A method for removing cyanide from cyanide tailings
By using main treatment agents such as sodium ferrochloride and sub-treatment agents such as cobalt 2-ethylhexanoate, the separation problem of cyanide in cyanide tailings was solved by using flotation technology, and the cyanide was improved removal efficiency.
Patent Information
- Application Number
- CN202211467151.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-11-22
AI Technical Summary
In the existing methods for decyanide tailings, the cyanide conversion method is difficult to completely separate the cyanide tailings in the cyanide tailings, especially the iron salt precipitation method, which has the problems of separation and deep separation, which limits its application.
The mixture of sodium ferrate, ferrous sulfate, EDDHA-Fe, EDTA-Fe and other main treatment agents and cobalt 2-ethylhexanoate, octamine and isopropanol as sub-treatment agents is used to form a ferrocyanomic complex. and foam, using flotation technology to separate and remove cyanide roots.
It improves the removal efficiency of cyanide, simplifies the process flow, effectively solves the separation problem between solid ferrocyanum complex and ore slurry, and achieves efficient cyanide removal.
Smart Images

Figure CN115888970B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hazardous waste treatment, and particularly relates to a method for removing cyanide from cyanide tailings. Background Art
[0002] Cyanide metallurgy technology has always been one of the main methods for gold extraction by gold mining companies at home and abroad, and it has a history of more than 100 years. Due to its advantages such as simple process, wide range of action, high recovery rate, low unit cost, and strong adaptability to ore, it has been widely used in practical production of gold extraction since the last century. Due to the use of cyanide, wastewater and tailings discharged from gold smelting often contain cyanide. According to statistics, the annual output of cyanide tailings in major gold producing areas such as China, South Africa and Australia alone is about 500 million tons. Cyanide tailings are currently mainly treated by stockpiling or landfilling. The cyanide remaining in the tailings can easily cause serious environmental pollution and ecological harm to soil, water bodies, etc.
[0003] At present, the decyanation treatment methods of cyanide tailings can be divided into cyanide destruction method, cyanide conversion method and cyanide recovery method according to the principle. Among them, cyanide destruction method is the mainstream of decyanation research of cyanide tailings, including alkaline chlorination method, INCO method, hydrogen peroxide oxidation method, ozone oxidation method, pressurized hydrolysis method, electrolytic oxidation method, ferrate oxidation method, peroxysulfuric acid oxidation method and high temperature decomposition method (incineration method). Cyanide conversion method includes zinc salt precipitation method, iron salt precipitation method and copper salt precipitation method. Cyanide recovery method includes acid recovery method and ion exchange method.
[0004] However, the cyanide conversion method usually requires the precipitation of free cyanide and metal cyanide complex ions, which is often used in the treatment of cyanide-containing wastewater, and the complete separation of it from the cyanide tailings becomes a problem; therefore, its application in the decyanation of cyanide tailings is limited. Among them, iron salts are more commonly used in the cyanide conversion method due to their wide reagent sources and low prices, but in addition to the above-mentioned separation problems, there is also the problem of deep separation. Summary of the invention
[0005] The present invention aims at the deficiencies of the above-mentioned prior art and provides a method for removing cyanide from cyanide tailings, thereby solving the problem of cyanide separation in cyanide tailings treatment and achieving high cyanide removal efficiency.
[0006] The specific technical solutions are as follows:
[0007] A method for removing cyanide from cyanide tailings comprises the following steps:
[0008] (1) Pretreatment: slurry the cyanide tailings with water and adjust the pH value to 4-6;
[0009] (2) Decyanation treatment: add the main treatment agent to the slurry obtained in step (1) and react for 0.1 to 2 hours; then add the secondary treatment agent and react for 0.1 to 1 hour;
[0010] Wherein, the main treatment agent is one or more of sodium ferrate, ferrous sulfate, ferric sulfate, EDDHA-Fe, EDTA-Fe, and ferric acetate;
[0011] Wherein, the secondary treatment agent is a mixture of cobalt 2-ethylhexanoate, octadecylamine and isopropanol;
[0012] (3) Flotation separation treatment.
[0013] Wherein, continuous stirring is performed during the reaction process in step (2).
[0014] Specifically, the process flow of the present invention can refer to Figure 1 .
[0015] The main treatment agent of the present invention forms an iron salt cyanide complex with the cyanide in the cyanide tailings, and the secondary treatment agent can be used as a flotation agent to form foam with the iron cyanide complex and float on the surface of the ore pulp, so that the upper foam can be easily removed by flotation, thereby obtaining tailings with cyanide effectively removed and solid cyanide.
[0016] Furthermore, in step (2), in the secondary treatment agent, the mass ratio of cobalt 2-ethylhexanoate: octadecylamine: isopropanol is 1:(1.5-10):(30-55).
[0017] Furthermore, the amount of the above-mentioned secondary treatment agent is 0.2-1 kg / t based on the slurry obtained in step (1).
[0018] Furthermore, in step (2), the amount of the main treatment agent used is 0.5-3 kg / t based on the slurry obtained in step (1).
[0019] Furthermore, in step (1), the slurry concentration is adjusted to 10wt%~50wt%.
[0020] Furthermore, in step (1), sulfuric acid is used to adjust the pH value.
[0021] Furthermore, in step (3), the slurry obtained in step (2) is sequentially fed into a flotation machine, a thickener and a filter press for solid-liquid separation. The flotation process adopts a coarse and fine two-sweep process.
[0022] The filtrate obtained after filtration can be returned to the pretreatment process as water for slurry preparation.
[0023] Furthermore, the cyanidation tailings are cyanidation tailings produced by the cyanidation gold extraction process. Preferably, the present invention is applicable to whole mud cyanidation tailings, sulfide ore cyanidation tailings or roasted cyanidation tailings.
[0024] The beneficial effects of the present invention are as follows:
[0025] The present invention uses a main treatment agent and a secondary treatment agent to react cyanide in cyanidation tailings with the main treatment agent to generate a ferrocyanide complex, and then forms foam floating on the surface of the ore pulp through the action of the secondary treatment agent, and then removes the foam through flotation, effectively solving the problem of separation of the solid ferrocyanide complex and the ore pulp, simplifying the process, and improving the cyanide removal efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The process flow chart of a specific embodiment of the present invention. DETAILED DESCRIPTION
[0027] The principles and features of the present invention are described below in conjunction with examples, which are only used to explain the present invention and are not used to limit the scope of the present invention. The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.
[0028] In each embodiment, the total cyanide content is determined by the method of "Spectrophotometric method for determination of cyanide and total cyanide in soil" HJ745-2015.
[0029] Example 1
[0030] The steps for treating the direct cyanidation tailings of gold concentrate with a total cyanide content of 1273 mg / kg are as follows:
[0031] (1) Pretreatment: slurry the cyanide tailings with water in a stirring tank to a concentration of 20 wt%, and add sulfuric acid to the stirring tank to adjust the pH value to 4;
[0032] (2) Decyanation treatment: under normal temperature conditions, add the main treatment agent to the slurry obtained in step (1) and stir for 60 minutes; then add the secondary treatment agent and stir for 30 minutes;
[0033] Wherein: the main treatment agent is sodium ferrate, and the amount used is 2 kg / t based on the ore pulp obtained in step (1); the secondary treatment agent is a mixture of cobalt 2-ethylhexanoate, octadecylamine and isopropanol, and the amount used is 0.5 kg / t based on the ore pulp obtained in step (1); the mass ratio of cobalt 2-ethylhexanoate: octadecylamine: isopropanol is 1:2:40;
[0034] (3) Flotation separation treatment: The ore pulp obtained in step (2) is sequentially fed into a flotation machine, a thickener and a filter press for solid-liquid separation; wherein, the flotation adopts a two-sweeping process of one coarse and one fine, and the upper layer product obtained by the fine separation is filtered to obtain solid cyanide, and the product is thickened after scavenging and filtered to obtain detoxified tailings.
[0035] The total cyanide content in the detoxified tailings obtained after filtration was 4.1 mg / kg.
[0036] The above process can refer to Figure 1 .
[0037] Example 2
[0038] The steps for treating the whole mud cyanide tailings with a total cyanide content of 453 mg / kg are as follows:
[0039] (1) Pretreatment: slurry the cyanide tailings with water in a stirring tank to a concentration of 30 wt%, and add sulfuric acid to the stirring tank to adjust the pH value to 5;
[0040] (2) Decyanation treatment: under normal temperature conditions, add the main treatment agent to the slurry obtained in step (1) and stir for 0.5 h; then add the secondary treatment agent and stir for 0.1 h;
[0041] Wherein: the main treatment agent is ferrous sulfate, and the amount used is 2 kg / t based on the ore pulp obtained in step (1); the secondary treatment agent is a mixture of cobalt 2-ethylhexanoate, octadecylamine and isopropanol, and the amount used is 0.5 kg / t based on the ore pulp obtained in step (1); the mass ratio of cobalt 2-ethylhexanoate: octadecylamine: isopropanol is 1:8:40;
[0042] (3) Flotation separation treatment: The ore pulp obtained in step (2) is sequentially fed into a flotation machine, a thickener and a filter press for solid-liquid separation; wherein, the flotation adopts a two-sweeping process of one coarse and one fine, and the upper layer product obtained by the fine separation is filtered to obtain solid cyanide, and the product is thickened after scavenging and filtered to obtain detoxified tailings.
[0043] The total cyanide content in the detoxified tailings obtained after filtration was 2.2 mg / kg.
[0044] The above process can refer to Figure 1 .
[0045] Example 3
[0046] The steps for treating roasting cyanide tailings with a total cyanide content of 608 mg / kg are as follows:
[0047] (1) Pretreatment: slurry the cyanide tailings with water in a stirring tank to a concentration of 40 wt%, and add sulfuric acid to the stirring tank to adjust the pH value to 6;
[0048] (2) Decyanation treatment: under normal temperature conditions, add the main treatment agent to the slurry obtained in step (1) and stir for 1.5 hours; then add the secondary treatment agent and stir for 0.2 hours;
[0049] Wherein: the main treatment agent is EDDHA-Fe, EDTA-Fe, and ferric acetate, with a weight ratio of 1:1:1, and the total amount is 2.5 kg / t based on the slurry obtained in step (1); the secondary treatment agent is a mixture of 2-ethylhexanoate cobalt, octadecylamine and isopropanol, and the amount is 0.7 kg / t based on the slurry obtained in step (1); the mass ratio of 2-ethylhexanoate cobalt: octadecylamine: isopropanol is 1:6:45;
[0050] (3) Flotation separation treatment: The ore pulp obtained in step (2) is sequentially fed into a flotation machine, a thickener and a filter press for solid-liquid separation; wherein, the flotation adopts a two-sweeping process of one coarse and one fine, and the upper layer product obtained by the fine separation is filtered to obtain solid cyanide, and the product is thickened after scavenging and filtered to obtain detoxified tailings.
[0051] The total cyanide content in the detoxified tailings obtained after filtration was 0.95 mg / kg.
[0052] The above process can refer to Figure 1 .
[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for removing cyanide from cyanide tailings, characterized in that: The steps include: (1) Pretreatment: slurry the cyanide tailings with water and adjust the pH value to 4-6; (2) Decyanation treatment: add the main treatment agent to the slurry obtained in step (1) and react for 0.1 to 2 hours; then add the secondary treatment agent and react for 0.1 to 1 hour; Wherein, the main treatment agent is one or more of sodium ferrate, ferrous sulfate, ferric sulfate, EDDHA-Fe, EDTA-Fe, and ferric acetate; Wherein, the secondary treatment agent is a mixture of cobalt 2-ethylhexanoate, octadecylamine and isopropanol, and the mass ratio of cobalt 2-ethylhexanoate:octadecylamine:isopropanol is 1:(1.5-10):(30-55); (3) Flotation separation treatment.
2. The method for removing cyanide from cyanide tailings according to claim 1, characterized in that: The dosage of the secondary treatment agent is 0.2-1 kg / t based on the ore pulp obtained in step (1).
3. The method for removing cyanide from cyanide tailings according to any one of claims 1 to 2, characterized in that: In step (2), the amount of the main treatment agent used is 0.5-3 kg / t based on the slurry obtained in step (1).
4. The method for removing cyanide from cyanide tailings according to any one of claims 1 to 2, characterized in that: In step (1), the slurry concentration is adjusted to 10wt%~50wt%.
5. The method for removing cyanide from cyanide tailings according to any one of claims 1 to 2, characterized in that: In step (1), sulfuric acid is used to adjust the pH value.
6. The method for removing cyanide from cyanide tailings according to any one of claims 1 to 2, characterized in that: In step (3), the slurry obtained in step (2) is sequentially fed into a flotation machine, a thickener and a filter press for solid-liquid separation.
7. The method for removing cyanide from cyanide tailings according to claim 6, characterized in that: In step (3), the flotation process adopts two sweeps, one coarse and one fine.
8. The method for removing cyanide from cyanide tailings according to any one of claims 1 to 2, characterized in that: The cyanide tailings are cyanide tailings produced by the cyanide gold extraction process.
9. The method for removing cyanide from cyanide tailings according to claim 8, characterized in that: The cyanidation tailings are full mud cyanidation tailings, gold concentrate direct cyanidation tailings or roasting cyanidation tailings.
Citation Information
Patent Citations
Method for flotation recovery of gold from gold-extracting tailings obtained from preliminary biooxidation-carbon-in-pulp process
CN104451173A
Cyanogen removal nitrogen reduction decolorizing agent suitable for coking phenol cyanogen wastewater and preparation and use methods
CN109052594A
Decyanation system for cyaniding tailings
CN217431924U
Method for treating cyanide-containing wastewater
JP2013123655A
method for CONDITIONING CYANIDE-CONTAINING PRODUCTS BEFORE FLOTATION EXTRACTION OF NON-FERROUS AND NOBLE METALS
RU2014141242A