Spherical silver powder for automobile glass silver paste and preparation method thereof
By reacting the silver nitrate solution with the reduction solution under stirring conditions, and adding a surface modifier for coating treatment, the existing problems of poor dispersion and wide particle size distribution were solved, and spherical silver powder was prepared, achieving high-quality silver powder The preparation of the product is suitable for the production of high-end automotive glass silver paste.
Patent Information
- Application Number
- CN202211426643.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-14
AI Technical Summary
The existing silver powder for automotive glass silver paste has problems such as poor dispersion, wide particle size distribution, and poor matching with organic solvents, which limits the production and application of high-end automotive glass silver paste.
The silver nitrate solution is added to the reducing solution under stirring conditions, and after reaction, the surface modifier is added for coating treatment. After filtration, washing, vacuum drying and airflow depolymerization, spherical silver powder is prepared to control particle size and surface characteristics. Improve dispersion and compatibility.
The prepared spherical silver powder has good dispersion, concentrated particle size distribution and excellent wetting properties. It is suitable as a high-quality raw material for automotive glass silver paste, improves the compatibility and stability of silver powder in organic carriers, and is suitable for industrial production.
Smart Images

Figure CN115889801B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive metal powder preparation, and in particular relates to spherical silver powder for automobile glass silver paste and a preparation method thereof. Background Art
[0002] The automotive glass defogger line is a silver conductive paste printed on the surface of the automotive glass and black glaze according to the designed circuit. After the glass is tempered, it firmly adheres to the surface of the glass and black glaze to form a defogger line silver film, which is mainly used for heating the automotive glass to quickly defrost and defog, thus affecting the comfort and safety of the car. The automotive glass defogger line silver film is exposed to harsh environments such as humidity, exposure, wind and sand, and even acid rain for a long time. It is easily affected by the environment and causes disconnection, aging, and even falling off, thus affecting the effectiveness of the defogger line. Silver powder, as a key functional component of automotive glass silver paste, is a key technical barrier to the preparation of automotive glass silver paste. At present, the silver powder used in automotive glass silver paste on the market has problems such as poor dispersibility, wide particle size distribution, and poor compatibility with organic solvents, which limits the production and application of high-end automotive glass silver paste. Therefore, how to prepare high-quality conductive silver powder is of vital importance to the development of automotive glass heating line silver paste. Summary of the invention
[0003] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a spherical silver powder for automotive glass silver paste and a preparation method thereof, and to develop a spherical silver powder with good sphericity, concentrated particle size distribution, good dispersibility and excellent wettability to meet the requirements for the preparation of automotive glass silver paste.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] The invention discloses a method for preparing spherical silver powder for automobile glass silver paste, comprising the following steps:
[0006] S1: under stirring, adding silver nitrate solution to reducing solution at a uniform speed, reacting to obtain silver powder suspension; adding surface modifier to the silver powder suspension for coating treatment, then filtering, washing, and solid-liquid separation to obtain silver powder wet material;
[0007] S2: Drying the silver powder wet material to obtain dried silver powder, and then performing airflow depolymerization on the dried silver powder to obtain spherical silver powder for automobile glass silver paste.
[0008] Furthermore, in S1, the mass ratio of the silver nitrate solution, the reducing solution, and the surface modifier is (150-250) g: (433-538) g: (0.09-0.15) g.
[0009] Furthermore, in S1, the concentration of the silver nitrate solution is 250-500 g / L; the reducing solution is prepared from a reducing agent, a dispersant and ultrapure water; the concentration of the reducing agent in the reducing solution is 60-80 g / L, and the concentration of the dispersant is 10-20 g / L; the temperatures of the silver nitrate solution and the reducing solution are both 28-32°C; the resistivity of the ultrapure water is greater than 18.25 MΩ.
[0010] Furthermore, in S1, the reducing agent is one or more of glucose, ascorbic acid, and hydrazine hydrate; and the dispersing agent is one or more of Tween-80, polyvinyl pyrrolidone, or polyvinyl alcohol.
[0011] Furthermore, in S1, the stirring speed is 400-500 r / min; and the adding speed of the silver nitrate solution into the reducing solution is 0.1-0.2 L / min.
[0012] Furthermore, in S1, the surface modifier is composed of a surfactant and a wetting agent; the surfactant is one of oleic acid, stearic acid or palmitic acid, and the wetting agent is octadecyl alcohol; the mass ratio of the surfactant to the wetting agent is 7:3.
[0013] Furthermore, in S1, the filtration is performed by vacuum filtration, and the vacuum degree of the vacuum filtration is -0.06 to -0.08 MPa; the washing is performed until the conductivity of the filtration solution is ≤10 ms; and the coating treatment time is 30 to 60 min.
[0014] Furthermore, in S2, the drying is performed by vacuum drying, the drying temperature is 60°C to 80°C, and the drying time is 18 to 24 hours; the airflow depolymerization is performed by a disc-type airflow mill, and the gas pressure of the airflow depolymerization is 0.7 to 1.0 MPa.
[0015] The invention also discloses spherical silver powder for automobile glass silver paste prepared by the preparation method.
[0016] Furthermore, the average particle size of the spherical silver powder for automobile glass silver paste is 1.7-2.0 μm, and the tap density is greater than 6.20 g / cm 3 , the specific surface area is 0.40~0.45m 2 / g, the burning loss at 538℃ is less than 0.6%, and the impurity content is less than 3ppm.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The invention discloses a method for preparing spherical silver powder for automobile glass silver paste. By controlling material concentration, feeding speed, reaction speed, type of surface modifier, depolymerization gas pressure, etc., the particle size, surface morphology and surface characteristics of the silver powder can be accurately controlled. The preparation process is simple to operate, the raw material source is wide, the process is stable, the equipment requirement is not high, and industrial production is easy to realize.
[0019] Furthermore, the surface of the silver powder is modified by a composite surface modifier, which effectively ensures the high dispersibility and good wettability of the silver powder and can effectively improve the compatibility, dispersibility and stability of the silver powder in the organic carrier.
[0020] The present invention also discloses spherical silver powder prepared by the above preparation method. The prepared spherical silver powder has good sphericity, concentrated particle size distribution and good dispersibility. According to relevant experimental results, the average particle size of the spherical silver powder for automobile glass silver paste is 1.7-2.0um, and the tap density is greater than 6.20g / cm 3 , the specific surface area is 0.40~0.45m 2 / g, the burnout at 538℃ is less than 0.6%, and the impurity content (chlorine, copper, iron, lead, nickel) is less than 3ppm, which is suitable as a high-quality raw material for preparing automotive glass silver paste. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The SEM image and particle size distribution diagram of the spherical silver powder for automotive glass silver paste prepared in Example 1;
[0022] Among them: a-SEM image; b-particle size distribution diagram;
[0023] Figure 2 The SEM image and particle size distribution diagram of the spherical silver powder for automotive glass silver paste prepared in Example 2;
[0024] Among them: c-SEM image; d-particle size distribution diagram;
[0025] Figure 3 The SEM image and particle size distribution diagram of the spherical silver powder for automotive glass silver paste prepared in Example 3;
[0026] Among them: e-SEM image; f-particle size distribution diagram. DETAILED DESCRIPTION
[0027] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0028] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0029] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0030] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0031] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0032] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0033] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0034] Example 1
[0035] A method for preparing spherical silver powder for automobile glass silver paste comprises the following steps:
[0036] S1: Dissolve 1 kg of silver nitrate in 2 L of ultrapure water, and keep the temperature at 30° C. after fully dissolved to obtain a silver nitrate solution; dissolve 600 g of ascorbic acid and 160 g of polyvinyl alcohol in 10 L of ultrapure water in sequence, and keep the temperature at 30° C. after fully dissolved to obtain a reduction solution;
[0037] At a stirring speed of 400 r / min, 3 kg of silver nitrate solution was uniformly added to 10.76 kg of reducing solution, and the silver powder suspension was obtained by reacting while adding the materials; wherein the adding speed of the silver nitrate solution was controlled to be 0.1 L / min;
[0038] After the reaction is completed, 3.0 g of a composite surface modifier is added to the silver powder suspension for coating treatment for 30 min under high shear force, wherein the surface modifier is a mixture of stearic acid and octadecanol, and the addition amounts of stearic acid and octadecanol are 2.10 g and 0.90 g, respectively. The suspension is then filtered and washed 4 times until the conductivity of the filtered solution is ≤10 ms, wherein the filtration is performed by vacuum filtration with a vacuum degree of -0.06 MPa; solid-liquid separation is performed to obtain a silver powder wet material;
[0039] S2: The wet silver powder material is vacuum dried at a drying temperature of 60° C. for 24 hours until the moisture content is ≤0.1% to obtain dried silver powder. The dried silver powder is subjected to airflow depolymerization, and the depolymerization gas pressure is controlled at 0.8 MPa. The silver powder material is fully depolymerized to obtain spherical silver powder for automotive glass silver paste. The obtained spherical silver powder for automotive glass silver paste has an average particle size D50 of 1.73 μm and a tap density of 6.34 g / cm 3 , with a specific surface area of 0.45m 2 / g, loss on burning is 0.59%, and the contents of impurities (chlorine, copper, iron, lead, nickel) are all less than 3ppm.
[0040] Example 2
[0041] A method for preparing spherical silver powder for automobile glass silver paste comprises the following steps:
[0042] S1: Dissolve 1 kg of silver nitrate in 4 L of ultrapure water, keep the temperature constant at 32° C. after fully dissolved, to obtain a silver nitrate solution; dissolve 580 g of glucose and 80 g of polyvinyl pyrrolidone in 8 L of ultrapure water in sequence, keep the temperature constant at 32° C. after fully dissolved, to obtain a reduction solution;
[0043] At a stirring speed of 500 r / min, 5 kg of silver nitrate solution was evenly added to 8.66 kg of reducing solution, and the silver powder suspension was obtained by reacting while adding the materials; wherein the adding speed of the silver nitrate solution was controlled to be 0.2 L / min;
[0044] After the reaction is completed, 1.8 g of a composite surface modifier is added to the silver powder suspension for coating treatment under high shear force for 60 min, wherein the surface modifier is a mixture of oleic acid and octadecanol, and the addition amounts of oleic acid and octadecanol are 1.27 g and 0.54 g, respectively. The suspension is then filtered and washed 4 times until the conductivity of the filtered solution is ≤10 ms, wherein the filtration is performed by vacuum filtration with a vacuum degree of -0.08 MPa; solid-liquid separation is performed to obtain a silver powder wet material;
[0045] S2: The wet silver powder material is vacuum dried at a drying temperature of 80°C for a drying time of 18 hours until the moisture content is ≤0.1% to obtain dried silver powder, and the dried silver powder is subjected to airflow depolymerization, and the depolymerization gas pressure is controlled at 0.7 MPa. The silver powder material is fully depolymerized to obtain spherical silver powder for automotive glass silver paste; the obtained spherical silver powder for automotive glass silver paste has an average particle size D50 of 1.73 um and a tap density of 6.39 g / cm 3 , with a specific surface area of 0.40m 2 / g, loss on burning is 0.45%, and the contents of impurities (chlorine, copper, iron, lead, nickel) are all less than 3ppm.
[0046] Example 3
[0047] A method for preparing spherical silver powder for automobile glass silver paste comprises the following steps:
[0048] S1: Dissolve 1 kg of silver nitrate in 3 L of ultrapure water, keep the temperature constant at 30° C. after fully dissolved, to obtain a silver nitrate solution; dissolve 585 g of ascorbic acid, 60 g of polyvinyl alcohol, and 60 g of polyvinyl pyrrolidone in 9 L of ultrapure water in sequence, keep the temperature constant at 30° C. after fully dissolved, to obtain a reduction solution;
[0049] At a stirring speed of 450 r / min, 4 kg of silver nitrate solution was uniformly added to 9.705 kg of reducing solution, and a solid-liquid mixture was obtained by reacting while adding the materials; wherein the adding speed of the silver nitrate solution was controlled to be 0.15 L / min;
[0050] After the reaction is completed, 2.1 g of a composite surface modifier is added to the silver powder suspension for coating treatment under high shear force for 45 min, wherein the surface modifier is a mixture of oleic acid and octadecanol, and the addition amounts of oleic acid and octadecanol are 1.47 g and 0.63 g, respectively. The suspension is then filtered and washed 4 times until the conductivity of the filtered solution is ≤10 ms, wherein the filtration is performed by vacuum filtration with a vacuum degree of -0.06 MPa; solid-liquid separation is performed to obtain a silver powder wet material;
[0051] S2: The wet silver powder material is vacuum dried at a drying temperature of 70°C for 20 hours until the moisture content is ≤0.1% to obtain dried silver powder, and the dried silver powder is subjected to airflow depolymerization, and the depolymerization gas pressure is controlled at 0.75 MPa. The silver powder material is fully depolymerized to obtain spherical silver powder for automotive glass silver paste; the obtained spherical silver powder for automotive glass silver paste has an average particle size D50 of 1.81 um and a tap density of 6.35 g / cm 3 , with a specific surface area of 0.43m 2 / g, loss on burning is 0.52%, and the contents of impurities (chlorine, copper, iron, lead, nickel) are all less than 3ppm.
[0052] Example 4
[0053] A method for preparing spherical silver powder for automobile glass silver paste comprises the following steps:
[0054] S1: Dissolve 1 kg of silver nitrate in 3 L of ultrapure water, keep the temperature constant at 28° C. after fully dissolved, to obtain a silver nitrate solution; dissolve 640 g of ascorbic acid and 160 g of Tween-80 in 8 L of ultrapure water in sequence, keep the temperature constant at 28° C. after fully dissolved, to obtain a reduction solution;
[0055] At a stirring speed of 450 r / min, 4 kg of silver nitrate solution was uniformly added to 8.8 kg of reducing solution, and a solid-liquid mixture was obtained by reacting while adding the materials; wherein the adding speed of the silver nitrate solution was controlled to be 0.2 L / min;
[0056] After the reaction is completed, 2.1 g of a composite surface modifier is added to the silver powder suspension and coated for 50 min under high shear force, wherein the surface modifier is a mixture of palmitic acid and octadecanol, and the addition amounts of oleic acid and octadecanol are 1.47 g and 0.63 g, respectively. The suspension is then filtered and washed for 5 times until the conductivity of the filtered solution is ≤10 ms, wherein the filtration is performed by vacuum filtration with a vacuum degree of -0.06 MPa; solid-liquid separation is performed to obtain a silver powder wet material;
[0057] S2: The wet silver powder material is vacuum dried at a drying temperature of 75° C. for 22 h until the moisture content is ≤0.1% to obtain dried silver powder. The dried silver powder is subjected to airflow depolymerization with the depolymerization gas pressure controlled at 1.0 MPa. The silver powder material is fully depolymerized to obtain spherical silver powder for automotive glass silver paste.
[0058] Table 1 shows the performance indicators of the spherical silver powder obtained by the present invention. It can be seen from Table 1 that the tap density of the prepared silver powder is greater than 6.20 g / cm 3 The average particle size is 1.7-2.0um, the maximum particle size is less than 4um, and the specific surface area is 0.40-0.45m 2 / g, the burning loss at 538℃ is less than 0.6%, and the impurity content (chlorine, copper, iron, lead, nickel) is less than 3ppm. It has the characteristics of high tap density, uniform particle size, moderate specific surface area and low impurity content.
[0059] Table 1 Performance indexes of spherical silver powder obtained by the present invention
[0060]
[0061]
[0062] Figure 1 to Figure 3 Shown are the SEM images and particle size distribution diagrams of the spherical silver powder for automotive glass silver paste prepared in Examples 1 to 3. From the diagrams, it can be seen that the prepared silver powder has good sphericity, a smooth surface of the silver powder particles, good dispersibility, and a concentrated particle size distribution, and is suitable for debugging high-quality automotive glass silver paste.
[0063] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing spherical silver powder for automobile glass silver paste, characterized in that: The following steps are involved: S1: under stirring, adding silver nitrate solution to reducing solution at a uniform speed, reacting to obtain silver powder suspension; adding surface modifier to the silver powder suspension for coating treatment, then filtering, washing, and solid-liquid separation to obtain silver powder wet material; S2: drying the silver powder wet material to obtain dried silver powder, and then performing airflow depolymerization on the dried silver powder to obtain spherical silver powder for automobile glass silver paste; In S1, the concentration of the silver nitrate solution is 250-500 g / L; the reducing solution is prepared from a reducing agent, a dispersant and ultrapure water; the concentration of the reducing agent in the reducing solution is 60-80 g / L, and the concentration of the dispersant is 10-20 g / L; the temperatures of the silver nitrate solution and the reducing solution are both 28-32° C.; the resistivity of the ultrapure water is greater than 18.25 MΩ; In S1, the stirring speed is 400-500 r / min; the adding speed of the silver nitrate solution to the reducing solution is 0.1-0.2 L / min; In S1, the surface modifier is composed of a surfactant and a wetting agent; the surfactant is one of oleic acid, stearic acid or palmitic acid, and the wetting agent is octadecyl alcohol; the mass ratio of the surfactant to the wetting agent is 7:3; In S2, the drying is performed by vacuum drying, the drying temperature is 60°C to 80°C, and the drying time is 18 to 24 hours; the airflow depolymerization is performed by a disc-type airflow mill, and the gas pressure of the airflow depolymerization is 0.7 to 1.0 MPa; In S1, the mass ratio of the silver nitrate solution, the reducing solution, and the surface modifier is 150-250 g: 433-538 g: 0.09-0.15 g; In S1, the reducing agent is one or more of glucose, ascorbic acid, and hydrazine hydrate; and the dispersing agent is one or more of Tween-80, polyvinyl pyrrolidone, or polyvinyl alcohol.
2. The method for preparing spherical silver powder for automobile glass silver paste according to claim 1, characterized in that: In S1, the filtration is performed by vacuum filtration, and the vacuum degree of the vacuum filtration is -0.06~-0.08MPa; the washing is performed until the conductivity of the filtration solution is ≤10ms; and the coating treatment time is 30~60min.
3. A spherical silver powder for automobile glass silver paste, characterized in that: The spherical silver powder is prepared by the method for preparing spherical silver powder for automobile glass silver paste according to claim 1 or 2.
4. The spherical silver powder for automobile glass silver paste according to claim 3, characterized in that: The average particle size of the spherical silver powder for automobile glass silver paste is 1.7-2.0 μm, and the tap density is greater than 6.20 g / cm 3 , the specific surface area is 0.40~0.45m 2 / g, the burning loss at 538℃ is less than 0.6%, and the impurity content is less than 3ppm.
Citation Information
Patent Citations
Preparation method of high tap density monodisperse silver powder
CN103100722A
Preparation method of single-dispersion and high-tap-density spherical silver powder
CN105583407A
Preparation method for spherical silver powder high in tap density
CN105817646A
Preparation method for high-dispersity spherical silver powder
CN107971502A
Preparation method of high-compaction spherical ultrafine silver powder
CN109365830A