A contact parts cleaning process
By using a combination process of pickling liquid, light-vibration liquid and anti-copper discoloration treatment on copper and copper alloy contact parts, the problem of the inability to remove oxide films and welding slag in the prior art is solved, ensuring the protection of silver contacts and Environmentally friendly, meets the control requirements of RoHS and silicones, and achieves efficient cleaning results.
Patent Information
- Application Number
- CN202211411522.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-11
AI Technical Summary
The prior art cannot effectively remove the oxide film, welding slag and copper color on the surface of copper and copper alloy contact parts, and at the same time it cannot ensure that the silver contacts are not corroded, and cannot take into account both RoHS and silicone control requirements.
The pickling solution (a mixture of hydrogen peroxide and dilute sulfuric acid) at room temperature removes the oxide film and copper color, and then use the shaking liquid to remove the welding slag, and form a protective film through acid activation and anti-copper discoloration treatment, and finally performs multi-stage Wash against the flow and scald hot water to ensure clean and dryness.
The oxide film, welding slag and copper color on the surface of the contact parts were successfully removed, which prevented the corrosion of silver contacts and met the control requirements of RoHS and silicones. The resulting product was smooth, dry and compliant with environmental standards.
Smart Images

Figure CN115852380B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cleaning process, in particular to a contact component cleaning process. Background Art
[0002] At present, a contact component of the prior art includes a substrate and a silver contact welded on the substrate, wherein the substrate is copper or a copper alloy, and is brazed with the silver contact to form a component. Because the temperature during the brazing process is as high as 800°C, and the component is cooled by water cooling after welding, the surface of the component is severely oxidized due to water stains, and welding slag remains. The surface of the brass component also has an obvious pure copper color due to the zinc reaction, so it needs to be cleaned. In the traditional strong pickling process, a mixture of sulfuric acid and nitric acid is usually used for cleaning. Although it can remove the oxide film, welding slag and replacement copper color on the surface of the copper and copper alloy components welded by the silver contact, it also has a corrosive effect on the silver contact and changes the size of the contact welding component. In addition, after strong pickling, because copper and copper alloys need to rely on chromic anhydride leaching solution to remove the film (the black film layer produced after the strong acid reacts with copper and copper alloys) to restore the copper color, it does not meet the RoHS control requirements. The environmentally friendly weak pickling process launched on the market in recent years uses a weak acid cleaning agent, and the acidity of the cleaning solution is weak, so it cannot completely remove the severe oxide film, welding slag and copper color on the surface of the parts.
[0003] The Chinese invention patent No. 201010110076.1 discloses a pollution-free bright pickling process for copper and brass parts, which comprises mixing 45%-55% of hydrogen peroxide with a mass fraction of 30%, 4%-6% of D11 stabilizer, 0.4%-0.6% of sulfuric acid with a density of 1.84 g / ml, and 39.4%-50.6% of water to prepare a pickling solution, adding the pickling solution into a pickling tank and heating it to 44°C-46°C, keeping the temperature constant, and performing bright pickling. Then, the pickling solution on the surface of the copper and brass parts is cleaned with running water, and a film remover is prepared by mixing D11 brightener and water in a volume ratio of 1:1 to perform bright film removal, thereby achieving the purpose of removing the oxide film on the surface of the copper and brass parts and maintaining brightness. Although this process is suitable for copper and brass parts, it is not suitable for welding copper or copper alloys with silver contacts. It cannot ensure that the silver contacts will not be corroded, nor can it take into account the product's RoHS control requirements and silicone control requirements. Summary of the invention
[0004] In view of the technical problems existing in the prior art, the present invention provides a contact component cleaning process, which can not only remove the oxide film layer, welding slag and copper color on the surface of copper and copper alloy components, and prevent the welded components from re-oxidation and discoloration after cleaning, but also ensure that the silver contacts are not corroded, while taking into account the RoHS control requirements and silicone control requirements of the product.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a contact component cleaning process, the contact component comprises a substrate and a silver contact welded on the substrate, the substrate comprises copper and / or copper alloy; the cleaning process comprises the following steps:
[0006] (1) Pickling to remove oxide film and copper color: Immerse the contact parts in a pickling solution for pickling at room temperature for 10-15 seconds; the components and volume percentages of the pickling solution are: 4%-6% of 30% hydrogen peroxide, 8%-12% of dilute sulfuric acid with a density of 1.84 g / ml, and the balance is water;
[0007] (2) Vibration treatment to remove solder slag: a pre-prepared grinding liquid, brightener and water are mixed in a preset ratio to form a vibration treatment liquid, and the contact parts obtained in step (1) are subjected to vibration treatment at room temperature for 20-40 minutes;
[0008] (3) Acid activation: The contact components obtained in step (2) are cleaned with a 5% to 10% dilute sulfuric acid aqueous solution for 10 to 15 seconds to remove the acid wash solution remaining on the surface of the contact components;
[0009] (4) Anti-copper discoloration treatment: The contact parts obtained in step (3) are immersed in a 20%-25% aqueous solution of OY-8A anti-copper discoloration agent for 1-2 minutes to form a protective film on the surface thereof;
[0010] Furthermore, in step (2), the proportions of the components in each liter of the vibration liquid are as follows: 10-15 mL / L of grinding liquid, 10-15 mL / L of brightener, and the balance is water; the components and volume percentages of the grinding liquid are: 10%-20% of sodium dodecylbenzene sulfonate, 5%-15% of citric acid, 15%-25% of sodium carbonate, 10%-20% of sodium metasilicate, 20%-30% of fatty alcohol, and 10%-20% of castor oil; the components and volume percentages of the brightener are: 30%-40% of sodium dodecylbenzene sulfonate, 5%-15% of glycerol, 15%-25% of nonylphenol polyoxyethylene ether, 5%-15% of SLS needle-shaped multi-effect active agent, and 20%-30% of fatty alcohol polyoxyethylene ether.
[0011] Furthermore, the components and volume percentages of the grinding liquid are: 15% sodium dodecylbenzene sulfonate, 10% citric acid, 20% sodium carbonate, 15% sodium metasilicate, 25% fatty alcohol, and 15% castor oil; the components and volume percentages of the brightener are: 35% sodium dodecylbenzene sulfonate, 10% glycerol, 20% nonylphenol polyoxyethylene ether, 10% SLS needle-shaped multi-effect active agent, and 25% fatty alcohol polyoxyethylene ether.
[0012] Furthermore, the method further comprises step (5): washing the contact parts obtained in step (4) in sequence to remove water stains.
[0013] Furthermore, the water washing process in step (5) includes multiple stages of countercurrent water washing and hot water scalding in sequence, the time of each stage of countercurrent water washing is 5-10s, the time of hot water scalding is 10-30s, and the temperature of the hot water is greater than or equal to 80°C.
[0014] Furthermore, in step (5), the process for removing water stains includes hot air drying and drying in sequence, wherein the temperature of hot air drying is 60°C-70°C, the temperature of drying is 70°C-80°C, the drying time is 20-30s, and the drying time is 20-40min.
[0015] Furthermore, in the steps (1) to (3), the contact parts are washed with water after each step is completed, and the washing process is implemented by a multi-stage countercurrent washing process.
[0016] Furthermore, the step (1) also includes a chemical degreasing step: immersing the contact parts in a 10%-15% HMC-02A degreasing aqueous solution for 10-15 minutes; and washing the contact parts with water after the degreasing is completed.
[0017] Furthermore, the water washing after the chemical degreasing step is achieved by a multi-stage countercurrent water washing process.
[0018] Furthermore, the components and volume percentages of the pickling solution are: 5% of 30% by mass hydrogen peroxide, 10% of dilute sulfuric acid with a density of 1.84 g / ml, and the balance is water.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention uses the pickling solution prepared by the hydrogen peroxide and dilute sulfuric acid to replace the mixed solution of sulfuric acid and nitric acid in the traditional strong pickling process for cleaning, which can remove the severe oxide film layer on the contact surface and the pure copper color on the surface of the brass component while ensuring that the silver contact is not corroded; the present invention uses the vibrating light liquid to perform vibrating light treatment on the pickled contact component, which can remove the welding slag on the surface of the contact component and make the surface of the contact component cleaner and smoother; the present invention performs acid activation on the contact component, which can ensure that there is no residue of the hydrogen peroxide pickling solution with strong oxidizing property on the surface of the contact component, and then performs anti-copper discoloration treatment to form a protective film on the surface of the contact component, thereby improving the protective performance of the component surface, and taking into account the RoHS control requirements and silicone control requirements of the product, so that the cleaning process is more harmless and pollution-free.
[0021] 2. The present invention also includes the step (5), which can remove the substances remaining in the contact parts in step (4) on the one hand, and can dry the contact parts on the other hand to avoid residual water stains, and finally obtain a smooth and dry product.
[0022] 3. In the steps (1) to (3), the contact parts are washed with water after each step is completed, which can prevent the residual cleaning materials from the previous process from affecting the next process. In particular, the washing process adopts a multi-stage countercurrent washing process, which can better clean the residual materials on the contact parts after the previous process.
[0023] 4. The step (1) also includes a chemical degreasing step, which can remove the oil stains on the surface of the contact parts and completely expose the surface of the contact parts to facilitate comprehensive pickling.
[0024] 5. The present invention can realize batch cleaning operations of contact parts, thereby facilitating batch production of contact parts.
[0025] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments; however, a contact component cleaning process of the present invention is not limited to the embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a comparative schematic diagram of a contact part before and after being cleaned by the cleaning process of the present invention;
[0027] Figure 2 It is a RoHs and silicone test report after the contact parts are cleaned by the cleaning process of the present invention. DETAILED DESCRIPTION
[0028] A contact component cleaning process of the present invention comprises a substrate and a silver contact welded on the substrate, wherein the substrate comprises copper and / or a copper alloy; the cleaning process comprises the following steps:
[0029] (1) Pickling to remove oxide film and copper color: prepare a pickling solution, the components and volume percentages of which are: 4%-6% of 30% hydrogen peroxide, 8%-12% of dilute sulfuric acid with a density of 1.84 g / ml, and the balance is water; immerse the contact parts in the pickling solution for pickling at room temperature for 10-15 seconds; after the pickling is completed, wash the contact parts with water;
[0030] (2) Vibration treatment to remove solder slag: a pre-prepared grinding liquid, brightener and water are mixed in a preset ratio to form a vibration treatment liquid, and the contact parts obtained in step (1) are subjected to vibration treatment at room temperature for 20-40 minutes; after the vibration treatment is completed, the contact parts are washed with water;
[0031] (3) Acid activation: The contact components obtained in step (2) are cleaned with a 5% to 10% dilute sulfuric acid aqueous solution for 10 to 15 seconds to remove the acid wash solution remaining on the surface of the contact components; after the acid activation is completed, the contact components are washed with water;
[0032] (4) Anti-copper discoloration treatment: The contact parts obtained in step (3) are immersed in a 20%-25% aqueous solution of OY-8A anti-copper discoloration agent for 1-2 minutes to form a protective film on the surface thereof;
[0033] (5) The contact parts obtained in step (4) are washed with water in sequence to remove water stains.
[0034] In this embodiment, in the step (2), the proportions of the components in each liter of the vibration light liquid are as follows: 10-15 mL / L of grinding liquid, 10-15 mL / L of brightener, and the balance is water; the components and volume percentages of the grinding liquid are: 10%-20% of sodium dodecylbenzene sulfonate, 5%-15% of citric acid, 15%-25% of sodium carbonate, 10%-20% of sodium metasilicate, 20%-30% of fatty alcohol, and 10%-20% of castor oil; the components and volume percentages of the brightener are: 30%-40% of sodium dodecylbenzene sulfonate, 5%-15% of glycerol, 15%-25% of nonylphenol polyoxyethylene ether, 5%-15% of SLS needle-shaped multi-effect active agent, and 20%-30% of fatty alcohol polyoxyethylene ether.
[0035] In this embodiment, the water washing process in step (5) includes multi-stage countercurrent water washing and hot water washing in sequence, the time of each stage of countercurrent water washing is 5-10 seconds, the time of hot water washing is 10-30 seconds, and the temperature of the hot water is greater than or equal to 80° C. The multi-stage countercurrent water washing specifically adopts a three-stage countercurrent water washing process, but is not limited thereto.
[0036] In this embodiment, in step (5), the process for removing water stains includes hot air drying and drying in sequence, wherein the temperature of hot air drying is 60°C-70°C, the temperature of drying is 70°C-80°C, the drying time is 20-30s, and the drying time is 20-40min.
[0037] In this embodiment, the water washing process in step (1) to step (3) is respectively implemented by a multi-stage countercurrent water washing process. The multi-stage countercurrent water washing specifically adopts a three-stage countercurrent water washing process, but is not limited thereto. In this embodiment, when the product is contaminated with oil during the production process, the present invention can add a chemical degreasing step before step (1): immerse the contact parts in a 10%-15% HMC-02A degreasing aqueous solution for 10-15 minutes; after the degreasing is completed, the contact parts are subjected to a multi-stage countercurrent water washing. The multi-stage countercurrent water washing specifically adopts a three-stage countercurrent water washing process, but is not limited thereto.
[0038] In this embodiment, the 5%-10% dilute sulfuric acid aqueous solution refers to the dilute sulfuric acid aqueous solution whose components and volume percentages are: dilute sulfuric acid 5%-10%, and the balance is water. The 20%-25% OY-8A anti-copper discoloration agent aqueous solution refers to the OY-8A anti-copper discoloration agent aqueous solution whose components and volume percentages are: OY-8A anti-copper discoloration agent 20%-25%, and the balance is water. The 10%-15% HMC-02A degreasing aqueous solution refers to the HMC-02A degreasing aqueous solution whose components and volume percentages are: HMC-02A degreasing agent 10%-15%, and the balance is water.
[0039] The following provides a specific implementation step of a contact component cleaning process of the present invention:
[0040] S1. Chemical degreasing: immerse the contact parts in 13% HMC-02A degreasing aqueous solution for 13 minutes. After the degreasing is completed, the contact parts are washed with a three-stage countercurrent water washing process;
[0041] S2. Pickling to remove oxide film and copper color: prepare a pickling solution, the components and volume percentages of which are: 5% hydrogen peroxide with a mass fraction of 30%, 10% dilute sulfuric acid with a density of 1.84 g / ml, and the balance is water. Immerse the contact parts in the pickling solution for pickling for 13 seconds at room temperature; after the pickling is completed, the contact parts are washed with water using a three-stage countercurrent water washing process;
[0042] S3, vibration light removal of solder slag: the pre-prepared grinding liquid, brightener and water are mixed in a preset ratio to form a vibration light liquid, the ratio of each component in each liter of vibration light liquid is as follows: grinding liquid 13mL / L, brightener 13mL / L, the balance is water; the components and volume percentages of the grinding liquid are: 15% sodium dodecylbenzene sulfonate, 10% citric acid, 20% sodium carbonate, 15% sodium metasilicate, 25% fatty alcohol, 15% castor oil; the components and volume percentages of the brightener are: 35% sodium dodecylbenzene sulfonate, 10% glycerol, 20% nonylphenol polyoxyethylene ether, 10% SLS needle-shaped multi-effect active agent, 25% fatty alcohol polyoxyethylene ether; the contact parts obtained in step (2) are subjected to vibration light treatment for 30 minutes at room temperature using the vibration light liquid; after the vibration light treatment is completed, the contact parts are washed with water using a three-stage countercurrent washing process;
[0043] S4, acid activation: the contact components obtained in step (3) are cleaned for 13 seconds using an 8% dilute sulfuric acid aqueous solution to remove the acid wash solution remaining on the surface of the contact components; after the acid activation is completed, the contact components are washed using a three-stage countercurrent washing process.
[0044] S5. Anti-copper discoloration treatment: The contact parts obtained in step (4) are immersed in a 23% aqueous solution of OY-8A anti-copper discoloration agent for 1 minute to form a protective film on the surface thereof.
[0045] S6. Water washing: The contact parts obtained in step (5) are sequentially subjected to three-stage countercurrent water washing and hot water scalding, wherein the time for each stage of countercurrent water washing is 8 seconds, and the time for hot water scalding is 20 seconds, and the temperature of the hot water is 85°C.
[0046] S7, removing water stains: the contact parts obtained in step (6) are sequentially subjected to hot air drying and drying, drying at 65° C. for 250 seconds, and then drying at 75° C. for 30 minutes.
[0047] In the above, the values of the volume percentage of the 30% mass fraction hydrogen peroxide and the dilute sulfuric acid with a density of 1.84 g / ml are not limited to the above values, and can be taken within the respective preset numerical ranges, for example, the minimum or maximum value of the respective numerical ranges can be taken. Similarly, the ratio of the grinding liquid and the brightener in each liter of the vibration light liquid is not limited to the above values, and can be taken within the respective preset numerical ranges, for example, the minimum or maximum value of the respective numerical ranges can be taken. The values of the volume percentage of each component of the grinding liquid and the volume percentage of each component of the brightener are also not limited to the above values, and can be taken within the respective preset numerical ranges, for example, the minimum or maximum value of the respective numerical ranges can be taken. The values of the volume percentage of the HMC-02A degreasing agent in the HMC-02A degreasing aqueous solution, the volume percentage of the dilute sulfuric acid in the dilute sulfuric acid aqueous solution, and the volume percentage of the OY-8A anti-copper discoloration agent in the OY-8A anti-copper discoloration agent aqueous solution are not limited to the above values, and can also be taken within the respective preset numerical ranges, for example, the minimum or maximum value of the respective numerical ranges can be taken.
[0048] In a contact component cleaning process of the present invention, the operation sequence of the above-mentioned steps cannot be reversed, otherwise the cleaning requirements of silver contacts and copper or copper alloys cannot be met. This is because: the present invention first performs chemical degreasing to remove the oil stains on the surface of the contact component, so that the surface of the contact component is completely exposed, and then the oxide film and copper color on the surface of the contact component are removed by a pickling process, and then a specific vibration light process is used to remove the welding slag remaining around the contact component. After the contact component is cleaned, the highly oxidizing hydrogen peroxide pickling liquid remaining on the surface of the contact component is further removed by acid activation. After ensuring that the surface of the contact component is fully cleaned, it is treated with an environmentally friendly anti-copper discoloration agent to form a protective film on the surface of the contact component to prevent the surface of the contact component from being corroded by oxygen, carbon dioxide, etc. in the air after cleaning to produce a new oxide film layer. After the treated contact component is washed with water, it is finally dried to obtain a finished product after cleaning. The steps of the pickling process and the vibration process cannot be reversed. This is because the vibration process can not only remove the welding slag, but also make the contact parts brighter. If the vibration process is performed first and then pickled, the contact parts will become very dark after pickling. After each step is completed, water washing is performed to prevent the residual substances of the previous step from affecting the next step. The above step (6) also uses hot water for scalding, which can accelerate the removal of water stains.
[0049] The state of the contact parts before cleaning is as follows: Figure 1 As shown in the left picture, its surface is covered with an oxide film and welding slag, and it presents the pure copper color of the surface of the brass parts, and the overall color is very dull. Figure 1 The contact parts in the left figure are in the state after being cleaned by the cleaning process of the present invention. Figure 1 As shown in the right picture: it removes the oxide film layer, welding slag and the pure copper color on the surface of the brass parts, the overall surface is very bright, and the contact parts will not be re-oxidized and discolored after cleaning.
[0050] The contact component cleaning process of the present invention removes the oxide film layer, welding slag and pure copper color on the surface of the brass component through the operation of each process in the process flow, prevents the welded component from being oxidized and discolored again after cleaning, and ensures that the silver contact is not corroded. At the same time, it also takes into account the RoHS control requirements and silicone control requirements of the product (such as Figure 2 , which is a RoHs and silicone test report of the contact parts after being cleaned by the cleaning process of the present invention. The present invention can also realize batch cleaning operation of the contact parts, thereby facilitating batch production of the contact parts.
[0051] The contact component cleaning process of the present invention, the uninvolved parts are the same as the prior art or can be implemented by using the prior art.
[0052] The above embodiments are only used to further illustrate a contact component cleaning process of the present invention, but the present invention is not limited to the embodiments. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention fall within the protection scope of the technical solution of the present invention.
Claims
1. A contact component cleaning process, wherein the contact component comprises a substrate and a silver contact welded on the substrate, wherein the substrate comprises copper and / or a copper alloy; characterized in that: The cleaning process comprises the following steps: (1) Pickling to remove oxide film and copper color: Immerse the contact parts in a pickling solution for pickling at room temperature for 10-15 seconds; the components and volume percentages of the pickling solution are: 4%-6% hydrogen peroxide with a mass fraction of 30%, 8%-12% dilute sulfuric acid with a density of 1.84 g / ml, and the balance is water; (2) Vibration treatment to remove solder slag: a pre-prepared grinding liquid, brightener and water are mixed in a preset proportion to form a vibration treatment liquid, and the contact parts obtained in step (1) are subjected to vibration treatment at room temperature for 20-40 minutes; (3) Acid activation: The contact parts obtained in step (2) are cleaned with a 5% to 10% by volume aqueous solution of dilute sulfuric acid for 10 to 15 seconds to remove the acid wash solution remaining on the surface of the contact parts; (4) Anti-copper discoloration treatment: The contact parts obtained in step (3) are immersed in an aqueous solution of an OY-8A anti-copper discoloration agent with a volume percentage of 20% to 25% for 1 to 2 minutes to form a protective film on the surface thereof; In the step (2), the proportions of the components in each liter of the vibration light liquid are as follows: 10-15 mL / L of grinding liquid, 10-15 mL / L of brightener, and the balance is water; the components and volume percentages of the grinding liquid are: 10%-20% sodium dodecylbenzene sulfonate, 5%-15% citric acid, 15%-25% sodium carbonate, 10%-20% sodium metasilicate, 20%-30% fatty alcohol, and 10%-20% castor oil; the components and volume percentages of the brightener are: 30%-40% sodium dodecylbenzene sulfonate, 5%-15% glycerol, 15%-25% nonylphenol polyoxyethylene ether, 5%-15% SLS needle-shaped multi-effect active agent, and 20%-30% fatty alcohol polyoxyethylene ether.
2. The contact component cleaning process according to claim 1, characterized in that: The components and volume percentages of the grinding liquid are: 15% sodium dodecylbenzene sulfonate, 10% citric acid, 20% sodium carbonate, 15% sodium metasilicate, 25% fatty alcohol, and 15% castor oil; the components and volume percentages of the brightener are: 35% sodium dodecylbenzene sulfonate, 10% glycerol, 20% nonylphenol polyoxyethylene ether, 10% SLS needle-shaped multi-effect active agent, and 25% fatty alcohol polyoxyethylene ether.
3. The contact component cleaning process according to claim 1, characterized in that: The method further comprises step (5): washing the contact parts obtained in step (4) in sequence to remove water stains.
4. The contact component cleaning process according to claim 3, characterized in that: The water washing process in step (5) includes multiple stages of countercurrent water washing and hot water scalding in sequence. The time of each stage of countercurrent water washing is 5-10 seconds, and the time of hot water scalding is 10-30 seconds. The temperature of the hot water is greater than or equal to 80°C.
5. The contact component cleaning process according to claim 3, characterized in that: In the step (5), the process of removing water stains includes hot air drying and drying in sequence, wherein the temperature of hot air drying is 60°C-70°C, the temperature of drying is 70°C-80°C, the drying time is 20-30s, and the drying time is 20-40min.
6. The contact component cleaning process according to claim 1, characterized in that: In the steps (1) to (3), the contact parts are washed with water after each step is completed, and the washing is achieved by a multi-stage countercurrent washing process.
7. The contact component cleaning process according to claim 1, characterized in that: The step (1) also includes a chemical degreasing step: immersing the contact parts in a 10%-15% by volume HMC-02A degreasing aqueous solution for 10-15 minutes; and washing the contact parts with water after the degreasing is completed.
8. The contact component cleaning process according to claim 7, characterized in that: The water washing after the chemical degreasing step is completed is achieved by a multi-stage countercurrent water washing process.
9. The contact component cleaning process according to claim 1, characterized in that: The components and volume percentages of the pickling solution are: 5% hydrogen peroxide with a mass fraction of 30%, 10% dilute sulfuric acid with a density of 1.84 g / ml, and the balance is water.
Citation Information
Patent Citations
Pollution-free bright pickling process for copper and brass parts
CN101942665A
Environment-friendly copper and copper alloy pickling agent and copper and copper alloy silver-plating pretreatment method
CN104313610A
Welding process for hot pipe