High modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material and preparation method thereof

Through the combination technology of nitrogen-phosphorus and silicon-based flame retardants and surface modification of hemp fiber, the problems of flammability and poor interface compatibility of plant fiber composite materials have been solved, and high modulus, halogen-free flame retardant hemp fiber has been prepared. Fiber-reinforced polypropylene composite materials achieve excellent flame retardant and mechanical properties and are suitable for automotive interior and exterior parts.

CN115873344BActive Publication Date: 2024-10-11CHINA FAW CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211565332.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-10-11
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

Among existing automotive materials, plant fiber composites have high flammability and poor interface compatibility, which limits their application in the automotive field, especially in interior parts with combustion requirements, and halogen flame retardants can produce toxic and harmful substances. Gas affects the environment.

Method used

Using a combination of nitrogen-phosphorus and silicon-based flame retardants, combined with surface modification treatment and compatibilizer, a high-modulus, halogen-free flame-retardant hemp fiber-reinforced polypropylene composite material was prepared. By modifying the hemp fiber and polypropylene Acrylic resins are mechanically mixed and melt blended at low temperatures to form high-performance automotive materials.

Benefits of technology

The flame retardant grade reaches UL94V-0 level, the tensile and bending strength are significantly improved, the simply supported beam has no notch impact strength and no fracture, the material is green and environmentally friendly, and the cost is low. It is suitable for automotive interior and exterior parts with different processing and molding processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003985922820000021
    Figure BDA0003985922820000021
  • Figure BDA0003985922820000051
    Figure BDA0003985922820000051
  • Figure BDA0003985922820000071
    Figure BDA0003985922820000071
Patent Text Reader

Abstract

This specification discloses a high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material and its preparation method. The composite material includes the following raw materials in parts by weight: 29-78 parts of polypropylene resin; 8-36 parts of natural hemp fiber; 12-28 parts of flame retardant; 0.8-4.2 parts of compatibilizer; 0.3-1.2 parts of antioxidant. The present invention also discloses a preparation method of the composite material; the properties of the hemp fiber reinforced polypropylene composite material prepared by the present invention are as follows: the flame retardant grade can reach V-0 level; the tensile strength is greater than 43.0MPa; the tensile modulus is greater than 1405MPa; the flexural strength is greater than 34.5MPa; the flexural modulus is greater than 1420MPa; the simply supported beam unnotched impact strength has no fracture; the simply supported beam notched impact strength is greater than 21.5kJ / m 2 .
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One or more embodiments of the present specification relate to the field of automotive material technology, and more particularly to a high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material and a preparation method thereof. Background Art

[0002] In recent years, China's automobile industry has maintained a rapid and stable development momentum, with automobile production and sales ranking first in the world. The application of plastics in automobiles has a long history. At present, the use of modified plastics in automobiles has become an important indicator of the level of automobile design and manufacturing. The large-scale application of plastic accessories has promoted the weight reduction and energy saving of automobiles and improved the aesthetics and comfort of automobiles. In the automotive field, polypropylene (PP), as a general-purpose plastic, has become the largest, most frequently used and fastest-growing variety of automotive plastics due to its wide sources, low prices, corrosion resistance, excellent mechanical properties and other advantages.

[0003] At the same time, artificial fibers such as carbon fiber, glass fiber and aramid fiber have been widely used as reinforcing phases in polymer-based composites. However, artificial fibers have disadvantages such as poor degradability and high cost. Toxic and harmful gases are produced during the production process, and environmental problems will also arise in the later treatment (landfill or incineration). In contrast, plant fibers are derived from natural plants and have the advantages of low cost, low density, renewability, degradability, high specific strength and specific modulus.

[0004] At present, the automobile industry is one of the main sources of carbon emissions in my country, so automobile energy conservation and emission reduction are of great significance to my country's realization of the "dual carbon" goal. Automobile lightweighting is currently the most direct and effective way to achieve energy conservation and emission reduction. Composite materials are important lightweight materials and have become a hot spot in automobile lightweighting research. Plant fibers have low density, high specific strength and specific modulus. At the same time, compared with glass fibers, hemp fibers have higher specific modulus. Therefore, plant fibers are ideal substitutes for artificial fibers. Compared with carbon fiber and glass fiber reinforced resin-based composite materials, hemp fiber reinforced resin-based composite materials have the advantages of low price, biodegradability, low production energy consumption, sound insulation and noise reduction, so they have broad application prospects in the automotive field. That is, introducing high-strength and light-weight plant fibers into the polymer matrix can prepare high-performance green and environmentally friendly composite materials. Although plant fibers can make composite materials have good mechanical properties, the high flammability of plant fiber composite materials limits the application of composite materials in the automotive field, so it is crucial to improve the flame retardant properties of composite materials. At the same time, the oxygen index of polypropylene material itself is too low, and it has the disadvantage of being easy to burn, which limits its use in automotive interior parts with combustion requirements; therefore, it is necessary to add flame retardants to plant fibers to improve its easy burning defects. Although halogen flame retardants have high flame retardant efficiency, halogen flame retardants generate more smoke and toxic and harmful gases when burned, which have adverse effects on human health and seriously affect the ecological environment.

[0005] Moreover, since plant fibers contain a large number of hydroxyl groups, making them polar and hydrophilic, most thermoplastics are non-polar and hydrophobic, resulting in poor interfacial compatibility. This will cause more pores to exist between the composite matrix and the fibers, resulting in a decrease in the performance of the composite material and failing to meet expectations. Summary of the invention

[0006] In view of this, the purpose of one or more embodiments of the present specification is to provide a high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material. The properties of the hemp fiber reinforced polypropylene composite material of the present invention are as follows: the flame retardant grade can reach V-0 level; the tensile strength is greater than 43.0MPa; the tensile modulus is greater than 1405MPa; the flexural strength is greater than 34.5MPa; the flexural modulus is greater than 1420MPa; the simply supported beam unnotched impact strength has no fracture; the simply supported beam notched impact strength is greater than 21.5kJ / m 2 .

[0007] The second object of the present specification is to provide a high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material and a preparation method thereof.

[0008] Based on the above first item, this specification provides the following technical solutions:

[0009] A high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0010]

[0011] As an embodiment, the polypropylene resin is selected from the polypropylene resin F401 produced and sold by Beijing Yanshan Petrochemical Company.

[0012] As an embodiment, the natural hemp fiber is selected from one or more of ramie, flax, hemp, jute and sisal fibers.

[0013] As an embodiment, the flame retardant is a combination of a nitrogen-phosphorus flame retardant and a silicon-based flame retardant.

[0014] As an embodiment, the mass ratio of the nitrogen-phosphorus flame retardant to the silicon-based flame retardant is 0.5-5.5:1.

[0015] As a preferred embodiment, the nitrogen-phosphorus flame retardant is selected from one or more of melamine, ammonium polyphosphate, and melamine polyphosphate; the silicon-based flame retardant is selected from one or more of silicon dioxide and organosilicon flame retardants; preferably, the organosilicon flame retardant is one or more of polysiloxane, polyborosiloxane, and silicone oil.

[0016] As an embodiment, the compatibilizer is one or more of ethylene-butyl acrylate-glycidyl methacrylate (EGMA), triglycidyl isocyanurate (TGIC), triallyl isocyanurate (TAIC), and maleic anhydride grafted polypropylene (PP-g-MAH).

[0017] As an embodiment, the antioxidant consists of a primary antioxidant and a secondary antioxidant.

[0018] As a preferred embodiment, the main antioxidant is a hindered phenol antioxidant, and the hindered phenol antioxidant is selected from one or more of antioxidant 1035, antioxidant 1010, and antioxidant 1076; the auxiliary antioxidant is a sulfur-containing antioxidant, and the sulfur-containing antioxidant is selected from one or both of antioxidant DLTP and antioxidant DSTP.

[0019] As a preferred embodiment, the mass ratio of the primary antioxidant to the secondary antioxidant is 0.5-2.2:1.

[0020] Based on the above second item, this specification provides the following technical solutions:

[0021] A high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material and a preparation method thereof, comprising the following steps:

[0022] 1) cutting natural hemp fibers into 2-8 mm long short fibers, soaking the short hemp fibers in an alkaline solution with a mass fraction of 1.5-9 wt% for 15-90 min for modification, filtering, and then washing with a 0.03-0.3 wt% acetic acid deionized water solution until neutral, and drying the modified short hemp fibers; or

[0023] The natural hemp fibers are cut into short fibers with a length of 2-8 mm, and the short hemp fibers are soaked in a silane coupling agent ethanol solution with a mass fraction of 10-40 wt% for 90-240 min for modification, filtered, and the short hemp fibers treated with the coupling agent are dried;

[0024] 2) Drying the modified chopped hemp fibers, polypropylene resin, flame retardant, compatibilizer and antioxidant at 40-70° C. for 4-10 hours; Mechanically mixing the polypropylene resin, the surface-modified chopped hemp fibers, flame retardant, compatibilizer and antioxidant in a high-speed mixer for 10-30 minutes according to the formula amount, putting them into an internal mixer for melt blending for 5-25 minutes after mixing evenly, cooling and granulating after mixing to obtain a high modulus, halogen-free and flame-retardant hemp fiber reinforced polypropylene composite material.

[0025] As an embodiment, in step 1), the drying temperature is 30-70° C., and the drying time is 6-72 hours.

[0026] As an embodiment, the rotation speed of the high-speed mixer is 500-1000 rpm; the mixing temperature of the internal mixer is 170-220° C., and the rotor speed is 35-120 rpm.

[0027] Any range described in the present invention includes the end value and any numerical value between the end values ​​and any sub-range formed by the end value or any numerical value between the end values.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material prepared by the present invention has excellent mechanical properties, and the flame retardant performance reaches UL94V-0 level, and is excellent in flame retardant performance, green and environmentally friendly, and low in cost; it can realize batch production, is safe and reliable, and can be widely used in automotive interior and exterior parts with different processing and molding processes;

[0030] The properties of the hemp fiber reinforced polypropylene composite material of the present invention are as follows: the flame retardant grade can reach V-0 level; the tensile strength is greater than 43.0MPa; the tensile modulus is greater than 1405MPa; the flexural strength is greater than 34.5MPa; the flexural modulus is greater than 1420MPa; the simply supported beam unnotched impact strength has no fracture, and the simply supported beam notched impact strength is greater than 21.5kJ / m2 . DETAILED DESCRIPTION

[0031] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in conjunction with specific embodiments.

[0032] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in one or more embodiments of this specification should be understood by people with ordinary skills in the field to which this disclosure belongs. The words "first", "second" and similar words used in one or more embodiments of this specification do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprises" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.

[0033] In the present invention, the sources of raw materials are as follows:

[0034] Polypropylene resin F401 was purchased from Beijing Yanshan Petrochemical Company;

[0035] Natural hemp fiber and jute fiber were purchased from the Hemp Fiber Research Institute of the Chinese Academy of Agricultural Sciences;

[0036] Flame retardants (ammonium polyphosphate, polysiloxane, melamine polyphosphate, silicon dioxide) were purchased from Jinan Xinnuo Chemical Co., Ltd.

[0037] Compatibilizers (TGIC, TAIC) were purchased from Shandong Shengcang Chemical Co., Ltd.;

[0038] The main antioxidant 1010 and the secondary antioxidant DLTP were purchased from Lanzhou Chemical Industry Company;

[0039] Silane coupling agent KH560 was purchased from Henan Wanshan New Material Technology Co., Ltd.

[0040] Unless otherwise specified, all raw materials in the present invention can be purchased from the market, and the equipment used in the present invention can adopt conventional equipment in the relevant field or refer to the existing technology in the relevant field.

[0041] The performance testing method of the product hemp fiber reinforced polypropylene composite material of the present invention is as follows :

[0042] Flame retardant performance: tested according to UL-94 testing standards;

[0043] Tensile strength and tensile modulus: tested in accordance with ISO 527 standard;

[0044] Flexural strength and flexural modulus: tested in accordance with ISO 178 standard;

[0045] Simply supported beam unnotched impact strength, simply supported beam notched impact strength: tested in accordance with ISO 179 standard;

[0046] As one aspect of the present invention, a high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material of the present invention comprises the following raw materials in parts by weight:

[0047]

[0048] As an embodiment, the polypropylene resin is selected from the polypropylene resin F401 produced and sold by Beijing Yanshan Petrochemical Company.

[0049] As an embodiment, the natural hemp fiber is selected from one or more of ramie, flax, hemp, jute and sisal fibers. The natural hemp fiber is a kind of plant fiber, which has low density, high specific strength and specific modulus, and has many advantages such as wide source, low price, green environmental protection, and recyclability.

[0050] As an embodiment, the flame retardant is a combination of a halogen-free nitrogen-phosphorus flame retardant and a silicon-based flame retardant, which utilizes the synergistic flame retardant effect between the nitrogen-phosphorus flame retardant and the silicon-based flame retardant to improve the flame retardant properties while minimizing the impact on mechanical properties with the minimum addition amount.

[0051] As an embodiment, the mass ratio of the nitrogen-phosphorus flame retardant to the silicon-based flame retardant is 0.5-5.5:1.

[0052] As a preferred embodiment, the nitrogen-phosphorus flame retardant is selected from one or more of melamine, ammonium polyphosphate, and melamine polyphosphate; the silicon-based flame retardant is selected from one or more of silicon dioxide and organosilicon flame retardants; preferably, the organosilicon flame retardant is one or more of polysiloxane, polyborosiloxane, and silicone oil.

[0053] As an embodiment, the compatibilizer is one or more of ethylene-butyl acrylate-glycidyl methacrylate (EGMA), triglycidyl isocyanurate (TGIC), triallyl isocyanurate (TAIC), and maleic anhydride grafted polypropylene (PP-g-MAH). The addition of the compatibilizer can connect the molecular chain of polypropylene to the surface of the hemp fiber, enhance the interaction ability between the two phases, increase the adhesion between the phases, and improve the mechanical properties of the hemp fiber reinforced polypropylene composite material.

[0054] As an embodiment, the antioxidant is composed of a primary antioxidant and a secondary antioxidant. The addition of the antioxidant effectively inhibits or reduces the thermal oxidation and photooxidation reaction speed of the polypropylene material, significantly improves the heat resistance and light resistance of the material, delays the degradation and aging process of the polypropylene material, and prolongs the service life of the product; the present invention selects a combined antioxidant, utilizes the synergistic and complementary effect between the primary antioxidant and the secondary antioxidant, and achieves the best anti-thermal oxidation aging effect with the minimum addition amount and the lowest cost.

[0055] As a preferred embodiment, the main antioxidant is a hindered phenol antioxidant, and the hindered phenol antioxidant is selected from one or more of antioxidant 1035, antioxidant 1010, and antioxidant 1076; the auxiliary antioxidant is a sulfur-containing antioxidant, and the sulfur-containing antioxidant is selected from one or both of antioxidant DLTP and antioxidant DSTP.

[0056] As a preferred embodiment, the mass ratio of the primary antioxidant to the secondary antioxidant is 0.5-2.2:1.

[0057] As another aspect of the present invention, a high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material and a preparation method thereof include the following steps:

[0058] 1) Surface modification of natural hemp fiber: natural hemp fiber is cut into short hemp fiber with a length of 2-8 mm, the short hemp fiber is modified by soaking it in an alkaline solution with a mass fraction of 1.5-9 wt% for 15-90 min, filtered, and then washed with deionized water containing 0.03-0.3 wt% acetic acid solution until neutral, and the modified short hemp fiber is dried; or

[0059] The natural hemp fiber is cut into short fibers with a length of 2-8 mm, and the short hemp fiber is immersed in a silane coupling agent ethanol solution with a mass fraction of 10-40wt% for 90-240min for modification, and filtered, and the short hemp fiber treated with the coupling agent is dried; the polarity of the fiber surface is reduced by surface modification of the natural hemp fiber, thereby improving the interface bonding strength between the polypropylene resin and the fiber, thereby improving the interaction force between the hemp fiber and the polypropylene molecular chain, and improving the mechanical properties of the hemp fiber reinforced polypropylene composite material;

[0060] 2) Drying the modified chopped hemp fibers, polypropylene resin, flame retardant, compatibilizer and antioxidant at 40-70° C. for 4-10 hours; Mechanically mixing the polypropylene resin, the surface-modified chopped hemp fibers, flame retardant, compatibilizer and antioxidant in a high-speed mixer for 10-30 minutes according to the formula amount, putting them into an internal mixer for melt blending for 5-25 minutes after mixing evenly, cooling and granulating after mixing to obtain a high modulus, halogen-free and flame-retardant hemp fiber reinforced polypropylene composite material.

[0061] As an embodiment, in step 1), the drying temperature is 30-70° C., and the drying time is 6-72 hours.

[0062] As an embodiment, the rotation speed of the high-speed mixer is 500-1000 rpm; the mixing temperature of the internal mixer is 170-220° C., and the rotor speed is 35-120 rpm.

[0063] Example 1

[0064] A high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0065]

[0066] The method for preparing the above-mentioned high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material comprises the following steps:

[0067] 1) Surface modified natural hemp fiber:

[0068] The hemp fibers were cut into 5 mm short-cut hemp fibers, and the short-cut hemp fibers were modified by soaking them in a 6 wt% NaOH solution for 40 min, filtered, and then washed with a 0.15 wt% acetic acid deionized water solution until neutral, and finally, the washed short-cut hemp fibers were dried at 50° C. for 24 h;

[0069] 2) Dry the surface-modified chopped hemp fiber, polypropylene resin, compatibilizer and antioxidant at 60°C for 4h; Mechanically mix the polypropylene resin, surface-modified chopped hemp fiber, flame retardant, compatibilizer and antioxidant in a high-speed mixer according to the formula for 10min, the mixer speed is 800rpm, and after mixing evenly, put them into an internal mixer for melt blending for 15min, wherein the internal mixing temperature is 190°C and the rotor speed is 60rpm. After the mixing is completed, cool and granulate to obtain a high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material. The performance test results are shown in Table 1 below.

[0070] Example 2 :

[0071] A high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material comprises the following raw materials in parts by weight:

[0072]

[0073] The method for preparing the above-mentioned high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material comprises the following steps:

[0074] 1) Surface modified natural hemp fiber:

[0075] The hemp fibers were cut into 8 mm short-cut hemp fibers, and the short-cut hemp fibers were modified by soaking in a 1.5 wt% NaOH solution for 90 min, filtered, and then washed with a 0.06 wt% acetic acid deionized water solution until neutral, and finally, the washed short-cut hemp fibers were dried at 30° C. for 72 h;

[0076] 2) Dry the surface-modified chopped hemp fiber, polypropylene resin, compatibilizer and antioxidant at 40°C for 10 h; mechanically mix the polypropylene resin, surface-modified chopped hemp fiber, flame retardant, compatibilizer and antioxidant in a high-speed mixer according to the formula for 30 min, the mixer speed is 1000 rpm, and after mixing evenly, put them into an internal mixer for melt blending for 5 min, wherein the internal mixing temperature is 220°C and the rotor speed is 120 rpm. After mixing, cool and granulate to obtain a high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material. The performance test results are shown in Table 1 below.

[0077] Example 3

[0078] A high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material consisting of the following quality components:

[0079]

[0080] The method for preparing the above-mentioned high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material comprises the following steps:

[0081] 1) Surface modified natural hemp fiber:

[0082] Surface modified natural hemp fiber: cut the natural hemp fiber into 5mm short fibers, soak the short hemp fibers in 25wt% silane coupling agent KH560 ethanol solution for 150min and filter. Finally, dry the hemp fibers treated with the coupling agent at 60℃ for 12h.

[0083] 2) Dry the surface-modified chopped hemp fiber, polypropylene resin, compatibilizer and antioxidant at 70°C for 4h; Mechanically mix the polypropylene resin, surface-modified chopped hemp fiber, flame retardant, compatibilizer and antioxidant in a high-speed mixer according to the formula for 10min, the mixer speed is 500rpm, and after mixing evenly, put them into an internal mixer for melt blending for 25min, wherein the internal mixing temperature is 170°C and the rotor speed is 40rpm. After the mixing is completed, cool and granulate to obtain a high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material. The performance test results are shown in Table 1 below.

[0084] Example 4

[0085] Example 1 was repeated, except that the natural hemp fiber used was jute fiber from the Hemp Fiber Research Institute of the Chinese Academy of Agricultural Sciences instead of the natural hemp fiber. The performance test results are shown in Table 1 below.

[0086] Example 5

[0087] Example 1 was repeated, except that the flame retardant was a mixture of melamine polyphosphate and silicon dioxide in a mass ratio of 4:1. The performance test results are shown in Table 1 below.

[0088] Example 6

[0089] Example 1 was repeated, except that a mixture of triglycidyl isocyanurate (TGIC) and trienyl isocyanurate (TAIC) propyl ester was used as the compatibilizer, with a mass ratio of 1:1. The performance test results are shown in Table 1 below.

[0090] Performance testing

[0091] The high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite materials of Examples 1-6 were subjected to performance tests, and the test results are shown in Table 1 below:

[0092] Table 1: Performance test results of high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite materials of Examples 1-6

[0093]

[0094] From the data in Table 1, it can be seen that the flame retardant grade of the high modulus, halogen-free flame retardant hemp fiber reinforced polypropylene composite material of the present invention can reach V-0 grade; the tensile strength is greater than 43.0MPa; the tensile modulus is greater than 1405MPa; the flexural strength is greater than 34.5MPa; the flexural modulus is greater than 1420MPa; the simply supported beam unnotched impact strength has no fracture, and the simply supported beam notched impact strength is greater than 21.5kJ / m 2 .

[0095] Comparative Example 1

[0096] Example 1 was repeated, except that no natural hemp fiber was added. Other components, dosages and preparation methods were the same as those in Example 1. The product performance test results are shown in Table 2 below.

[0097] Comparative Example 2

[0098] Example 1 was repeated, except that no flame retardant was added; other components, amounts and preparation methods were the same as those in Example 1. The product performance test results are shown in Table 2 below.

[0099] Comparative Example 3

[0100] Example 1 was repeated, with the only difference being that only ammonium polyphosphate was used as the flame retardant, no silicon-based flame retardant was added, and the total amount of the flame retardant was still 22 parts; other components, amounts and preparation methods were the same as in Example 1, and the product performance test results are shown in Table 2 below.

[0101] Comparative Example 4

[0102] Example 1 was repeated, with the only difference being that only polysiloxane was used as the flame retardant, ammonium polyphosphate was not added, and the total amount of the flame retardant was still 22 parts; the other components, amounts and preparation methods were the same as those in Example 1, and the product performance test results are shown in Table 2 below.

[0103] Comparative Example 5

[0104] Example 1 was repeated, except that the compatibilizer TGIC was not added; the other components, amounts and preparation methods were the same as those in Example 1.

[0105] Comparative Example 6

[0106] Example 1 was repeated, except that the natural hemp fiber was not subjected to surface modification. The other components, amounts and preparation methods were the same as those in Example 1. The product performance test results are shown in Table 2 below.

[0107] Performance testing

[0108] The performance of the different polypropylene composite materials of Comparative Examples 1-6 was tested, and the test results are shown in the following 2 tables:

[0109] Table 2: Performance test results of different polypropylene composite materials of Comparative Examples 1-6

[0110]

[0111] By comparing the data of Example 1 and Comparative Example 1, it can be seen that the mechanical properties of the polypropylene material without adding natural hemp fiber modification are relatively poor, the tensile strength is only 16.2MPa, the tensile modulus is 754MPa; the flexural strength is only 9.6MPaMPa, the flexural modulus is 608MPa; the simply supported beam unnotched impact strength is only 13.2kJ / m 2, The notched impact strength of simply supported beam is 4.3 kJ / m 2 ; So it cannot meet the demand for some high-strength automotive plastic parts.

[0112] Comparing the data of Example 1 and Comparative Examples 2-4, it can be seen that the polypropylene material without adding flame retardant (Comparative Example 2) has no flame retardant properties, which limits its application in automobile interiors, automobile underbody guards, engine compartments and other exterior parts with flame retardant requirements. The flame retardant effect of adding only one flame retardant (Comparative Examples 3 and 4) is low, and the flame retardant grade is V-1, which limits its application in automobile interior parts with strict flame retardant requirements. The use of two flame retardants for synergistic flame retardancy (Example 1) can achieve a good flame retardant effect when the amount of flame retardant added is the lowest, which is energy-saving and efficient, and reduces production costs.

[0113] Further comparison of the test results of Example 1 and Comparative Example 5 shows that the addition of the compatibilizer improves the mechanical properties of the polypropylene material, and improves the tensile strength, flexural strength and impact strength. At the same time, the addition of the compatibilizer can improve the flame retardant level of the hemp fiber reinforced polypropylene composite material from V-1 to V-0, further improving the flame retardant effect of the hemp fiber reinforced polypropylene composite material.

[0114] Finally, by comparing the data of Example 1 and Comparative Example 6, it can be seen that without surface treatment of the natural hemp fiber, the compatibility of the hemp fiber and the polypropylene resin will be poor and the interaction force will be weak. At the same time, the difference in polarity leads to poor interface strength, which leads to a significant decrease in the mechanical properties of the final composite material. The tensile strength, flexural strength and impact strength are all greatly reduced, which limits the application of hemp fiber reinforced polypropylene composite materials in engineering fields such as automobiles.

[0115] In summary, the fiber raw materials, the selection of flame retardants, the selection of compatibilizers, the component contents and the preparation methods in the present invention have a significant impact on the products of the present invention. Exceeding any of the conditions will result in the product failing to meet the required performance of the present invention.

[0116] The above is a description of a specific embodiment of the present specification. Other embodiments are within the scope of the appended claims. In some cases, the actions or steps recorded in the claims can be performed in an order different from that in the embodiments and still achieve the desired results. In addition, the processes described in the specification do not necessarily require the specific order or continuous order shown to achieve the desired results. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.

[0117] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present disclosure (including the claims) is limited to these examples. In line with the present disclosure, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of different aspects of one or more embodiments of the present specification as described above, which are not provided in detail for the sake of simplicity.

[0118] In addition, to simplify the description and discussion, when specific details are set forth to describe the exemplary embodiments of the present disclosure, it is obvious to those skilled in the art that one or more embodiments of the present specification can be implemented without these specific details or with changes in these specific details. Therefore, these descriptions should be considered illustrative rather than restrictive.

[0119] While the disclosure has been described in conjunction with specific embodiments thereof, many alternatives, modifications and variations of these embodiments will be apparent to those skilled in the art in light of the foregoing description.

[0120] One or more embodiments of this specification are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of this specification should be included in the scope of protection of this disclosure.

Claims

1. High modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material, characterized in that: Made from the following raw materials in parts by weight: The flame retardant is a combination of a nitrogen-phosphorus flame retardant and a silicon-based flame retardant; The antioxidant consists of a primary antioxidant and a secondary antioxidant; The method for preparing the high modulus, halogen-free, flame-retardant hemp fiber reinforced polypropylene composite material comprises the following steps: 1) cutting natural hemp fibers into short fibers with a length of 2-8 mm, soaking the short hemp fibers in an alkaline solution with a mass fraction of 1.5-9 wt% for 15-90 min for modification, filtering, and then washing with a 0.03-0.3 wt% acetic acid deionized water solution until neutral, and drying the modified short hemp fibers; or The natural hemp fibers are cut into short fibers with a length of 2-8 mm, and the short hemp fibers are soaked in a silane coupling agent ethanol solution with a mass fraction of 10-40 wt% for 90-240 min for modification, filtered, and the short hemp fibers treated with the coupling agent are dried; 2) drying the modified chopped hemp fibers, polypropylene resin, flame retardant, compatibilizer and antioxidant at 40-70° C. for 4-10 hours; mechanically mixing the polypropylene resin, the surface-modified chopped hemp fibers, flame retardant, compatibilizer and antioxidant in a high-speed mixer for 10-30 minutes according to the formula amount, and after mixing evenly, putting them into an internal mixer for melt blending for 5-25 minutes. After the mixing is completed, cooling and granulating are performed to obtain a high modulus, halogen-free flame-retardant hemp fiber reinforced polypropylene composite material; In step 1), the drying temperature is 30-70°C and the drying time is 6-72h; The rotation speed of the high-speed mixer is 500-1000 rpm; the mixing temperature of the internal mixer is 170-220° C., and the rotor rotation speed is 35-120 rpm.

2. The hemp fiber reinforced polypropylene composite material according to claim 1, characterized in that: The natural hemp fiber is selected from one or more of ramie, flax, hemp, jute and sisal fibers.

3. The hemp fiber reinforced polypropylene composite material according to claim 1, characterized in that: The mass ratio of the nitrogen-phosphorus flame retardant to the silicon-based flame retardant is 0.5-5.5:

1.

4. The hemp fiber reinforced polypropylene composite material according to claim 1, characterized in that: The nitrogen-phosphorus flame retardant is selected from one or more of melamine, ammonium polyphosphate, and melamine polyphosphate; the silicon-based flame retardant is selected from one or more of silicon dioxide and organic silicon flame retardant.

5. The hemp fiber reinforced polypropylene composite material according to claim 1, characterized in that: The compatibilizer is one or more of ethylene-butyl acrylate-glycidyl methacrylate, triglycidyl isocyanurate, triallyl isocyanurate, and maleic anhydride grafted polypropylene.

6. The hemp fiber reinforced polypropylene composite material according to claim 1, characterized in that: The main antioxidant is a hindered phenol antioxidant, which is selected from one or more of antioxidant 1035, antioxidant 1010, and antioxidant 1076; the auxiliary antioxidant is a sulfur-containing antioxidant, which is selected from one or both of antioxidant DLTP and antioxidant DSTP.