequent quenching in oil can be carried out after coming out of the furnace.
[0040] For gears with shallow carburization, the carbon potential C p is the carbon activity α c =0.9 Carbon content corresponding to the treatment temperature (%); Carbon potential C p =0.9%-1.2%, nitrogen potential N p =0.1%-0.3%.
[0041] The process of strong penetration-diffusion of gears with medium penetration layer is as follows: the treatment time is 4≤t<10h, and the carbon potential C p =0.9%-1.1%, N p =0.2%-0.3%; Carbon potential C in the furnace during diffusion p =0.7%-0.9%, N p =0.15%-0.25%; strong penetration time (t b1 ) and diffusion time (t d1 ) is 1.
[0042] For gears with thicker infiltration layers, the cycle of strong infiltration-diffusion process time is 10≤t<14h. The process parameters of the first strong infiltration-diffusion are the same as those of the gears with medium infiltration layers mentioned above. The C of the strong infiltration during the second strong infiltration-diffusion is p =0.9%-1.0%, N p =0.05%-0.15%, the carbon potential and nitrogen potential during diffusion are the same as the first diffusion parameters, among which the strong penetration time (t b2 ) and diffusion time (t d2 ) are: t b2 =0.5t b1 ; 1.5t d1 ≧t d2 ≧0.5t d1 Before being taken out of the furnace, it can be strongly impregnated again for a short time (10-30 minutes) with a carbon potential of 0.85%-1.0% and a nitrogen potential of 0.1%-0.2% to avoid surface carbon and denitrification.
[0043] In the subsequent process, the alloy carburizing steel gears after carbonitriding treatment must be quenched and then tempered before they can be used normally. The temperature, time and other parameters used for quenching and tempering are all conventional.
[0044] Embodiment 1:
[0045] (1) Pretreatment:
[0046] A gear made of 20CrMnTi with a half-tooth width of 15 mm was selected, the carburizing furnace was heated to 680°C, 60% ammonia and 7.5% residual ammonia were introduced, and the gear block was placed in the carburizing furnace for 1 hour.
[0047] It should be noted that the process of the present invention is applicable to gears of all shapes and specifications, and this embodiment is just a specific example.
[0048] (2) Medium temperature carbonitriding composite treatment:
[0049] First, continue to heat the carburizing furnace to 860℃, carbon potential 1.0%, nitrogen potential 0.3%, and strong carburizing treatment for 4.5h; secondly, continue diffusion treatment for 4.5h, carbon potential 0.7%, nitrogen potential 0.15%, then take out of the furnace and quench in oil. Then carry out conventional tempering treatment, 160℃ / 1h, air cooling, and then it can be put into use.
[0050] The thickness of the carburized layer at the pitch circle of the gear block is 1.05 mm, the thickness of the non-martensitic structure on the surface is 11 μm, and the surface layer forms dispersed granular carbonitrides (white particles) with an average size of about 300 nm. The carbonitride grade is 1; the hidden needle martensite is obtained with an average size of less than 2 μm, and the metallographic structure belongs to grade 1. Figure 1a and Figure 1b shown.
[0051] Embodiment 2:
[0052] (1) Select a gear block made of 8620RH material, heat the carburizing furnace to 700℃, introduce 75% ammonia and 10% residual ammonia, and place the gear block in the carburizing furnace for 1.5 hours.
[0053] (2) Medium temperature carbonitriding composite treatment:
[0054] Continue to raise the carburizing furnace temperature to 880℃, carbon potential 1.1%, nitrogen potential 0.2%, and strong carburizing treatment for 4.8h. After strong carburizing, continue to adjust the atmosphere ratio in the furnace and start diffusion treatment: carbon potential 0.9%, nitrogen potential 0.2%, keep warm for 4.8h, that is, a total treatment of 9.6h, and quench oil after taking out of the furnace. Then carry out tempering treatment, 160℃ / 1h, air cooling.
[0055] The thickness of the carburized layer can be 1.18mm and 1.05mm at the pitch circle and tooth root respectively, and the surface hardness is as high as 793HV. 0.5 (measured at 0.1mm), subsurface hardness up to 821HV 0.5 (Measurement value at 0.2mm). Dispersed carbonitrides are formed on the surface, with an average size of about 550nm, a metallographic grade of 1, a thickness of 10μm on the surface non-horsepower structure, and a grade of 1 residual austenite. Figure 2 shown.
[0056] Embodiment 3:
[0057] (1) Select a gear block made of 20CrMnTi, heat the carburizing furnace to 690°C, introduce 50% ammonia and 6% residual ammonia, and place the gear block in the carburizing furnace for 0.5 h.
[0058] (2) Medium temperature carbonitriding treatment:
[0059] The carburizing furnace was heated to 880℃, carbon potential 0.9%, nitrogen potential 0.3%, and kept at this temperature for 3.5h before being quenched in oil. Then tempering treatment was carried out at 160℃ / 1h and air cooling. A carburized layer with a thickness of 0.68mm was obtained on the surface of the 20CrMnTi gear.
[0060] Embodiment 4:
[0061] (1) Select a bevel gear tooth block made of 20CrMnTi material, heat the Aixilin box-type multi-purpose furnace (furnace chamber size 800×1800×900mm, the furnace actually used in enterprise production, with the same function as the carburizing furnace) to 720°C, introduce ammonia gas accounting for 70% and residual ammonia 9%, and put the tooth block into the Aixilin box-type multi-purpose furnace for 45 minutes;
[0062] (2) Medium temperature carbonitriding treatment:
[0063] Continue to heat the Aixilin box-type multi-purpose furnace to 880℃, carbon and nitrogen 1.05%, nitrogen potential 0.25%, strong penetration for 3h; continue to diffuse treatment, carbon and nitrogen 0.85%, nitrogen potential 0.15%, keep warm for 3h before taking out of the furnace and quenching oil. Then carry out tempering treatment, 170℃ / 3h, air cooling.
[0064] The carburized layer with a thickness of 1.03mm and 0.84mm can be obtained at the gear pitch circle and tooth root respectively. The surface layer forms a dispersed carbonitride, the average size of the compound particles is 500nm, and the metallographic level is level 1; the thickness of the surface non-martensite structure is 13-17μm; the surface layer has hidden needle martensite, and the metallographic level is level 1-2. Figure 3a and Figure 3b shown.
[0065] Embodiment 5:
[0066] (1) Select a gear block made of 20CrMnTi, heat the carburizing furnace to 700°C, introduce 68% ammonia and 8% residual ammonia, and place the gear block in the carburizing furnace for 1 hour;
[0067] (2) Continue to raise the temperature of the carburizing furnace to 880°C, with a carbon potential of 1.05%, a nitrogen potential of 0.2%, and a strong carburizing for 4 hours; continue to perform diffusion treatment, with a carbon potential of 0.8%, a nitrogen potential of 0.25%, and a diffusion treatment for 4 hours;
[0068] (3) Then, the steel was subjected to strong permeation treatment for 2 hours, with a carbon potential of 1.0% and a nitrogen potential of 0.15%; diffusion treatment for 3 hours, with a carbon potential of 0.7% and a nitrogen potential of 0.15%; finally, in order to prevent surface decarburization and denitrification, the steel was subjected to strong permeation for 0.5 hours, with a carbon potential of 0.9% and a nitrogen potential of 0.15%. After a total treatment of 13.5 hours, the steel was taken out of the furnace and quenched in oil. Then, tempering treatment was carried out at 160°C / 1 hour, followed by air cooling.
[0069] A 1.4mm thick carburized layer can be obtained on the gear surface. The surface layer has dispersed spherical carbonitrides with an average size of 750nm and a metallographic grade of 1. The thickness of the non-martensite on the surface is 15-18μm. There is needle-shaped martensite on the surface, and its metallographic grade is 1-2. Figure 4 shown.
[0070] Embodiment 6:
[0071] (1) Select a gear block made of 20CrMnTi, heat the carburizing furnace to 700°C, introduce 65% ammonia and 8.5% residual ammonia, and place the gear block in the carburizing furnace for 1 hour;
[0072] (2) Continue to raise the carburizing furnace temperature to 840℃, carbon potential 1.2%, nitrogen potential 0.1%, and intensive carburizing for 2h; then perform tempering treatment at 160℃ / 1h and air cooling. A carburized layer with a thickness of 0.35mm can be obtained on the gear surface.
Claims
1. A rapid medium-temperature carbonitriding process for alloy carburizing steel gears, characterized in that: The following steps are involved: S1, heat treating the alloy carburizing steel gear in a carbon-nitrogen atmosphere for 0.5-1.5 h under a condition below the critical temperature of austenitization to obtain a pretreated alloy carburizing steel gear; S2, subjecting the pretreated alloy carburizing steel gear to the following carbonitriding process at 840-880° C. in a carbonitriding atmosphere to complete rapid medium-temperature carbonitriding of the alloy carburizing steel gear; When the thickness of the infiltrated layer d1 is less than 0.7 mm, the carbonitriding process is a strong infiltration process, and the strong infiltration time t1 satisfies the following relationship: 2≤t1<4h, the carbon potential is 0.9%-1.2%, and the nitrogen potential is 0.1%-0.3%; When the thickness of the carbonitriding layer d2 satisfies the following relationship: 0.7≤d2<1.2mm, the carbonitriding process is first strong penetration and then diffusion, the carbon potential of strong penetration is 0.9%-1.1%, the nitrogen potential is 0.2%-0.3%, the carbon potential of diffusion is 0.7%-0.9%, the nitrogen potential is 0.15%-0.25%, and the total time t2 satisfies the following relationship: 4≤t2<10h, and the strong penetration time is the same as the diffusion time; When the thickness of the carburizing layer d3 satisfies the following relationship: 1.2≤d3<1.5mm, the carbonitriding process is to perform strong carburizing first and then diffuse, the carbon potential and nitrogen potential of the strong carburizing, as well as the carbon potential and nitrogen potential of the diffused carbon potential and nitrogen potential are the same as the carbon potential and nitrogen potential corresponding to the thickness of the carburizing layer d2, and an alloy carburizing steel gear after one strong carburizing-diffusion is obtained, and then the alloy carburizing steel gear after one strong carburizing-diffusion is subjected to strong carburizing again and then diffused, the carbon potential of the strong carburizing is 0.9%-1.0%, and the nitrogen potential is 0.05%-0.15%, and the carbon potential and nitrogen potential of the diffused carbon potential and nitrogen potential are the same as the carbon potential and nitrogen potential of the first diffusion, and an alloy carburizing steel gear after a second strong carburizing-diffusion is obtained, and the total time t3 of the two strong carburizing-diffusions satisfies the following relationship: 10≤t3<14h, and the strong carburizing time t in the first strong carburizing-diffusion is t b1 , diffusion time t d1 , and the second strong penetration-diffusion time t b2 , diffusion time t d2 Satisfies the following relationship: b2 =0.5t b1 ; 0.5t d1 ≤t d2 ≤1.5t d1 Finally, the alloy carburized steel gear after two strong infiltration and diffusion processes was subjected to strong infiltration for 10-30 minutes, with a carbon potential of 0.85%-1.0% and a nitrogen potential of 0.1%-0.2%.
2. The rapid medium temperature carbonitriding process for alloy carburizing steel gears according to claim 1, characterized in that: The alloy carburized steel gears described in S1 were pre-treated at 680-720°C.
3. The rapid medium temperature carbonitriding process for alloy carburizing steel gears according to claim 1, characterized in that: The carbon-nitrogen atmosphere described in S1 and S2 is a mixed atmosphere formed by ammonia and gas obtained by cracking liquid ethanol or gas obtained by cracking liquid methanol.
4. The rapid medium temperature carbonitriding process for alloy carburizing steel gears according to claim 3, characterized in that: When the alloy carburizing steel gear described in S1 is heat treated, the volume of ammonia accounts for 50%-75% of the total volume of the mixed atmosphere when the mixed atmosphere is input, and the volume of residual ammonia in the mixed atmosphere during the heat treatment process accounts for 6%-10%.