Au-based composite brazing material for aluminum nitride ceramics and preparation and brazing method thereof

The use of Au-based composite solder solves the problems of poor welding quality and strict process requirements in aluminum nitride ceramic welding, achieves stable welding and multi-dimensional adaptability in high temperature environments, and improves welding strength and oxidation resistance. .

CN115890058BActive Publication Date: 2024-10-22ST CERA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211457458.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-21
Publication Date
2024-10-22
Estimated Expiration
2042-11-21

AI Technical Summary

Technical Problem

There is a lack of special solder in the existing aluminum nitride ceramic welding. Commonly used solders have short service life and poor welding quality in high temperature environments. The welding process requirements are strict, which limits the application of solder in different sizes and types of weldments.

Method used

Au-based composite solder is used, and the formula includes Au as the main metal and oxide synergists such as TiO2, B2O3, V2O5, MoO3, Bi2O3, etc., and the solder sheet or solder slurry is prepared through specific preparation methods and processes. Air reaction brazing of aluminum nitride ceramics.

Benefits of technology

It improves the welding strength, shear resistance and oxidation resistance, and reduces the thermal expansion coefficient. It is suitable for oxygen-rich environments and environments with drastic changes in cold and heat. It has good process adaptability, a wide brazing temperature range, and flexible welding layer thickness to meet the needs of a wide range of applications. size and micro weldment needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115890058B_ABST
    Figure CN115890058B_ABST
Patent Text Reader

Abstract

The invention belongs to the field of ceramic technology, and specifically relates to an Au-based composite solder for aluminum nitride ceramics, a method for preparing the Au-based composite solder, and an air reaction brazing method for aluminum nitride ceramics. The formula of the composite solder includes a main metal and an oxide co-component. The main metal is Au; the oxide co-component is TiO2 and another oxide selected from B2O3, V2O5, MoO3 and Bi2O3. In the composite solder, the molar percentage of TiO2 is 0.5% to 1% according to the amount of substance; the total molar percentage of the oxide co-component is 4% to 20%. The product form of the composite solder includes a solder sheet and a solder slurry; the solder slurry can be coated on the welded part by screen printing, and the composite solder has an excellent welding effect on aluminum nitride ceramics, and can produce a good welding effect under conditions of different thicknesses of the solder layer. The invention can solve the problems of poor welding quality of existing solders for air reaction brazing of aluminum nitride ceramics, and strict requirements of solders on welding processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramics, and in particular relates to an Au-based composite solder for aluminum nitride ceramics, a preparation method of the Au-based composite solder, and an air reaction brazing method for aluminum nitride ceramics. Background Art

[0002] Aluminum Nitride Ceramic is a ceramic with aluminum nitride (AIN) as the main crystal phase. Aluminum nitride ceramic substrate has the advantages of high thermal conductivity, low expansion coefficient, high strength, high temperature resistance, chemical corrosion resistance, high resistivity, and low dielectric loss. It is an ideal large-scale integrated circuit heat dissipation substrate and packaging material; it is widely used in the electronic industry such as high-frequency piezoelectric components and optical communication devices.

[0003] In some application scenarios, the ceramic substrate needs to be welded. Ceramic welding technologies include brazing, diffusion welding, instantaneous liquid phase connection, etc. Among them, the brazing method is convenient and flexible, with high production efficiency, and is applicable to both oxide and non-oxide ceramics. Ceramic brazing technologies include metallization brazing, active metal brazing, air reaction brazing, and auxiliary brazing such as ultrasonic, laser, and microwave. Compared with air reaction brazing, other brazing technologies are more complicated and have higher equipment requirements. For example, active metal brazing needs to be carried out under high vacuum or gas protection atmosphere, metallization brazing usually requires two major steps of high-temperature metallization and vacuum brazing (or atmosphere protection brazing), while air reaction brazing only needs to be heated in an ordinary muffle furnace. In particular, since the air reaction brazing filler metal is composed of a composite of antioxidant precious metals and oxides, the prepared brazed joints are used in oxygen-rich and high-temperature environments, and the joint strength is also high.

[0004] Based on the above advantages, air reaction brazing is the most commonly used welding process in the ceramic welding process. Different brazing materials are usually required for different types and uses of ceramics. For example, for zirconia, alumina and perovskite series ceramics, the air reaction brazing used is mainly Ag-CuO, Ag-V2O5, Ag-Nb2O5, Ag-Pd-CuO, Pt-Nb2O5 and other systems. For example, in the technical solution disclosed in U.S. Patent US1033434 "Weil KS, et al. Oxidation ceramic to metal braze seals for applications in high temperature electrochemical devices and method of making," Ag-CuO, Ag-V2O5 and Pt-Nb2O5 brazing materials are used to perform air reaction brazing on alumina ceramics. In the technical solution disclosed in the document "Luo Y, et al. Reactive air brazing of Al2O3 ceramic with Ag-CuO-Pt composite fillers: microstructure and joint properties. Journal of the European Ceramic Society, 2021, 41: 1407–1414", Ag-CuO-Pt brazing filler is used to perform air reaction brazing on alumina ceramic. In the technical solution disclosed in the Chinese invention patent authorization announcement number CN110253100B "A method for air reaction brazing connection of YSZ ceramic and stainless steel", Nb powder is oxidized to form Nb2O5 powder, which is then mixed with Ag powder and pressed into a sheet to prepare Ag-Nb2O5 brazing filler sheet, which is then set between YSZ ceramic and stainless steel for air reaction brazing.

[0005] However, there is no special solder for aluminum nitride ceramics in the prior art. The main metals used in these conventional brazing materials are Ag, Ag-Pd or Pt. Therefore, when used for aluminum nitride brazing, either the thermal expansion coefficient is too high (such as Ag), which will affect the high temperature resistance and service life of the weldment. Or the metal oxidation resistance in the composite brazing material is insufficient during air reaction brazing (such as Ag-Pd), which will affect the service life of the weldment in harsh environments. Or the brazing temperature is too high, such as when Pt is used, the brazing temperature is ≥1800℃; aluminum nitride ceramics cannot withstand such high temperatures, and are therefore not suitable for carbon nitride ceramic brazing.

[0006] In addition, most solders have high requirements for welding process, and the requirements for brazing temperature and solder layer thickness are also relatively strict. If the brazing temperature and solder layer thickness of the weldment during the brazing process do not meet expectations, the welding quality of the weldment will be significantly affected, which limits the application of solders in weldments of different sizes and types. Summary of the invention

[0007] In order to solve the problems in the prior art that the welding quality of existing solders during air reaction brazing of aluminum nitride is poor and the solders have strict requirements on the welding process, the present invention provides an Au-based composite solder for aluminum nitride ceramics, a method for preparing the Au-based composite solder, and an air reaction brazing method for aluminum nitride ceramics.

[0008] The present invention is implemented by the following technical solutions:

[0009] An Au-based composite solder for aluminum nitride ceramics, the formula of the composite solder comprising a main metal and an oxide co-component. The main metal is Au; the oxide co-component is TiO2 and another oxide selected from B2O3, V2O5, MoO3 and Bi2O3. In the composite solder, the molar percentage of TiO2 is 0.5% to 1% based on the amount of substance; the total molar percentage of the oxide co-component is 4% to 20%.

[0010] As a further improvement of the present invention, the product form of the composite solder includes solder sheets and solder slurry; when used as solder sheets, the product only contains uniformly dispersed composite solder components. When used as solder slurry, the product contains composite solder in powder form and an organic carrier in liquid form, and the composite solder is uniformly dispersed in the organic carrier.

[0011] The present invention also includes a method for preparing a composite solder, which is used to prepare the Au-based composite solder of the aluminum nitride ceramic as described above; the preparation method comprises the following steps:

[0012] S1: Au in the formula and ceramic powders of various selected oxides are mixed according to a preset material ratio, and anhydrous ethanol is added as a dispersant to mix and disperse the above mixture evenly.

[0013] S2: Drying the mixed wet material in the previous step at a temperature of 100-150° C. to remove the anhydrous ethanol therein.

[0014] S3: Grind the mixed dry materials in the previous step again into a uniform dry powder.

[0015] S4: Processing the dry powder into the required solder sheet or solder slurry.

[0016] As a further improvement of the present invention, among the raw materials used in step 1, Au powder is selected to have a particle size of micrometer level or below; and the purity of the ceramic powders of various oxides is ≥99.9%.

[0017] As a further improvement of the present invention, in step S4, the processing process of the solder sheet is as follows:

[0018] The dried powder from the previous step is pressed into a sheet with uniform thickness using a hydraulic press at a pressure of 150-200 MPa to obtain the desired solder sheet.

[0019] The thickness of the pressed solder sheet is 80 to 200 μm.

[0020] As a further improvement of the present invention, in step S4, the processing process of the solder slurry is as follows:

[0021] The solder paste prepared in the above step is mixed with the pre-prepared liquid organic carrier in a preset ratio and fully dispersed to obtain a paste which is the desired solder paste.

[0022] The present invention also includes an air reaction brazing method for aluminum nitride ceramics, which is used to braze welded parts made of the same aluminum nitride ceramic material; the air reaction brazing method includes the following steps:

[0023] S01: Grind and polish the welding surface of the aluminum nitride ceramic weldment to be welded; then clean and dry it.

[0024] S02: placing the aforementioned Au-based composite brazing material of aluminum nitride ceramic on the welding surface of the workpiece to be welded, and completing the assembly of the weldment;

[0025] S03: The assembled parts to be welded are placed in a muffle furnace and air reaction brazing is performed at a brazing temperature of 1080-1200°C.

[0026] As a further improvement of the present invention, in step S01, the welded parts are firstly ground and polished on a precision grinding and polishing machine; then boiled in a weak alkaline solution for 30 minutes, rinsed with water, and finally dried in an oven.

[0027] As a further improvement of the present invention, in step S02, when a solder sheet is used as the required brazing material, the solder sheet is first cut into a shape and size that matches the welding surface; then the solder sheet is placed between the welding surfaces of the two welds to complete the weld assembly.

[0028] When solder paste is used as the required brazing material, the solder paste is applied to the welding surfaces of the two parts to be welded by screen printing and dried, and the coating thickness of the solder paste on the two parts to be welded is made the same; then the welding surfaces of the two parts to be welded are aligned and fitted; and the weldment assembly is completed.

[0029] As a further improvement of the present invention, in step S03, the air reaction brazing process of the workpiece to be welded in the muffle furnace is as follows:

[0030] First, place the workpiece to be welded in a muffle furnace and apply a micro-pressure of 10 to 20 kPa to the workpiece. Then, raise the furnace temperature to a brazing temperature of 1080 to 1200 °C at a heating rate of no more than 10 °C / min, and heat treat for 5 to 60 minutes. Next, lower the furnace temperature to 500 °C at a cooling rate of 5 °C / min. Finally, cool the welded workpiece to room temperature with the furnace and take it out; brazing is completed.

[0031] The technical solution provided by the present invention has the following beneficial effects:

[0032] The composite solder of the present invention is a special solder applicable to aluminum nitride ceramic welding; Au is preferably used as the main metal in the composite solder, and TiO2 and another oxide selected from B2O3, V2O5, MoO3 and Bi2O3 are selected as oxide co-matching agents; TiO2 in the co-matching oxide is beneficial to improving the interface effect between the welding layer and the aluminum nitride ceramic, thereby enhancing the welding strength and shear resistance of the weldment. The addition of B2O3, V2O5, MoO3 and Bi2O3 can simultaneously reduce the thermal expansion coefficient of the composite solder, regulate the brazing temperature, and improve the oxidation resistance of the welding layer. This makes the brazed parts of the solder applicable to harsh working environments with oxygen-rich and drastic changes in temperature.

[0033] The formula of the composite brazing material provided by the present invention is optimized so that the thermal expansion coefficient of the material of the welding layer generated by the brazing material after brazing is very close to the thermal expansion coefficient of the aluminum nitride ceramics on both sides, ensuring that the material can maintain a balanced internal stress distribution under different temperature states, thereby improving the thermal shock resistance and service life of the material.

[0034] The composite solder provided by the present invention also has the advantages of good process adaptability and low brazing difficulty. For example, when the composite solder coating is made by screen printing, since it can be printed on two connecting surfaces, the total thickness can be 20 to 80 μm; thus, a large-sized composite solder layer with a thickness of tens of microns can be produced; and when the composite solder sheet is made by the sheet pressing process, it is conducive to achieving a thicker and denser composite solder layer; the thickness of the solder layer can reach, for example, 80 to 200 μm.

[0035] During the brazing process, the brazing material of this embodiment does not have strict requirements on the welding process parameters, and welding can be achieved using the simplest muffle furnace and air reaction brazing process; within a wide temperature range of 1080°C-1200°C, better welding effects can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a process flow chart of a method for preparing a composite solder provided in Example 1 of the present invention.

[0037] Figure 2 This is a process flow chart of an air reaction brazing method for aluminum nitride ceramics provided in Example 2 of the present invention. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0039] Example 1

[0040] An Au-based composite solder for aluminum nitride ceramics, the formula of the composite solder comprising a main metal and an oxide co-component. The main metal is Au; the oxide co-component is TiO2 and another oxide selected from B2O3, V2O5, MoO3 and Bi2O3. In the composite solder, the molar percentage of TiO2 is 0.5% to 1% based on the amount of substance; the total molar percentage of the oxide co-component is 4% to 20%.

[0041] In the brazing material formula of this embodiment, the main metal is Au; the thermal expansion performance of Au is relatively matched with that of aluminum nitride ceramics, and it has a wide brazing temperature range, and the Au material itself has good anti-oxidation properties. Therefore, the use of Au as the main metal in this embodiment is the basis for improving the welding effect of aluminum nitride ceramic weldments, and ensures that the welding layer has better anti-oxidation properties.

[0042] The solder formula of this embodiment preferably selects two types of oxide materials with different properties as oxide co-matching agents for the main metal. One of them is TiO2, which is mainly used in the formula of this embodiment to improve the interface effect between the solder layer and the aluminum nitride ceramic matrix in the two weldments after welding, and significantly improves the welding strength. The other is a specific oxide selected according to the physical and chemical properties such as the thermal expansion coefficient of aluminum nitride ceramics. These oxides include B2O3, V2O5, MoO3 and Bi2O3. The addition of the above oxide co-matching agents can further adjust the overall thermal expansion coefficient of the solder, so that the thermal expansion coefficient of the solder layer and the weldment are closer.

[0043] In particular, after adding the oxide co-formulator of the above components according to the formula provided in this embodiment, the welding temperature range of the weldment can also be significantly widened. It has been experimentally verified that within a wide temperature range of 1080-1200°C, a better welding effect can be achieved for aluminum nitride ceramics, and at the same time, a heat treatment of 5 minutes can achieve a better welding quality; the welding process only requires a simple muffle furnace to complete, without the need for vacuum or special atmosphere protection, and the requirements for the welding process are relatively low, and the restrictions on process parameters are relatively loose.

[0044] Another outstanding advantage of the composite solder with a specific formula provided in this embodiment is its good adaptability to various brazing processes and different welding scenarios. Whether a thinner (20-80 μm) solder layer thickness or a thicker (80-200 μm) solder layer thickness is used, the composite solder can maintain a high welding quality, and even if the solder layer thickness reaches more than 150 μm, a relatively dense solder layer can still be formed; this allows the solder to be used for brazing large-sized weldments and ultra-thin micro weldments at the same time.

[0045] Based on the above advantages, the product forms of the composite solder of a specific formula provided in this embodiment include solder sheets and solder slurry. When used as a solder sheet, the product only contains uniformly dispersed composite solder components. This type of product is mainly used for the welding of larger welds, and the thickness of the solder sheet is 80 to 200 μm. When used as a solder slurry, the product contains a composite solder in a powdered state and an organic carrier in a liquid state, and the composite solder is uniformly dispersed in the organic carrier. This solder product can be used for the welding of thinner micro welds, especially when the solder is applied by screen printing, the thickness of the solder layer can be as low as about 20 μm.

[0046] In this embodiment, the Au-based composite brazing material of the aluminum nitride ceramic can be prepared by Figure 1 The specific process steps are as follows:

[0047] S1: Au in the formula and ceramic powders of various selected oxides are mixed according to a preset material ratio, and anhydrous ethanol is added as a dispersant, and the above mixture is mixed and dispersed evenly in a mixing tank.

[0048] Among them, Au powder can be selected from commercial products with a particle size of micrometer level or below; and the purity of ceramic powders using various oxides should reach more than 99.9%.

[0049] S2: Drying the mixed wet material in the previous step at a temperature of 100-150° C. to remove the anhydrous ethanol therein.

[0050] S3: Grind the mixed dry materials in the previous step again into a uniform dry powder.

[0051] S4: Processing the dry powder into the required solder sheet or solder slurry;

[0052] Among them, the processing process of the solder sheet is as follows:

[0053] The dried powder in the above step is pressed into a sheet with uniform thickness using a hydraulic press at a pressure of 150-200 MPa to obtain the desired solder sheet. The thickness of the pressed solder sheet is 80-200 μm.

[0054] The processing of solder paste is as follows:

[0055] The solder paste prepared in the above step is mixed with the pre-prepared liquid organic carrier in a preset ratio and fully dispersed to obtain a paste which is the desired solder paste.

[0056] It should be noted that in the solder paste, the organic carrier generally includes a variety of functional additives such as dispersants, antioxidants, anticoagulants, thickeners, defoamers, etc. The composite paste provided in this embodiment has no special restrictions on the components and types of the organic carrier when preparing the solder paste, and various conventional formulas can be used.

[0057] In addition, in order to be applied to different scenarios, technicians can also reasonably adjust the ratio of the composite solder and the organic carrier according to the requirements of the solder concentration and viscosity of the solder slurry. For example, in this embodiment, the components of the organic carrier used include: 86wt.% pine alcohol, 8wt.% ethyl cellulose, 2wt.% hydrogenated castor oil, 2wt.% Span 85 and 2wt.% 1,4-butyrolactone by mass percentage. Among them, the mixing mass ratio of the powder and the liquid organic carrier in the slurry preparation process is 1:1.

[0058] Example 2

[0059] This embodiment provides an air reaction brazing method for aluminum nitride ceramics, which uses the composite brazing material in Example 1 as a welding material. Depending on the type of aluminum nitride ceramic weldment, different types of composite brazing products can be used and welded using different welding processes. Among them, for conventional aluminum nitride ceramic weldments with thicker materials and larger volumes. The brazing sheet in Example 1 is preferably used as the welding material, while for thinner and smaller micro aluminum nitride ceramic weldments, the brazing slurry in Example 1 is preferably selected as the welding material.

[0060] Specifically, the process flow of the air reaction brazing method of aluminum nitride ceramics provided in this embodiment is as follows: Figure 2 As shown, the process steps include:

[0061] S01: Grind and polish the welding surface of the aluminum nitride ceramic weldment to be welded; then clean and dry it.

[0062] Specifically, the welded parts are firstly ground and polished on a precision grinding and polishing machine; then boiled in a weak alkaline solution for 30 minutes, rinsed with water, and finally dried in an oven.

[0063] S02: placing the aforementioned Au-based composite brazing material of aluminum nitride ceramic on the welding surface of the workpiece to be welded, and completing the assembly of the weldment. Specifically,

[0064] (1) When a brazing sheet is used as the required brazing material, the brazing sheet is first cut into a shape and size that matches the welding surface; then the brazing sheet is placed between the welding surfaces of the two welds to complete the weldment assembly.

[0065] (2) When solder paste is used as the required brazing material, the solder paste is applied to the welding surfaces of the two parts to be welded by screen printing and dried, and the coating thickness of the solder paste on the two parts to be welded is made the same; then the welding surfaces of the two parts to be welded are aligned and fitted; and the weldment assembly is completed.

[0066] S03: The assembled parts to be welded are sent into a muffle furnace and air reaction brazing is performed at a brazing temperature of 1080-1200° C. In this embodiment, the air reaction brazing process of the parts to be welded in the muffle furnace is described in detail as follows:

[0067] First, place the workpiece to be welded in a muffle furnace and apply a micro-pressure of 10 to 20 kPa to the workpiece. Then, raise the furnace temperature to a brazing temperature of 1080 to 1200 °C at a heating rate of no more than 10 °C / min, and heat treat for 5 to 60 minutes. Next, lower the furnace temperature to 500 °C at a cooling rate of 5 °C / min. Finally, cool the welded workpiece to room temperature with the furnace and take it out; brazing is completed.

[0068] Performance Testing

[0069] In order to verify the various properties of the composite brazing material provided by this embodiment, and the welding effect of the composite brazing material on different types of aluminum nitride ceramics, different test cases are set up below, samples of composite brazing materials with different proportions and types are trial-produced, and different types of weldments are welded using different processes; finally, the welding quality of the weldments after welding is tested.

[0070] 1. Trial production of brazing connectors

[0071] Test Example 1

[0072] (1) Grind and polish the connection surface of the aluminum nitride ceramic to be welded on a precision grinding and polishing machine, boil it in a weak alkaline solution for 30 minutes, rinse it with water, and place it in an oven at 100°C for 60 minutes to dry it.

[0073] (2) Commercially available Au, B2O3 and TiO2 powders with molar percentages of 89.5%, 10% and 0.5%, respectively, were placed in a rolling ball mill, anhydrous ethanol was used as a dispersant, and the mixture was mixed at a speed of 60 r / min for 48 hours. The mixture was taken out and dried, and then ground into a uniform powder; the mixed powder with a mass ratio of 1:1 and the above-mentioned organic carrier were prepared into a composite solder slurry.

[0074] (3) The composite solder paste is screen-printed twice on the connection surface of the aluminum nitride ceramic to a thickness of 10 μm, and then placed in an oven at 150° C. for 30 minutes for drying.

[0075] (3) Two pieces of aluminum nitride ceramics with composite brazing material coating on the connection surface are placed face to face and placed in a muffle furnace. The additional pressure is 10 kPa, and the temperature is increased to 1080 °C brazing temperature at a heating rate of ≤10 °C / min. The holding time is 60 min, and then the temperature is cooled to 500 °C at a cooling rate of 5 °C / min, and then cooled in the furnace.

[0076] Test Example 2

[0077] (1) Grind and polish the connection surface of the aluminum nitride ceramic to be welded on a precision grinding and polishing machine, boil it in a weak alkaline solution for 30 minutes, rinse it with water, and place it in an oven at 150°C for 30 minutes to dry it.

[0078] (2) Commercially available Au, V2O5 and TiO2 powders with molar percentages of 79%, 20% and 1%, respectively, were placed in a rolling ball mill, anhydrous ethanol was used as a dispersant, and the mixture was mixed at a speed of 60 r / min for 48 hours. The mixture was taken out and dried, and then ground into a uniform powder; the mixed powder with a mass ratio of 1:1 and the above-mentioned organic carrier were prepared into a composite solder slurry.

[0079] (3) The composite solder paste is screen-printed 6 times on the connection surface of the aluminum nitride ceramic to a thickness of 25 μm, and then placed in an oven at 150° C. for 30 minutes for drying.

[0080] (4) Two pieces of aluminum nitride ceramics with composite brazing material coating on the connection surface are placed face to face and placed in a muffle furnace. The additional pressure is 15 kPa, and the temperature is increased to 1100 °C brazing temperature at a heating rate of ≤10 °C / min. The temperature is kept at this temperature for 30 min, and then the temperature is reduced to 500 °C at a cooling rate of 5 °C / min, and then cooled in the furnace.

[0081] Test Example 3

[0082] (1) Grind and polish the connection surface of the aluminum nitride ceramic to be welded on a precision grinding and polishing machine, boil it in a weak alkaline solution for 30 minutes, rinse it with water, and place it in an oven at 100°C for 60 minutes to dry it.

[0083] (2) Commercially available Au, MoO3 and TiO2 powders with molar percentages of 91.5%, 8% and 0.5%, respectively, were placed in a rolling ball mill, anhydrous ethanol was used as a dispersant, and the mixture was mixed at a speed of 60 r / min for 48 hours. The mixture was taken out and dried, and then ground into a uniform powder; the mixed powder with a mass ratio of 1:1 and the above-mentioned organic carrier were prepared into a composite solder slurry.

[0084] (3) The composite solder paste is screen-printed 10 times on the connection surface of the aluminum nitride ceramic to a thickness of 40 μm, and then placed in an oven at 150° C. for 30 minutes for drying.

[0085] (4) Two pieces of aluminum nitride ceramics with composite brazing material coating on the connection surface are placed face to face and placed in a muffle furnace. The additional pressure is 20 kPa, and the temperature is increased to 1150 °C brazing temperature at a heating rate of ≤10 °C / min. The temperature is kept at this temperature for 20 min, and then the temperature is cooled to 500 °C at a cooling rate of 5 °C / min, and then cooled in the furnace.

[0086] Test Example 4

[0087] (1) Grind and polish the connection surface of the aluminum nitride ceramic to be welded on a precision grinding and polishing machine, boil it in a weak alkaline solution for 30 minutes, rinse it with water, and place it in an oven at 100°C for 60 minutes to dry it.

[0088] (2) Commercially available Au, MoO3 and TiO2 powders with molar percentages of 95.5%, 4% and 0.5%, respectively, were placed in a rolling ball mill, with anhydrous ethanol as a dispersant, mixed at a speed of 60 r / min for 48 hours, taken out and dried, and then ground into a uniform powder; using a hydraulic press at a pressure of 200 MPa, the above powders were pressed into a composite solder sheet with a thickness of 200 μm.

[0089] (3) The pressed composite brazing sheet is cut into pieces according to the size of the aluminum nitride ceramic connection surface.

[0090] (4) The cut composite brazing material sheet is placed between the two aluminum nitride ceramics treated above and placed in a muffle furnace. The additional pressure is 15 kPa. The temperature is increased to a brazing temperature of 1150 °C at a heating rate of ≤10 °C / min for 30 min. The temperature is then decreased to 500 °C at a cooling rate of 5 °C / min and then cooled in the furnace.

[0091] Test Example 5

[0092] (1) Grind and polish the connection surface of the aluminum nitride ceramic to be welded on a precision grinding and polishing machine, boil it in a weak alkaline solution for 30 minutes, rinse it with water, and place it in an oven at 100°C for 60 minutes to dry it.

[0093] (2) Commercially available Au, Bi2O3 and TiO2 powders with molar percentages of 89.5%, 10% and 0.5%, respectively, were placed in a rolling ball mill, with anhydrous ethanol as a dispersant, mixed at a speed of 60 r / min for 48 hours, taken out and dried, and then ground into a uniform powder; the above powders were pressed into a composite solder sheet with a thickness of 80 μm using a hydraulic press at a pressure of 150 MPa.

[0094] (3) The pressed composite brazing sheet is cut into pieces according to the size of the aluminum nitride ceramic connection surface.

[0095] (4) The cut composite brazing sheet is placed between the two aluminum nitride ceramics treated above and placed in a muffle furnace. The additional pressure is 20 kPa. The temperature is increased to 1200 °C brazing temperature at a heating rate of 10 °C / min for 5 min. The temperature is then decreased to 500 °C at a cooling rate of 5 °C / min and then cooled in the furnace.

[0096] 2. Brazed joint shear strength test results and analysis

[0097] In this experiment, two identical 10 mm×5 mm×5 mm square aluminum nitride specimens were used in test examples 1-5, and the square surfaces were used as welding surfaces, and brazing was performed in an overlapping manner.

[0098] Then, in the following test experiment, the room temperature shear strength of the brazed joint is mainly tested. The test method for the room temperature shear strength test of the welded joint can be performed by referring to the method of the reference (Wang ZQ, et al, Interfacial microstructure and mechanical properties of SiC joints achieved by reactive air brazing using Ag-V2O5 filler, Journal of the European Ceramic Society, 2019, 39: 2617–2625).

[0099] The test results of the brazed connection specimens of the five test cases in this experiment in different test cases are shown in the following table:

[0100] Table 1: Statistics of welding performance test results of brazed joints in different test cases

[0101]

[0102] Analysis of the test data in the above table shows that when the brazing slurry produced under different formulas and process parameters in this experiment is used for aluminum nitride ceramic welding, the shear strength of the welded joint at room temperature can reach more than 50 MPa, which reflects that the composite brazing material provided by the present invention has an excellent welding effect in the aluminum nitride ceramic welding process.

[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An Au-based composite brazing material of aluminum nitride ceramic, characterized in that: The formula of the composite solder includes a main metal and an oxide co-component; the main metal is Au; the oxide co-component is TiO2 and another oxide selected from B2O3, MoO3 and Bi2O3; in the composite solder, the molar percentage of TiO2 is 0.5% to 1% based on the amount of substance; the total molar percentage of the oxide co-component is 4% to 20%; The Au-based composite brazing material of aluminum nitride ceramic is used for brazing connection between AlN ceramics; the brazing conditions are: placing the workpiece to be welded in a muffle furnace, applying a micro-pressure of 10-20 kPa to the workpiece to be welded; then, raising the furnace temperature to a brazing temperature of 1080°C-1200°C at a heating rate not exceeding 10°C / min, and heat-treating the workpiece for 5-60 minutes; then, lowering the furnace temperature to 500°C at a cooling rate of 5°C / min; finally, cooling the welded workpiece to room temperature with the furnace and taking it out; the brazing is completed.

2. The Au-based composite brazing material of aluminum nitride ceramic according to claim 1, characterized in that: The product forms of the composite solder include solder sheets and solder slurries; when used as solder sheets, the product only contains uniformly dispersed composite solder components; when used as solder slurries, the product contains composite solder in powder form and an organic carrier in liquid form, and the composite solder is uniformly dispersed in the organic carrier.

3. A method for preparing a composite solder, characterized in that: It is used to prepare the Au-based composite brazing material of aluminum nitride ceramic as claimed in claim 1 or 2; the preparation method comprises the following steps: S1: Mixing Au in the formula and ceramic powders of various selected oxides according to a preset material ratio, adding anhydrous ethanol as a dispersant, and mixing and dispersing the mixture uniformly; S2: Drying the mixed wet material in the previous step at a temperature of 100-150° C. to remove the anhydrous ethanol therein; S3: Grind the mixed dry materials in the previous step again into a uniform dry powder; S4: Processing the dry powder into the required solder sheet or solder slurry.

4. The method for preparing the composite solder according to claim 3, characterized in that: Among the raw materials used in step 1, Au powder is selected to have a particle size of micrometer level or below; the purity of ceramic powders of various oxides is ≥99.9%.

5. The method for preparing the composite solder according to claim 3, characterized in that: In step S4, the processing process of the solder sheet is as follows: Use a hydraulic press to press the dried powder in the previous step into a sheet with uniform thickness at a pressure of 150-200 MPa to obtain the desired solder sheet; The thickness of the solder sheet is 80-200 μm.

6. The method for preparing the composite solder according to claim 3, characterized in that: In step S4, the processing process of the solder slurry is as follows: The solder paste prepared in the above step is mixed with the pre-prepared liquid organic carrier in a preset ratio and fully dispersed to obtain a paste which is the desired solder paste.

7. A method for air reaction brazing of aluminum nitride ceramics, characterized in that: It is used for brazing weldments made of the same aluminum nitride ceramic material; the air reaction brazing method comprises the following steps: S01: Grind and polish the welding surface of the aluminum nitride ceramic weldment to be welded, and then clean and dry it; S02: placing the Au-based composite brazing material of aluminum nitride ceramic as described in claim 1 or 2 on the welding surface of the workpiece to be welded, and completing the assembly of the weldment; S03: The air reaction brazing process of the parts to be welded in the muffle furnace is as follows: First, place the workpiece to be welded in a muffle furnace and apply a micro-pressure of 10~20kPa to the weldment; then, increase the furnace temperature to the brazing temperature of 1080℃~1200℃ at a heating rate not exceeding 10°C / min, and keep the heat treatment for 5~60min; then, reduce the furnace temperature to 500°C at a cooling rate of 5°C / min; finally, cool the weld product to room temperature with the furnace and take it out; the brazing is completed.

8. The air reaction brazing method of aluminum nitride ceramics according to claim 7, characterized in that: In step S01, the welded parts are firstly ground and polished on a precision grinding and polishing machine; then boiled in a weak alkaline solution for 30 minutes, rinsed with water, and finally dried in an oven.

9. The air reaction brazing method of aluminum nitride ceramics according to claim 7, characterized in that: In step S02, when a solder sheet is used as the required brazing material, the solder sheet is first cut into a shape and size that matches the welding surface; then the solder sheet is placed between the welding surfaces of the two weldments to complete the weldment assembly; When solder paste is used as the required brazing material, the solder paste is applied to the welding surfaces of the two parts to be welded respectively by screen printing and dried; then the welding surfaces of the two parts to be welded are aligned and fitted; and the weldment assembly is completed.